A method for fabricating a multilayer HDI packaging substrate
By employing X-shaped hole filling electroplating and copper reduction treatment combined with the lamination of the outer PP material during the fabrication of multilayer HDI packaging substrates, the thickness control problem was solved, and production efficiency and finished product yield were improved.
Patent Information
- Application Number
- CN202311048975.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-08-18
AI Technical Summary
In existing technologies, controlling the thickness of multilayer HDI packaging substrates is difficult, resulting in low production efficiency and low finished product yield.
By combining X-shaped hole filling electroplating and copper reduction treatment with outer PP material lamination, the thickness of the inner and outer layers of the packaging substrate can be precisely controlled by controlling the thickness of the electroplating layer and the lamination process, thereby improving production efficiency and product yield.
It enables precise control of the thickness of multilayer HDI packaging substrates, improving production efficiency and yield, and reducing processing difficulty.
Smart Images

Figure CN117198891B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor process technology, and in particular to a method for fabricating a multilayer HDI packaging substrate. Background Technology
[0002] As High Density Interconnect (HDI) products continue to evolve towards smaller, thinner, and more highly integrated designs, a demand for multilayer HDI packaging substrates has emerged in the market. Due to the increased number of layers, the thickness requirements for the packaging substrate are becoming increasingly stringent. This places strict demands on engineering design and the parameters of various manufacturing processes (lamination, solder masking, electroplating, etc.). The process is wide-ranging, involves long workflows, and has many control points, making it difficult to control the overall board thickness in actual production. Summary of the Invention
[0003] This invention aims to at least solve one of the technical problems existing in the prior art. To this end, this invention proposes a method for manufacturing a multilayer HD I package substrate, which can improve the accuracy of thickness control of the package substrate, and improve production efficiency and finished product yield.
[0004] In a first aspect, embodiments of the present invention provide a method for fabricating a multilayer HDI packaging substrate, comprising:
[0005] X-shaped holes are obtained by inner layer laser engraving on copper-clad substrates;
[0006] The X-shaped holes are filled by electroplating to obtain an electroplated layer;
[0007] The electroplated layer is subjected to copper reduction treatment;
[0008] PP material is laminated onto the outer layer of the copper-clad substrate;
[0009] The target point is drilled out using a target drilling machine, and the outer layer blind hole laser is performed based on the target point.
[0010] The outer layer blind holes obtained by laser engraving are filled with electroplating to obtain the outer layer pattern;
[0011] The process involves solder resist, nickel-gold plating, and molding to obtain a multilayer HDI packaging substrate.
[0012] According to some embodiments of the present invention, the process of filling the X-shaped holes with electroplating to obtain an electroplated layer includes:
[0013] The copper-clad substrate is degreased and acid-washed;
[0014] The copper-clad substrate is placed in a copper bath, the components of which include copper sulfate, sulfuric acid, chloride ions, brightener, leveling agent and wetting agent;
[0015] The electroplating layer is obtained by performing inner-layer hole-filling electroplating according to the set electroplating time.
[0016] According to some embodiments of the present invention, the concentration range of the degreasing agent used for degreasing is 150 to 200 ml / L, and the degreasing temperature range is 35 to 45 degrees Celsius; the concentration range of the sulfuric acid used for pickling is 2% to 5%, and the pickling temperature is 25 to 30 degrees Celsius; the concentration range of the copper sulfate is 200 to 250 g / L.
[0017] According to some embodiments of the present invention, the concentration of the sulfuric acid is in the range of 40 to 60 g / L, the concentration of the chloride ion is in the range of 40 to 60 ppm, the concentration of the brightener is in the range of 0.5 to 2 ppm, the concentration of the leveling agent is in the range of 12 to 16 ppm, and the concentration of the wetting agent is in the range of 15 to 25 ppm.
[0018] According to some embodiments of the present invention, the thickness of the electroplated layer ranges from 15 to 20 micrometers, the electroplating time ranges from 40 to 60 minutes, and the thickness of the electroplated layer after copper reduction treatment ranges from 10 to 14 micrometers.
