tunable copper-based electronic paste system and its preparation method

By preparing a copper-based electronic paste system composed of nano-copper powder and organic phase, the problems of poor conductivity uniformity and stability of existing electronic pastes were solved, and the conductivity stability and resistance value adjustment of thick film resistors were realized, thus broadening the application conditions.

CN117198593BActive Publication Date: 2026-11-10CHINA ELECTRIC POWER RESEARCH INSTITUTE CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311302609.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-09
Publication Date
2026-11-10
Estimated Expiration
2043-10-09

AI Technical Summary

Technical Problem

The conductivity uniformity and stability of existing electronic pastes are poor, which affects their performance.

Method used

A tunable copper-based electronic paste system composed of nano-copper powder, glass powder, and organic phase is used. Nano-copper powder and organic phase are prepared through specific steps, and then mixed with glass powder. The mixture is printed onto a substrate and heat-treated to form a thick film resistor.

Benefits of technology

It achieves conductivity stability and uniformity of thick film resistors, can adjust the resistance value within a certain range, maintains structural stability at high temperatures, and has low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117198593B_ABST
    Figure CN117198593B_ABST
Patent Text Reader

Abstract

This invention provides a tunable copper-based electronic paste system and its preparation method, relating to the technical field of electronic materials. The electronic paste system includes nano-copper powder, glass powder, and an organic phase. The preparation method of the tunable copper-based electronic paste system specifically includes the following steps: S1. Preparing nano-copper powder; S2. Mixing the organic phase, glass powder, and the nano-copper powder from step S1 evenly, followed by grinding to obtain the electronic paste. This invention applies the electronic paste prepared using nano-copper powder as the functional phase to the fabrication of thick-film resistors. The thick-film resistors exhibit stable internal structures and form a uniformly dispersed conductive network, demonstrating excellent conductivity stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of electronic materials, specifically to a tunable copper-based electronic paste system and its preparation method. Background Technology

[0002] Electronic pastes, as a novel type of conductive composite material, are widely used in the manufacture of printed circuits for thick-film resistor integration, various resistors, crystalline silicon solar cell devices, lithium-ion battery electrodes, and other emerging technological fields. Conductive fillers are a crucial component of electronic pastes; their morphology, particle size, and content determine the electrical properties of the electronic paste and also affect its other physical properties after sintering. Therefore, preparing a stable conductive filler and developing corresponding electronic paste formulations with excellent performance is of great application significance.

[0003] In recent years, many researchers have attempted to prepare electronic pastes and study their conductivity using different types of conductive fillers, including carbon-based, metallic, and metal oxide-based fillers. However, existing electronic pastes still have certain shortcomings, such as uneven conductivity and poor mechanical properties. Nano-copper powder, as a widely used metallic material, possesses excellent conductivity, making it a promising candidate for applications in composite conductive materials and thermal conductivity. Summary of the Invention

[0004] (a) Technical problems to be solved

[0005] To address the shortcomings of existing technologies, this invention provides a controllable copper-based electronic paste system and its synthesis method, solving the technical problems of poor conductivity uniformity and stability of existing electronic pastes.

[0006] (II) Technical Solution

[0007] To achieve the above objectives, the present invention provides the following technical solution:

[0008] A tunable copper-based electronic paste system, including nano-copper powder, glass powder, and organic phase.

[0009] The preparation method of the tunable copper-based electronic paste system specifically includes the following preparation steps:

[0010] S1. Preparation of nano-copper powder

[0011] S1.1. Add 1.0–3.0 g CuSO4·5H2O to 40–60 mL C2H5OH and stir at room temperature for 0.5–2 h. Then add 1.0–3.0 g NaOH and stir for another 0.5–2 h.

[0012] S1.2. Transfer the above mixture to a 70-120 mL tetrafluoroethylene-lined stainless steel autoclave and heat at 140-180 °C for 4-8 h;

[0013] S1.3. The precipitate in the reactor was washed several times with ethanol and distilled water until the pH was 6.0-8.0, and then vacuum dried for 12-48 h to obtain nano copper powder;

[0014] S2. Preparation of organic phase

[0015] S2.1. Mix terpineol, butyl carbitol acetate, and tributyl citrate, and stir until homogeneous at 70-90°C;

[0016] S2.2. Simultaneously add ethyl cellulose for thickening. After the ethyl cellulose is completely dissolved, add leveling agent, Span 85 and castor oil. Stir everything evenly and let stand for 48 hours. If there is no precipitation or layering, the preparation is complete.

