A kind of polysulfone resin and polymerization method thereof
By introducing cyano aromatic group bisphenol monomers into the polysulfone resin to form polymers with high aromatic ring content, the problem of insufficient wear resistance and mechanical strength of PSU materials is solved, and its heat resistance and mechanical properties are significantly improved. Broaden its application areas.
Patent Information
- Application Number
- CN202311326722.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-10-13
AI Technical Summary
The wear resistance and mechanical strength of PSU materials are low, which limits its application in the fields of wear-resistant components such as automobile high-temperature components, aerospace engines, and aviation bearings.
By introducing a cyano-containing aromatic group bisphenol monomer into the traditional polysulfone resin repeating unit, a polymer containing a large amount of aromatic ring on the main chain of the macromolecule and a cyano group on the side chain is formed.
It improves the heat resistance, wear resistance and mechanical strength of polymers, and broadens its application in automotive heat-resistant parts, aerospace wear-resistant parts, aviation bearings and other fields.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to a polysulfone resin and a polymerization method thereof. Background Art
[0002] Bisphenol A polysulfone (PSU) is a thermoplastic special engineering plastic containing sulfone functional groups in the molecular chain. PSU material has excellent chemical resistance, excellent flame retardancy, balanced mechanical properties, non-toxicity, etc., making it a major candidate material in the fields of medical devices, food contact, water treatment, electronic appliances, etc.
[0003] However, compared with other special engineering plastics, PSU materials have lower wear resistance and mechanical strength, which limits their application in wear-resistant parts such as automotive high-temperature parts, aerospace engines, and aviation bearings. Therefore, developing a high-performance PSU resin is of practical significance for improving the wear resistance of such materials, enhancing their temperature resistance and mechanical properties, and accelerating their promotion and application. Summary of the invention
[0004] The object of the present invention is to provide a polysulfone resin having good heat resistance, wear resistance and mechanical properties.
[0005] The present invention is achieved through the following technical solutions:
[0006] A polysulfone resin derived from monomers comprising, by mole percent:
[0007] Bisphenol A 20-40 mol%
[0008] 10-30 mol% of bisphenol monomer containing cyano aromatic group;
[0009] 4,4'-Dichlorodiphenyl sulfone 45-55 mol%;
[0010] Wherein, the bisphenol monomer containing cyano aromatic group is:
[0011] Among them, R1 and R2 are Any one of a heterocyclic aromatic group or a polycyclic aromatic group; n1 is a positive integer greater than or equal to 1; R3 is Any one of oxygen atoms, sulfur atoms or straight-chain or branched aliphatic divalent groups with more than 6 carbon atoms, wherein n2 is a positive integer from 1 to 6; the heterocyclic aromatic group refers to an aromatic group whose ring-constituting atoms contain at least one heteroatom in addition to carbon atoms; the polycyclic aromatic group refers to an aromatic group in which two or more benzene rings are connected in the form of a condensed ring.
[0012] Preferably, in terms of mole percentage, it is derived from the following monomers:
[0013] Bisphenol A 25-35 mol%
[0014] 15-25 mol% of bisphenol monomer containing cyano aromatic group;
[0015] 4,4'-Dichlorodiphenyl sulfone 47-51 mol%.
[0016] Specifically, the bisphenol containing cyano aromatic group is selected from:
[0017] Any one of .
[0018] Preferably, in the bisphenol containing cyano aromatic groups, R1 and R2 are At least one of, and R3 is At least one sulfur atom.
[0019] Specifically preferably, the bisphenol containing cyano aromatic group is selected from:
[0020] At least one of .
[0021] More preferably, the bisphenol containing cyano aromatic group is selected from:
[0022] At least one of .
[0023] In order to improve other physical properties of the polysulfone resin, 0-0.05 mol% of other monomers are also included, calculated by molar percentage, and the other monomers are selected from bisphenol S, bisphenol F, biphenol, hydroquinone, resorcinol, 4,4-difluorodiphenyl sulfone, 4,4-dibromodiphenyl sulfone, bis(2 At least one of chlorophenyl) sulfone.
[0024] The weight average molecular weight of the polysulfone resin of the present invention is in the range of 45,000-80,000 Daltons.
[0025] The polymerization method of the polysulfone resin of the present invention comprises the following steps:
[0026] Salt-forming reaction: Add solvent to the reactor, stir and heat to 50-70°C, add bisphenol A, 4,4'-dichlorodiphenyl sulfone and bisphenol monomer containing cyano aromatic group, then add salt-forming agent and water-separating agent, continue stirring and heat to 170-200°C, and form salt for 1-4h;
[0027] Polymerization reaction: evaporate the water-separating agent, raise the temperature to 190-210°C, stir at a speed of 40-70r / min, keep the temperature constant for 9-15h, increase the stirring speed to 80-100r / min to the set viscosity, and obtain a polysulfone resin viscous liquid, which is then cooled, crushed, filtered, washed, and dried to obtain the product;
[0028] The solvent is at least one of N-methylpyrrolidone, N,N'-dimethylformamide, N,N'-dimethylacetamide, diphenyl sulfone, dimethyl sulfoxide and cyclopentane; the salt-forming agent is potassium hydroxide, potassium carbonate, sodium hydroxide or sodium carbonate; the molar amount of the salt-forming agent is 1.05-1.5 times the molar amount of 4,4-dichlorodiphenyl sulfone; the water-separating agent is at least one of toluene, xylene, mesitylene, o-trimethylbenzene, m-trimethylbenzene, ethylbenzene, ethylbenzene and ethylidene.