[0019] According to some embodiments of the present invention, the copper reduction treatment of the electroplated layer includes:
[0020] The electroplated layer is pickled;
[0021] The copper-clad substrate is placed in a copper reduction tank, the solution in which the copper reduction tank consists of sulfuric acid, hydrogen peroxide and copper ions;
[0022] Copper reduction is performed based on the preset etching amount and line speed.
[0023] According to some embodiments of the present invention, the sulfuric acid concentration used for pickling the electroplated layer ranges from 3% to 5%; the sulfuric acid concentration in the copper reduction tank ranges from 250 to 300 g / L; the hydrogen peroxide concentration ranges from 2% to 6%; the copper ion concentration is less than or equal to 40 g / L; the etching amount ranges from 5 to 10 micrometers; and the linear velocity ranges from 3 to 5 meters per minute.
[0024] According to some embodiments of the present invention, the outer lamination PP material of the copper-clad substrate comprises:
[0025] Add copper cylinder blocks to the surface of the copper-clad substrate;
[0026] Add a resist pattern to the edge of the copper-clad substrate;
[0027] PP material is bonded to the outer layer of the copper-clad substrate at high temperature.
[0028] According to some embodiments of the present invention, the thickness of the PP material after lamination ranges from 18 to 20 micrometers.
[0029] According to some embodiments of the present invention, the diameter of the outer blind hole is less than 50 micrometers, and the indentation of the outer blind hole ranges from ±5 micrometers.
[0030] Embodiments of the present invention include: laser engraving an inner layer of a copper-clad substrate to obtain X-shaped holes; performing hole-filling electroplating on the X-shaped holes to obtain an electroplated layer; performing copper reduction treatment on the electroplated layer; laminating PP material onto the outer layer of the copper-clad substrate; drilling target points using a target drilling machine, and performing outer layer blind hole laser engraving based on the target points; performing hole-filling electroplating on the laser-obtained outer layer blind holes to obtain an outer layer pattern; and sequentially performing solder resist, nickel-gold electroplating, and molding to obtain a multilayer HDI packaging substrate. According to the technical solution of this embodiment, the thickness of the electroplated layer can be adjusted by the copper reduction treatment, and the thickness of the outer PP material can be more accurately controlled by the lamination process, improving the accuracy of controlling the thickness of the inner and outer layers of the packaging substrate, and increasing production efficiency and product yield. Attached Figure Description
[0031] Figure 1 This is a flowchart of a method for manufacturing a multilayer HDI packaging substrate according to an embodiment of the present invention;
[0032] Figure 2 This is a flowchart of an inner layer via-filling electroplating process provided in another embodiment of the present invention;
[0033] Figure 3 This is a flowchart of a copper reduction process provided in another embodiment of the present invention;
[0034] Figure 4 This is a flowchart of an outer layer PP material provided in another embodiment of the present invention. Detailed Implementation
[0035] Embodiments of the present invention are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0036] In the description of this invention, it should be understood that the orientation descriptions, such as up, down, front, back, left, right, etc., are based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limiting this invention.
[0037] In the description of this invention, "several" means one or more, "more than" means two or more, "greater than," "less than," and "exceeding" are understood to exclude the stated number, while "above," "below," and "within" are understood to include the stated number. The use of "first" and "second" in the description is merely for distinguishing technical features and should not be construed as indicating or implying relative importance, or implicitly indicating the number of indicated technical features, or implicitly indicating the order of the indicated technical features.
[0038] This invention provides a method for fabricating a multilayer HDI packaging substrate. The method includes: laser-drilling an inner layer of a copper-clad substrate to obtain X-shaped holes; performing hole-filling electroplating on the X-shaped holes to obtain an electroplated layer; performing copper reduction treatment on the electroplated layer; laminating PP material onto the outer layer of the copper-clad substrate; drilling target points using a target drilling machine; performing outer layer blind hole laser-drilling based on the target points; performing hole-filling electroplating on the laser-derived outer layer blind holes to obtain an outer layer pattern; and sequentially performing solder resist, nickel-gold electroplating, and molding to obtain a multilayer HDI packaging substrate. According to the technical solution of this embodiment, the thickness of the electroplated layer can be adjusted by the copper reduction treatment, and the thickness of the outer PP material can be more accurately controlled by the lamination process, improving the accuracy of controlling the thickness of the inner and outer layers of the packaging substrate, and increasing production efficiency and yield.