[0017] S2.3. Mix the organic phase with the glass powder and the nano copper powder from step S1 until homogeneous, and then grind them to obtain the electronic paste.

[0018] Preferably, the amount of terpineol added accounts for 57% of the total organic phase material, the amount of butyl carbitol acetate added accounts for 19% of the total organic phase material, the amount of tributyl citrate added accounts for 19% of the total organic phase material, the amount of leveling agent added accounts for 1% of the total organic phase material, the amount of Span 85 added accounts for 0.5% of the total organic phase material, the amount of castor oil added accounts for 0.5% of the total organic phase material, and the amount of ethyl cellulose added accounts for 3% of the total organic phase material.

[0019] Preferably, the nano-copper powder in step S1 accounts for 5-50% of the solid content of the electronic paste system.

[0020] The electronic paste system prepared above is printed onto a substrate to prepare a thick-film resistor. The specific preparation method is as follows:

[0021] S3.1. Clean the substrate with deionized water and anhydrous ethanol and then dry it;

[0022] S3.2. The prepared electronic paste is printed onto the substrate by screen printing, and then dried in a muffle furnace at 200-300°C.

[0023] S3.3. Thick film resistor samples are prepared by heat treatment at 600-800℃ under the action of protective gas.

[0024] Preferably, the substrate is any one of aluminum oxide, aluminum nitride, and boron nitride.

[0025] Preferably, the protective gas is any one of helium, nitrogen, and argon.

[0026] Preferably, by changing the proportion of the nano-copper powder in the electronic paste system, the resistance value of the thick film resistor can be controllably adjusted within the range of 124Ω / □ to 1503Ω / □.

[0027] (III) Beneficial Effects

[0028] This invention provides a tunable copper-based electronic paste system and its preparation method. Compared with the prior art, it has the following advantages:

[0029] 1. Electronic pastes prepared using nano-copper powder as the functional phase are applied to the fabrication of thick-film resistors. These thick-film resistors exhibit stable and uniformly dispersed internal structures, forming a uniform conductive network and demonstrating excellent conductivity stability. Copper-based electronic pastes possess low sheet resistance and resistivity, and the widest possible sheet resistance adjustment range can be achieved by adjusting the solid content of the nano-copper powder functional phase within the electronic paste system.

[0030] 2. In an air atmosphere at 400℃, thick film resistors using nano copper powder as the functional phase can still maintain structural and compositional stability, and the oxidation phenomenon above 400℃ is reversible, which broadens its application conditions and can meet the requirements of various application scenarios.

[0031] 3. The overall preparation process is simple and controllable, with low cost, and has broad application prospects. Attached Figure Description

[0032] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0033] Figure 1 Scanning electron microscope (SEM) images of the electronic pastes from Example 1 and Comparative Examples 1, 2, and 3;

[0034] in, Figure 1 a, Figure 1 b is a scanning electron microscope (SEM) characterization of the paste using micron-sized porous carbon as the functional phase; Figure 1 c. Figure 1 d is a scanning electron microscope (SEM) characterization of the paste using carbon nanotubes as the functional phase;

[0035] Figure 1 e Figure 1 f is a scanning electron microscope (SEM) characterization of the slurry using biochar as the functional phase; Figure 1g、 Figure 1 h is a scanning electron microscope (SEM) characterization of the paste using nano-copper powder as the functional phase.

[0036] Figure 2 The sheet resistance diagrams are for the thick film resistors of Example 1 and Comparative Examples 1, 2, and 3. Detailed Implementation

[0037] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0038] This invention provides an adjustable copper-based electronic paste system and its preparation method, which solves the technical problem of poor conductivity uniformity and stability of existing electronic pastes. The thick film resistor prepared by the electronic paste disclosed in this invention has good mechanical properties and conductivity stability. Furthermore, by adjusting the solid content of the nano-copper powder functional phase in the electronic paste system, the resistance value of the thick film resistor can be effectively adjusted.

[0039] To better understand the above technical solutions, the following will provide a detailed explanation of the technical solutions in conjunction with the accompanying drawings and specific implementation methods.