[0029] The present invention has the following beneficial effects:
[0030] The present invention introduces a bisphenol monomer containing a cyano aromatic group into the repeating unit of the traditional polysulfone resin, so that the main chain of the macromolecule contains a large number of aromatic rings and the side chain is a cyano group, thereby giving the polymer higher heat resistance, increasing the wear resistance and mechanical strength of the product, improving the problem of wear resistance, and broadening its application in the fields of automotive heat-resistant parts, aerospace wear-resistant parts, aviation bearings, etc. DETAILED DESCRIPTION
[0031] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0032] The sources of experimental raw materials used in the present invention are as follows:
[0033] Bisphenol A, 4,4'-dichlorodiphenyl sulfone, resorcinol, bisphenol monomer containing cyano aromatic group, solvent, catalyst and other raw materials are commercially available.
[0034] Bisphenol monomer A containing cyano aromatic group:
[0035]
[0036] Bisphenol monomer B containing cyano aromatic group:
[0037]
[0038] Bisphenol monomer C containing cyano aromatic group:
[0039]
[0040] Bisphenol monomer D containing cyano aromatic group:
[0041]
[0042] Bisphenol monomer E containing cyano aromatic group:
[0043]
[0044] Bisphenol monomer F containing cyano aromatic group:
[0045]
[0046] Various test methods:
[0047] (1) Tensile strength: test method refers to ISO527;
[0048] (2) Heat deformation temperature: test method refers to ISO 75-1 / -2;
[0049] (3) Dynamic friction coefficient: the test method refers to GB / T3960.
[0050] Table 1: Molar content of repeating units of polysulfone resin in embodiments and comparative examples and test results
[0051]
[0052] It can be seen from Examples 1-6 that the preferred bisphenol monomer containing cyano aromatic groups has better properties.
[0053] Table 1 continued:
[0054]
[0055]
[0056] It can be seen from Examples 1 / 7-11 that the preferred monomer ratios provide better performance.
[0057] It can be seen from Examples 10 / 12 that a small amount of other monomers does not affect the basic properties of the polysulfone resin of the present invention.
[0058] Table 1 continued:
[0059]
[0060] It can be seen from Comparative Example 1 that the friction coefficient of the polysulfone resin that does not contain the bisphenol monomer containing a cyano aromatic group is larger.
[0061] It can be seen from Comparative Examples 2 / 3 that when the content of each monomer is not within the scope of the present invention, the various properties are poor.
Claims
1. A polysulfone resin, characterized in that In mole percent, derived from monomers including: Bisphenol A 25-35mol%, Bisphenol monomer containing cyano aromatic group 15-25 mol%; 4,4'-Dichlorodiphenyl sulfone 47-51 mol%; Wherein, the bisphenol monomer containing a cyano aromatic group is selected from any one of the following chemical formulas: 、 、 、 、 、 。 2. The polysulfone resin according to claim 1, characterized in that The bisphenol containing cyano aromatic group is selected from: 、 、 At least one of .
3. The polysulfone resin according to claim 2, characterized in that The bisphenol containing cyano aromatic group is selected from: 、 At least one of .
4. The polysulfone resin according to claim 1, characterized in that In terms of molar percentage, 0-0.05 mol % of other monomers are also included, and the other monomers are selected from at least one of bisphenol S, bisphenol F, biphenol, hydroquinone, resorcinol, 4,4-difluorodiphenyl sulfone, 4,4-dibromodiphenyl sulfone, and bis(2-chlorophenyl) sulfone.
5. The polysulfone resin according to claim 1, characterized in that The weight average molecular weight of the polysulfone resin is in the range of 45,000-80,000 Daltons.
6. The method for polymerizing a polysulfone resin according to any one of claims 1 to 5, characterized in that: The following steps are involved: Salt-forming reaction: Add solvent to the reactor, stir and heat to 50-70°C, add bisphenol A, 4,4'-dichlorodiphenyl sulfone and bisphenol monomer containing cyano aromatic group, then add salt-forming agent and water-separating agent, continue stirring and heat to 170-200°C, and form salt for 1-4h; Polymerization reaction: evaporate the water-separating agent, then heat to 190-210°C, stir at a speed of 40-70r / min, keep constant temperature for 9-15h, increase the stirring speed to 80-100r / min to the set viscosity, and obtain polysulfone resin viscous liquid, which is then cooled, crushed, filtered, washed and dried to obtain the product; The solvent is at least one of N-methylpyrrolidone, N,N'-dimethylformamide, N,N'-dimethylacetamide, diphenyl sulfone, dimethyl sulfoxide and sulfolane; The salt-forming agent is potassium hydroxide, potassium carbonate, sodium hydroxide or sodium carbonate; the molar amount of the salt-forming agent is 1.05-1.5 times the molar amount of 4,4-dichlorodiphenyl sulfone; The water-separating agent is at least one of toluene, xylene, mesitylene, o-trimethylbenzene and ethylbenzene.
Citation Information
Patent Citations
Cyanogens radical containing phenyl-hydrochinone monomer, preparation method and application thereof
CN101219968A
Novel dihydric phenol and production thereof
JP1987145054A
Cited By
Sulfone polymer capable of improving heat resistance as well as preparation method and application of sulfone polymer
CN120309945A