[0039] The embodiments of the present invention will be further described below with reference to the accompanying drawings.
[0040] like Figure 1 As shown, Figure 1 This is a flowchart of a method for fabricating a multilayer HDI packaging substrate according to an embodiment of the present invention. The method includes, but is not limited to, the following steps:
[0041] S1, an X-shaped hole is obtained by inner layer laser engraving on the copper-clad substrate;
[0042] S2, fill the X-shaped holes with electroplating to obtain the electroplated layer;
[0043] S3, copper reduction treatment is applied to the electroplated layer;
[0044] S4, PP material is laminated onto the outer layer of the copper-clad substrate;
[0045] S5, drill the target point using a target drilling machine, and perform outer blind hole laser based on the target point;
[0046] S6, fill the blind holes obtained by laser processing with electroplating to obtain the outer layer pattern;
[0047] S7, in sequence, solder resist, nickel-gold plating and molding are performed to obtain a multilayer HDI packaging substrate.
[0048] It should be noted that the core thickness of common copper clad laminates can range from 40 micrometers to 100 micrometers, such as the common thicknesses of 40 micrometers, 60 micrometers, 80 micrometers, and 100 micrometers. In order to reduce the thickness of multilayer HDI packaging substrates, copper clad laminates with a core thickness of 40 micrometers can be used. If the low copper thickness on the surface of the copper clad laminate is large, such as reaching a thickness of 10 to 12 micrometers, the low copper on the surface of the copper clad laminate can be reduced before electroplating to reduce the bottom copper thickness on both sides of the copper clad laminate, for example, reducing the bottom copper thickness to 3 to 4 micrometers. Of course, if the low copper thickness is already in the range of 3 to 4 micrometers, this copper reduction treatment can be omitted to reduce process steps, as long as the thickness requirements of the copper clad laminate are met.
[0049] It should be noted that laser-drilling inner layers of copper-clad laminates is a technique well-known to those skilled in the art, and the specific laser principle is not limited here. In related technologies, inner layer laser-drilled holes are usually cylindrical holes. However, cylindrical holes have the disadvantages of being difficult to fill with metal and having a slow filling speed during the electroplating process. Moreover, because cylindrical holes are regular in shape, the rising speed of the electroplated layer is stable, making it difficult to control the thickness of the electroplated layer and easily leading to an excessively thick electroplated layer. In contrast, this embodiment uses X-shaped holes, with the cross-section gradually increasing from the inside to the outside. This makes the thickness increase of the electroplated layer slower as it approaches the hole opening, allowing it to be removed in time after meeting the thickness requirements, and making it easier to control the thickness of the electroplated layer.
[0050] In one embodiment, the thickness of the electroplated layer ranges from 15 to 20 micrometers, the electroplating time ranges from 40 to 60 minutes, and the thickness of the electroplated layer after copper reduction treatment ranges from 10 to 14 micrometers.
[0051] It should be noted that the total thickness of the multilayer HDI packaging substrate needs to meet certain requirements. Taking a 4-layer HDI packaging substrate as an example, the total thickness of the packaging substrate is 140±30 micrometers. If a 40-micrometer thick copper-clad substrate is used, due to the double-sided copper structure, the sum of the inner and outer layer thicknesses on both sides is 30±15 micrometers. In this embodiment, the thickness control during electroplating is achieved by controlling the electroplating time to 40 to 60 minutes, combined with the shape of the X-shaped holes. However, to ensure sufficient hole filling, the thickness of the electroplated layer is usually 15 to 20 micrometers. If the outer layer is directly laminated on this basis, the thickness of the PP material needs to be reduced in order to meet the total thickness requirements, which increases the processing difficulty of lamination. Based on this, in order to further control and adjust the thickness, this embodiment performs a copper reduction treatment after electroplating, which etches the copper layer thickness of the electroplated layer. By using the copper reduction treatment as a thickness control process, the thickness of the electroplated layer after the copper reduction treatment is reduced from 15 to 20 micrometers to 10 to 14 micrometers. This not only makes the inner copper layer thinner, but also provides more margin for outer layer lamination and reduces the difficulty of lamination.