[0040] Example 1

[0041] The preparation method of the tunable copper-based electronic paste system specifically includes the following steps:

[0042] S1. Preparation of nano-copper powder

[0043] S1.1. Add 2.0 g CuSO4·5H2O to 50 mL C2H5OH and stir at room temperature for 0.5 h. Then add 2.0 g NaOH and stir for another 1 h.

[0044] S1.2. Transfer the mixture to a 100 mL PTFE-lined stainless steel autoclave and heat at 160 °C for 6 h;

[0045] S1.3. The precipitate in the reactor was washed several times with ethanol and distilled water until the pH reached 7.0, and then vacuum dried for 24 hours to obtain nano-copper powder.

[0046] S2. Preparation of organic phase

[0047] S2.1. Mix 57% of terpineol, 19% of butyl carbitol acetate, and 19% of tributyl citrate, and stir evenly at 70°C. At the same time, add 3% ethyl cellulose for thickening. After the ethyl cellulose is completely dissolved, add 1% leveling agent, 0.5% Span 85, and 0.5% castor oil. Stir evenly to complete the preparation.

[0048] S2.2. The organic phase, glass powder, and nano copper powder are ground using a low-speed ball mill to obtain the electronic paste.

[0049] The electronic paste prepared above is applied to the field of thick film resistors. The specific method for preparing thick film resistors is as follows:

[0050] S3. The alumina substrate is cleaned with deionized water and anhydrous ethanol and dried. Then, the prepared electronic paste is printed onto the substrate by screen printing. The substrate is placed in a muffle furnace and heated to 250°C to dry it. Finally, the copper-based thick film resistor is obtained by heat treatment at 800°C under the protection of argon.

[0051] Example 2

[0052] The preparation method of the tunable copper-based electronic paste system specifically includes the following steps:

[0053] S1. Preparation of nano-copper powder

[0054] S1.1. Add 3.0g CuSO4·5H2O to 60mL C2H5OH and stir at room temperature for 1h. Then add 1.0g NaOH and stir for another 1h.

[0055] S1.2. Transfer the mixture to a 100 mL PTFE-lined stainless steel autoclave and heat at 140 °C for 6 h;

[0056] S1.3. The precipitate in the reactor was washed several times with ethanol and distilled water until the pH reached 6.0, and then vacuum dried for 12 hours to obtain nano-copper powder.

[0057] S2. Preparation of organic phase

[0058] S2.1. Mix 57% of terpineol, 19% of butyl carbitol acetate, and 19% of tributyl citrate, and stir evenly at 70°C. At the same time, add 3% ethyl cellulose for thickening. After the ethyl cellulose is completely dissolved, add 1% leveling agent, 0.5% Span 85, and 0.5% castor oil. Stir evenly to complete the preparation.

[0059] S2.2. The organic phase, glass powder, and nano copper powder are ground using a low-speed ball mill to obtain the electronic paste.

[0060] The electronic paste prepared above is applied to the field of thick film resistors. The specific method for preparing thick film resistors is as follows:

[0061] S3. The aluminum nitride substrate is cleaned with deionized water and anhydrous ethanol and dried. Then, the prepared electronic paste is printed onto the substrate by screen printing. The substrate is placed in a muffle furnace and heated to 220°C to dry it. Finally, under the protection of helium, it is heat-treated at 600°C to obtain a copper-based thick film resistor.

[0062] Example 3

[0063] The preparation method of the tunable copper-based electronic paste system specifically includes the following steps:

[0064] S1. Preparation of nano-copper powder

[0065] S1.1. Add 1.0 g CuSO4·5H2O to 50 mL C2H5OH and stir at room temperature for 0.5 h. Then add 3.0 g NaOH and stir for another 1 h.

[0066] S1.2. Transfer the mixture to a 90 mL PTFE-lined stainless steel autoclave and heat at 160 °C for 6 h;

[0067] S1.3. The precipitate in the reactor was washed several times with ethanol and distilled water until the pH reached 7.0, and then vacuum dried for 48 hours to obtain nano-copper powder.