[0052] In one embodiment, the thickness of the laminated PP material ranges from 18 to 20 micrometers.
[0053] It should be noted that, according to the description of the above embodiments, the thickness of the copper-clad substrate is 40 micrometers, and the thickness of the inner electroplated layer after copper reduction is 10 to 14 micrometers. After the inner layer copper reduction is completed, it can be directly laminated onto the surface of the copper-clad substrate by high-temperature lamination, so that the PP material is fixedly connected to the inner layer to form the outer layer structure. In this embodiment, the thickness of the PP material can be 20 micrometers. By controlling the lamination parameters (such as temperature and pressure), the thickness of the PP material after lamination is in the range of 18 to 20 micrometers, ensuring that the thickness of one side of the packaging substrate reaches 68 to 74 micrometers. Since there are subsequent operations such as solder masking, the control of copper reduction and lamination parameters in this embodiment can ensure that the total thickness of the 4-layer HDI packaging substrate is controlled within the range of 140 ± 30 micrometers after subsequent processing.
[0054] It should be noted that after copper reduction and lamination are completed, the outer layer pattern needs to be manufactured. In this embodiment, a target point is drilled in the outer PP material using a target drilling machine. The target point is used as a positioning point for laser drilling of the outer blind hole, thereby completing the fabrication of the outer layer pattern. In this embodiment, the specific shape of the outer layer pattern is not limited. The position, shape and parameters of the target point and the target drilling machine can be selected according to the actual requirements of the outer layer pattern.
[0055] It is worth noting that, since there are many types of drilling machines, after determining the outer layer pattern, the target position and shape of the drilling machine can be determined according to the type of drilling machine, thereby improving the alignment accuracy and ensuring the accuracy of the blind hole position obtained by the subsequent outer layer laser. Those skilled in the art are familiar with how to set the parameters of the drilling machine, so we will not go into details here.
[0056] In one embodiment, the diameter of the outer blind hole is less than 50 micrometers, and the indentation of the outer blind hole ranges from ±5 micrometers.
[0057] It should be noted that the blind holes obtained by laser engraving the outer PP material can also be X-shaped holes. Since the blind hole is actually the outer layer pattern, it also needs to be filled by electroplating. After the blind hole is filled by electroplating, copper reduction treatment can also be performed to further control the thickness of the outer layer. The operation of filling electroplating and copper reduction treatment can refer to the description of the inner layer X-shaped hole above, and will not be repeated here.
[0058] It should be noted that if the diameter of the outer blind via is too large, it will result in an excessively large copper layer during electroplating, causing the depth of the outer blind via to exceed the requirements. Therefore, in this embodiment, the diameter of the outer blind via is controlled within 50 micrometers to improve the control convenience during electroplating and increase processing efficiency.
[0059] It should be noted that although this embodiment achieves thickness control in terms of the thickness of the inner and outer core boards, the thickness of the thermosetting sheet used for lamination, and the thickness of the inner and outer copper layers through the copper reduction treatment of the inner electroplating layer and the lamination of the outer PP layer, effectively reducing the thickness of the 4-layer HDI packaging substrate, after the outer layer pattern is made, it is still necessary to perform solder resist, nickel-gold plating and molding processes to complete the processing of the 4-layer HDI packaging substrate.
[0060] It is worth noting that the solder mask in this embodiment may include roughening, coating, exposure, and development. In the roughening process, the copper surface of the copper-clad substrate is roughened using a roughening solution, making the copper surface more rough and improving the adhesion of the coated ink. In the coating process, the substrate is held by a fixture, and ink is applied to the outer surface of the copper-clad substrate using an ink scraper and an ink roller, forming an ink layer on the surface of the copper-clad substrate. Through the exposure and development processes, windows can be opened in the ink layer to expose the outer layer pattern for electrical connection of the 4-layer HDI packaging substrate. Because the thickness control achieved in this embodiment through inner layer copper reduction and outer layer lamination, even with the ink layer, the thickness can still meet the requirements of the 4-layer HDI packaging substrate. Therefore, the thickness control in this embodiment can reduce the processing difficulty of subsequent processes and improve production efficiency and product yield.
[0061] It should be noted that the electroplating of nickel and gold and the molding in this embodiment are processes in related technologies, which can electroplat gold ions and nickel ions onto the copper layer and complete the molding of the packaging substrate.
[0062] In one embodiment, reference is made to Figure 2 , Figure 1 Step S2 shown also includes, but is not limited to, the following steps:
[0063] S21, Degreasing and pickling of copper-clad substrate;
[0064] S22, placing the copper-clad substrate in a copper bath, the components of the solution in the copper bath include copper sulfate, sulfuric acid, chloride ions, brightener, leveling agent and wetting agent;
[0065] S23, perform inner layer filling electroplating according to the set electroplating time to obtain the electroplated layer.
[0066] In one embodiment, the concentration of the degreasing agent used for degreasing ranges from 150 to 200 ml / L, and the degreasing temperature ranges from 35 to 45 degrees Celsius; the concentration of sulfuric acid used for pickling ranges from 2% to 5%, and the pickling temperature ranges from 25 to 30 degrees Celsius; the concentration of copper sulfate ranges from 200 to 250 g / L, the concentration of sulfuric acid ranges from 40 to 60 g / L, the concentration of chloride ions ranges from 40 to 60 ppm, the concentration of brightener ranges from 0.5 to 2 ppm, the concentration of leveling agent ranges from 12 to 16 ppm, and the concentration of wetting agent ranges from 15 to 25 ppm.
[0067] It should be noted that the surface of the copper-clad substrate is covered with low copper content. Before electroplating the X-shaped holes obtained by inner layer laser, the copper-clad substrate can be immersed in a degreasing agent with a concentration range of 150 to 200 ml / L for degreasing. The degreasing temperature range is 35 to 45 degrees Celsius. Through the degreasing process, the copper surface and the inside of the X-shaped holes can be cleaned, so that the hole walls form a positive charge, which improves the adsorption effect during electroplating.
[0068] It should be noted that after the degreasing process is completed, the copper surface has been cleaned well. However, the copper surface will generate oxides when it comes into contact with air. Therefore, in this embodiment, after degreasing, the copper-clad substrate is placed in an acid pickling tank for acid pickling. The concentration of sulfuric acid in the acid pickling tank is in the range of 2%-5%, and the temperature range is 25 to 30 degrees Celsius. This can effectively remove oxides from the metal surface and improve the adsorption effect during electroplating.
[0069] It should be noted that after degreasing and pickling, the copper-clad substrate is placed in a through-hole for electroplating. By controlling the electroplating parameters, the uniformity of the electroplated layer can be effectively improved, and the surface smoothness can be enhanced. The electroplating solution used in this embodiment includes copper sulfate, sulfuric acid, chloride ions, brightener, leveling agent, and wetting agent. The concentration range of copper sulfate is 200 to 250 g / L, the concentration range of sulfuric acid is 40 to 60 g / L, the concentration of chloride ions is 40 to 60 ppm, the concentration of brightener is 0.5 to 2 ppm, the concentration of leveling agent is 12 to 16 ppm, and the concentration of wetting agent is 15 to 25 ppm. Under the influence of electricity, copper sulfate, sulfuric acid, and chloride ions, copper ions in the solution are adsorbed onto the walls of the X-shaped holes to form a copper layer. The sulfuric acid component enables the copper ions to adhere better to the hole walls, the brightener makes the copper layer surface smoother and finer, the leveling agent improves the flatness of the copper layer surface, and the wetting agent allows the gas generated by the electrolytic solution during the electroplating process to escape quickly, thereby reducing or eliminating pinholes and improving product yield.
[0070] It should be noted that, in order to further improve thickness control, the thickness of the electroplated layer can be tested after electroplating is completed. If the thickness is within the range of 15 to 20 micrometers, it can be determined that the current electroplating parameters meet the requirements. Otherwise, the above parameters should be adjusted to reduce the impact of the quality of different batches of copper-clad substrates and the concentration of the solution on the thickness of the electroplated layer.
[0071] In one embodiment, reference is made to Figure 3 , Figure 1 Step S3 shown also includes, but is not limited to, the following steps:
[0072] S31, pickling the electroplated layer;
[0073] S32, the copper-clad substrate is placed in the copper reduction tank, the solution in the copper reduction tank includes sulfuric acid, hydrogen peroxide and copper ions;
[0074] S33 performs copper reduction processing based on preset etching amount and line speed.