[0068] S2. Preparation of organic phase

[0069] S2.1. Mix 57% of terpineol, 19% of butyl carbitol acetate, and 19% of tributyl citrate, and stir evenly at 70°C. At the same time, add 3% ethyl cellulose for thickening. After the ethyl cellulose is completely dissolved, add 1% leveling agent, 0.5% Span 85, and 0.5% castor oil. Stir evenly to complete the preparation.

[0070] S2.1. The organic phase, glass powder, and nano copper powder are ground using a low-speed ball mill to obtain the electronic paste.

[0071] The electronic paste prepared above is applied to the field of thick film resistors. The specific method for preparing thick film resistors is as follows:

[0072] S3. The boron nitride substrate was cleaned with deionized water and anhydrous ethanol and dried. Then, the prepared electronic paste was printed onto the substrate by screen printing. The substrate was placed in a muffle furnace and heated to 260°C to dry it. Finally, under the protection of nitrogen, the substrate was heat-treated at 800°C to obtain a copper-based thick film resistor.

[0073] Comparative Example 1

[0074] The preparation method of the carbon-based electronic paste system specifically includes the following steps:

[0075] S1. Preparation of functional phases

[0076] S1.1. Place 5.0g of EDTA-2Na into a tube furnace and pyrolyze it under an argon atmosphere. Heat the mixture to 800℃ at a heating rate of 5℃ / min and hold it at that temperature for 2 hours. Remove the mixture after it cools naturally.

[0077] S1.2. The material obtained after calcination is first washed several times with 0.3M hydrochloric acid, and then washed repeatedly with deionized water until the pH value is 7.0;

[0078] S1.3. The sample was vacuum dried at 70℃ for 12h to obtain micron-sized porous carbon.

[0079] S2. Preparation of organic phase

[0080] S2.1. Mix 57% of terpineol, 19% of butyl carbitol acetate, and 19% of tributyl citrate, and stir evenly at 70°C. At the same time, add 3% ethyl cellulose for thickening. After the ethyl cellulose is completely dissolved, add 1% leveling agent, 0.5% Span 85, and 0.5% castor oil. Stir evenly to complete the preparation.

[0081] S2.2. The organic phase, glass powder, and micron-sized porous carbon are ground using a low-speed ball mill to obtain the electronic paste.

[0082] The electronic paste prepared above is applied to the field of thick film resistors. The specific method for preparing thick film resistors is as follows:

[0083] S3. The alumina substrate was cleaned with deionized water and anhydrous ethanol and dried. Then, the prepared electronic paste was screen-printed onto the substrate, and the substrate was dried in a muffle furnace at 250°C. Finally, the thick film resistor was obtained by heat treatment at 800°C under argon as a protective gas.

[0084] Comparative Example 2

[0085] The preparation method of the carbon-based electronic paste system specifically includes the following steps:

[0086] S1. Preparation of functional phases

[0087] S1.1. Acidify 0.8g of CNTs with an average diameter of 8-15nm and a length of 0.5-2mm in a mixed solution of 6ml concentrated sulfuric acid and 18ml nitric acid (volume ratio 1:3) at 80℃ for 2h.

[0088] S1.2. Wash the sample with deionized water until the pH reaches 7.0, centrifuge to collect the precipitate and dry it under vacuum at 60°C to obtain CNTs.

[0089] S2. Preparation of organic phase

[0090] S2.1. Mix 57% of terpineol, 19% of butyl carbitol acetate, and 19% of tributyl citrate, and stir evenly at 70°C. At the same time, add 3% ethyl cellulose for thickening. After the ethyl cellulose is completely dissolved, add 1% leveling agent, 0.5% Span 85, and 0.5% castor oil. Stir evenly to complete the preparation.

[0091] S2.2. The organic phase, glass powder, and CNTs are ground using a low-speed ball mill to obtain the electronic paste.

[0092] The electronic paste prepared above is applied to the field of thick film resistors. The specific method for preparing thick film resistors is as follows:

[0093] S3. The alumina substrate is cleaned with deionized water and anhydrous ethanol and dried. Then, the prepared electronic paste is printed onto the substrate by screen printing. The substrate is placed in a muffle furnace and heated to 250°C to dry it. Finally, the thick film resistor is obtained by heat treatment at 800°C under the protection of argon.