[0075] In one embodiment, the sulfuric acid concentration used for pickling the electroplated layer ranges from 3% to 5%; the sulfuric acid concentration in the copper reduction bath ranges from 250 to 300 g / L, the hydrogen peroxide concentration ranges from 2% to 6%, and the copper ion concentration is less than or equal to 40 g / L; the etching amount ranges from 5 to 10 micrometers, and the linear velocity ranges from 3 to 5 meters per minute.
[0076] It should be noted that, referring to Figure 2 According to the description of the embodiment shown, pickling can remove oxides from the metal surface, allowing for sufficient contact of the copper layer during copper reduction. Therefore, pickling is required not only during through-hole plating but also before copper reduction. Since the initial pickling only removes oxides from the bottom copper surface, while through-hole plating increases the amount of copper in the holes, the copper layer area is increased. In this embodiment, the sulfuric acid concentration used for pickling the plating layer is higher than the sulfuric acid concentration used for pickling the copper-clad substrate before plating, for example, it can be increased to 3% to 5%.
[0077] It should be noted that after pickling, the substrate is placed in the copper reduction tank and moved from one side to the other under the driving action of a carrier or clamp. In this embodiment, the moving linear speed is determined according to the linear speed. During the movement, the electroplated layer is etched by the solution in the copper reduction tank, resulting in a thinner copper layer and achieving the copper reduction effect. The solution in the copper reduction tank in this embodiment includes sulfuric acid, hydrogen peroxide, and copper ions. The specific reaction principle will not be elaborated here.
[0078] It should be noted that the thickness of the electroplated layer ranges from 15 to 20 micrometers. To meet the requirement of 10 to 14 micrometers, the etching amount ranges from 5 to 10 micrometers. The linear speed of the substrate moving in the copper reduction bath is 3 to 5 meters per minute. The concentration of sulfuric acid in the copper reduction bath ranges from 250 to 300 g / L, the concentration of hydrogen peroxide ranges from 2% to 6%, and the concentration of copper ions is less than or equal to 40 g / L. To ensure that the thickness of the copper layer meets the standard after copper reduction, the thickness of the electroplated layer can be tested after the copper reduction treatment is completed. If the thickness of the electroplated layer is too thin or too thick, the concentration of the above solutions or the linear speed can be adjusted. Those skilled in the art are familiar with how to adjust the parameters to make the thickness of the electroplated layer meet the requirements, so it will not be elaborated here.
[0079] In one embodiment, reference is made to Figure 4 , Figure 1 Step S4 shown also includes, but is not limited to, the following steps:
[0080] S41, Add copper cylinder blocks to the surface of the copper-clad substrate;
[0081] S42, Add resist pattern to the edge of the copper-clad substrate;
[0082] S43, PP material is bonded to the outer layer of copper-clad substrate by high temperature.
[0083] It should be noted that the PP material needs to be laminated onto the copper-clad substrate at high temperature. Under high temperature, the PP material will flow. The less the flow, the thicker the PP layer after lamination. Therefore, in order to control the thickness, copper cylinders are added to the surface of the copper area of the copper-clad substrate, and adhesive resistance patterns are added to the board edge. The direction of adhesive flow is controlled during high-temperature lamination. When the inner copper layer is thick after copper reduction treatment, the flow is increased to reduce the thickness of the PP material after lamination. When the inner layer is usually thin after copper reduction treatment, the flow is reduced to improve the lamination effect.
[0084] Other embodiments of this application will readily occur to those skilled in the art upon consideration of the specification and practice of the embodiments disclosed herein. This application is intended to cover any variations, uses, or adaptations of this application that follow the general principles of this application and include common knowledge or customary techniques in the art not disclosed herein.
[0085] It should be understood that this application is not limited to the precise structure described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of this application is limited only by the appended claims.
[0086] The above provides a detailed description of the preferred embodiments of the present invention. However, the present invention is not limited to the above embodiments. Those skilled in the art can make various equivalent modifications or substitutions without departing from the spirit of the present invention. All such equivalent modifications or substitutions are included within the scope defined by the claims of the present invention.