[0094] Comparative Example 3

[0095] The preparation method of the biochar-based electronic paste system specifically includes the following steps:

[0096] S1. Preparation of functional phases

[0097] S1.1. Wash the naturally fallen pine nuts several times with deionized water and ethanol, and dry them under vacuum at 60℃ to obtain clean pine nuts;

[0098] S1.2. Place 5.0g of clean pine nuts into a tube furnace and pyrolyze them under an argon atmosphere. Heat the pine nuts to 650℃ at a heating rate of 5℃ / min and hold for 2 hours. After natural cooling, remove the pine nuts to obtain biochar.

[0099] S2. Preparation of organic phase

[0100] S2.1. Mix 57% of terpineol, 19% of butyl carbitol acetate, and 19% of tributyl citrate, and stir evenly at 70°C. At the same time, add 3% ethyl cellulose for thickening. After the ethyl cellulose is completely dissolved, add 1% leveling agent, 0.5% Span 85, and 0.5% castor oil. Stir evenly to complete the preparation.

[0101] S2.2. The organic phase, glass powder, and biochar are ground using a low-speed ball mill to obtain the electronic slurry.

[0102] The electronic paste prepared above is applied to the field of thick film resistors. The specific method for preparing thick film resistors is as follows:

[0103] S3. The alumina substrate is cleaned with deionized water and anhydrous ethanol and dried. Then, the prepared electronic paste is printed onto the substrate by screen printing. The substrate is placed in a muffle furnace and heated to 250°C to dry it. Finally, the thick film resistor is obtained by heat treatment at 800°C under the protection of argon.

[0104] from Figure 1 The micron-sized porous carbon prepared in Comparative Example 1 can be observed in the scanning electron microscope image. Figure 1 a, Figure 1 b) and the biochar prepared in Comparative Example 3 ( Figure 1 e Figure 1 f) Porous structures of conductive powder at different magnifications. A comparison of the morphologies of the two porous carbon-based materials reveals that micron-sized porous carbon has thinner pore walls and a larger specific surface area, resulting in continuous conductive pathways; while biochar has thicker pore walls and discontinuous conductive pathways within. The carbon nanotubes prepared in Comparative Example 2 have a diameter of approximately 50 nm (…). Figure 1 c. Figure 1 d) While the particle size distribution is relatively uniform, the agglomeration problem is quite serious. This situation will inevitably affect the formation of conductive pathways to some extent. From Figure 1 g、 Figure 1 As can be seen from h, the size of the copper nanoparticles is relatively small, with a diameter of about 50-100 nm. This small size allows the surface of the electronic paste to have more conductive charges (small particles reduce porosity and increase density), which is beneficial to improving its conductivity and provides conditions for the formation of conductive pathways inside the thick film resistor.

[0105] like Figure 2The diagram shows the effect of solid content of different types of functional phase conductive fillers on the sheet resistance of thick-film resistors. Nano-copper powder exhibits a wide adjustable range within this range (adjustable from 124Ω / □ to 1503Ω / □). When the solid content of nano-copper powder is 5%, the thick-film resistor has a relatively high sheet resistance. This is because, under this condition, the nano-copper powder content is low, resulting in a narrow coverage area within the thick-film resistor, larger internal voids, less contact between conductive particles, and poor conductivity. When the solid content of nano-copper powder reaches 30% or more, the sheet resistance of the thick-film resistor begins to stabilize with increasing solid content. This is because at this solid content, the nano-copper powder is more widely distributed within the thick-film resistor, resulting in tighter connections between conductive particles and enhanced conductivity. Therefore, the sheet resistance of nano-copper powder thick-film resistors can be controlled by adjusting the solid content. Although the sheet resistance of thick film resistors with micron-porous carbon, carbon nanotubes and biochar as functional phase conductive fillers has the same trend as that of thick film resistors with nano-copper powder, the sheet resistance of carbon-based thick film resistors has a narrow adjustable range and cannot achieve low sheet resistance values ​​within the controllable range (324Ω / □-1326Ω / □, 499Ω / □-1425Ω / □, 286Ω / □-1313Ω / □, respectively).

[0106] In summary, compared with existing technologies, it has the following beneficial effects:

[0107] 1. Electronic pastes prepared using nano-copper powder as the functional phase are applied to the fabrication of thick-film resistors. These thick-film resistors exhibit stable and uniformly dispersed internal structures, forming a uniform conductive network and demonstrating excellent conductivity stability. Copper-based electronic pastes possess low sheet resistance and resistivity, and the widest possible sheet resistance adjustment range can be achieved by adjusting the solid content of the nano-copper powder functional phase within the electronic paste system.