Claims
1. A method for fabricating a multilayer HDI package substrate, the method comprising: include: X-shaped holes are obtained by inner layer laser engraving on copper-clad substrates; The X-shaped holes are filled by electroplating to obtain an electroplated layer; The electroplated layer is subjected to a copper reduction treatment to reduce the thickness of the electroplated layer to 10 to 14 micrometers; PP material is laminated onto the outer layer of the copper-clad substrate; The target point is drilled out using a target drilling machine, and the outer layer blind hole laser is performed based on the target point. The outer layer blind holes obtained by laser engraving are filled with electroplating to obtain the outer layer pattern; The process involves solder resist, nickel-gold plating, and molding to obtain a multilayer HDI packaging substrate.
2. The method for fabricating a multilayer HDI packaging substrate according to claim 1, characterized in that, The process of filling the X-shaped holes with electroplating to obtain the electroplated layer includes: The copper-clad substrate is degreased and acid-washed; The copper-clad substrate is placed in a copper bath, the components of which include copper sulfate, sulfuric acid, chloride ions, brightener, leveling agent and wetting agent; The electroplated layer is obtained by performing inner-layer hole-filling electroplating according to the set electroplating time.
3. The method for fabricating a multilayer HDI packaging substrate according to claim 2, characterized in that, The concentration range of the degreasing agent used for degreasing is 150 to 200 ml / L, and the degreasing temperature range is 35 to 45 degrees Celsius; the concentration range of the sulfuric acid used for pickling is 2% to 5%, and the pickling temperature is 25 to 30 degrees Celsius.
4. The method for fabricating a multilayer HDI packaging substrate according to claim 2, characterized in that, The concentration range of the copper sulfate is 200 to 250 g / L, the concentration range of the sulfuric acid is 40 to 60 g / L, the concentration of the chloride ion is 40 to 60 ppm, the concentration of the brightener is 0.5 to 2 ppm, the concentration of the leveling agent is 12 to 16 ppm, and the concentration of the wetting agent is 15 to 25 ppm.
5. The method for fabricating a multilayer HDI packaging substrate according to claim 2, characterized in that, The thickness of the electroplated layer ranges from 15 to 20 micrometers, the electroplating time ranges from 40 to 60 minutes, and the thickness of the electroplated layer after copper reduction treatment ranges from 10 to 14 micrometers.
6. The method for fabricating a multilayer HDI packaging substrate according to claim 5, characterized in that, The copper reduction treatment of the electroplated layer includes: The electroplated layer is pickled; The copper-clad substrate is placed in a copper reduction tank, the solution in which the copper reduction tank consists of sulfuric acid, hydrogen peroxide and copper ions; Copper reduction is performed based on the preset etching amount and line speed.
7. The method for fabricating a multilayer HDI packaging substrate according to claim 6, characterized in that, The sulfuric acid concentration used for pickling the electroplated layer ranges from 3% to 5%; the sulfuric acid concentration in the copper reduction tank ranges from 250 to 300 g / L; the hydrogen peroxide concentration ranges from 2% to 6%; the copper ion concentration is less than or equal to 40 g / L; the etching amount ranges from 5 to 10 micrometers; and the linear velocity ranges from 3 to 5 meters per minute.
8. The method for fabricating a multilayer HDI packaging substrate according to claim 1, characterized in that, The outer layer of the copper-clad substrate is laminated with PP material, comprising: Add copper cylinder blocks to the surface of the copper-clad substrate; Add a resist pattern to the edge of the copper-clad substrate; PP material is bonded to the outer layer of the copper-clad substrate at high temperature.
9. The method for fabricating a multilayer HDI packaging substrate according to claim 8, characterized in that, The thickness of the PP material after lamination ranges from 18 to 20 micrometers.
10. The method for fabricating a multilayer HDI packaging substrate according to claim 1, characterized in that, The diameter of the outer blind hole is less than 50 micrometers, and the indentation of the outer blind hole is within the range of ±5 micrometers.
Citation Information
Patent Citations
Manufacturing method of printed circuit board realizing any layer interconnection
CN107995803A
A HDI substrate machining process
CN109068490A