[0108] 2. In an air atmosphere at 400℃, thick film resistors using nano copper powder as the functional phase can still maintain structural and compositional stability, and the oxidation phenomenon above 400℃ is reversible, which broadens its application conditions and can meet the requirements of various application scenarios.

[0109] 3. The overall preparation process is simple and controllable, with low cost, and has broad application prospects.

[0110] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0111] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a tunable copper-based electronic paste system, characterized in that, This is used to prepare a tunable copper-based electronic paste system, wherein the tunable copper-based electronic paste system includes nano-copper powder, glass powder, and an organic phase; The tunable copper-based electronic paste system specifically includes the following preparation steps: S1. Preparation of nano-copper powder; The specific method for obtaining the nano-copper powder is as follows: S1.

1. Add 1.0~3.0 g CuSO4·5H2O to 40~60 mL C2H5OH and stir at room temperature for 0.5~2 h, then add 1.0~3.0 g NaOH and stir for another 0.5~2 h; S1.

2. Transfer the above mixture to a 70-120 mL autoclave and heat at 140-180 °C for 4-8 h; S1.

3. The precipitate in the autoclave was washed several times with ethanol and distilled water until the pH was 6.0-8.0, and then vacuum dried for 12-48 h to obtain nano copper powder; S2. Prepare an organic phase, and mix the organic phase, glass powder and nano copper powder from step S1 evenly, and then grind them to obtain an electronic paste.

2. The preparation method of the tunable copper-based electronic paste system as described in claim 1, characterized in that, The organic phase in step S2 is prepared using the following method: S2.

1. Mix terpineol, butyl carbitol acetate, and tributyl citrate, and stir evenly at 70~90℃; S2.

2. Simultaneously add ethyl cellulose for thickening. After the ethyl cellulose is completely dissolved, add leveling agent, Span 85 and castor oil. Stir everything evenly and let stand for 48 hours. If there is no precipitation or layering, the preparation is complete.

3. The preparation method of the tunable copper-based electronic paste system as described in claim 2, characterized in that, The amount of terpineol added accounts for 57% of the total organic phase material, the amount of butyl carbitol acetate added accounts for 19% of the total organic phase material, the amount of tributyl citrate added accounts for 19% of the total organic phase material, the amount of leveling agent added accounts for 1% of the total organic phase material, the amount of Span 85 added accounts for 0.5% of the total organic phase material, the amount of castor oil added accounts for 0.5% of the total organic phase material, and the amount of ethyl cellulose added accounts for 3% of the total organic phase material.

4. The preparation method of the tunable copper-based electronic paste system as described in claim 1, characterized in that, The nano-copper powder in step S1 accounts for 5-50% of the solid content of the electronic paste system.

5. The application of a tunable copper-based electronic paste system, characterized in that, The electronic paste system of any one of claims 1-4 is printed onto a substrate to prepare a thick-film resistor. The specific preparation method is as follows: S3.

1. Clean the substrate with deionized water and anhydrous ethanol and then dry it; S3.

2. The prepared electronic paste is printed onto the substrate by screen printing and then dried by heating to 200~300 ℃; S3.

3. Thick film resistor samples were prepared by heat treatment at 600~800 ℃ under the action of protective gas.

6. The application of the tunable copper-based electronic paste system as described in claim 5, characterized in that, The substrate is any one of aluminum oxide, aluminum nitride, and boron nitride.

7. The application of the tunable copper-based electronic paste system as described in claim 5, characterized in that, The protective gas is any one of helium, nitrogen, or argon.

8. The application of the tunable copper-based electronic paste system as described in claim 5, characterized in that, By changing the proportion of the nano-copper powder in the electronic paste system, the resistance value of the thick film resistor can be controllably adjusted within the range of 124 Ω / □ to 1503 Ω / □.

Citation Information

Patent Citations

  • Copper electrode paste and preparation method thereof

    CN107622809A

  • Low-cost green preparation method of nano copper

    CN107745133A

  • Thick-film resistor structure and its production process

    JP2006229166A