Plasma etching method and etching device
Through the multi-stage process of plasma etching method, the problem of difficult control of the bottom size of the hard mask layer etching pattern is solved, and high-quality etching morphology and memory yield improvement are achieved.
Patent Information
- Application Number
- CN202310506158.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-08
AI Technical Summary
During the formation of 3D NAND memory, the key dimensions at the bottom of the etching pattern of the hard mask layer are difficult to control, resulting in deformation and by-product sputtering during the etching process, affecting the quality and yield of the memory.
The plasma etching method is adopted to perform the first to third etching processes in sequence: the first etching process mainly uses anisotropic etching to form a second pattern with an etching depth not reaching the base layer; the second etching process Mainly isotropic etching, the etching material layer is completely etched to generate a third pattern with a preset key dimension at the bottom; the third etching process modifies the side walls of the third pattern to form the upper and lower contours The fourth graphic is consistent and the bottom key size reaches the preset.
High-quality etching of the hard mask layer is achieved, ensuring the sidewall perpendicularity and depth-to-face ratio of the etching pattern, improving the etching quality of the base layer by the next process, and reducing defect rate and processing costs.
Smart Images

Figure CN118919407A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductors, and in particular to a plasma etching method and an etching device. Background Art
[0002] NAND flash memory is a better storage device than hard disk drives. As people pursue non-volatile storage products with low power consumption, light weight and good performance, it has been widely used in electronic products. At present, the planar structure of NAND flash memory has reached the practical expansion limit. In order to further increase the storage capacity and reduce the storage cost per bit, 3D NAND memory is proposed.
[0003] In the process of forming existing 3D NAND memory, different materials need to be alternately deposited on the substrate to form a base layer of an overlapping structure, and through holes are etched in the base layer. As the storage capacity increases, the number of layers of the overlapping structure gradually increases, and the depth of the through holes in the base layer also increases accordingly. Since the etching selectivity of the hard mask layer and the base layer is relatively high, when the base layer is etched using a plasma etching process, a hard mask layer is usually formed on the base layer, and the etching pattern of the hard mask layer exposes the area of the base layer to be etched.
[0004] The etching of the hard mask layer is a high aspect ratio etching, and whether the morphology of the hard mask layer etching pattern meets the standard is crucial to the subsequent etching of the base layer. We hope that: 1) the sidewalls of the hard mask layer etching pattern are coherent and as vertical as possible to avoid pattern deformation during the etching process, resulting in the hard mask layer pattern not being well transferred to the base layer; 2) the critical dimension at the bottom of the hard mask layer etching pattern reaches the preset critical dimension, otherwise it will directly affect the through-hole size in the base layer.
[0005] Since low-frequency biased RF power can increase the bombardment force of plasma, in the prior art, low-frequency biased RF power is usually used in the etching process of the hard mask layer to increase the etching rate. In order to ensure that the hard mask layer is completely etched, the etching depth inevitably reaches the base layer. The byproducts generated during the plasma bombardment of the base layer are easily sputtered to the sidewalls of the hard mask layer pattern and are difficult to remove, resulting in the key dimensions at the bottom of the hard mask layer pattern being uncontrollable, and even causing etching to stop. This ultimately leads to defects in 3D NAND memory and reduces the processing yield. Summary of the invention
[0006] The purpose of the present invention is to provide a plasma etching method and a plasma etching device, which sequentially perform the first to third etching processes during the etching process of an etching material layer (a hard mask layer as a base layer). The first etching process is mainly anisotropic etching, forming a second pattern whose etching depth does not reach the base layer. The second etching process is mainly isotropic etching, completely etches the etching material layer, and generates a third pattern whose bottom critical dimension reaches a preset critical dimension. The third etching process modifies the sidewall morphology of the third etching pattern, generates a fourth pattern whose upper and lower contours are consistent and whose bottom critical dimension reaches a preset critical dimension, and provides a hard mask pattern with good etching morphology for the base layer. The present invention solves the problem that the key dimension of the bottom of the pattern cannot reach the preset critical dimension and the bottom morphology of the pattern is difficult to control during the high aspect ratio etching of the etching material layer, and ensures the etching quality and etching speed. The present invention ensures that the second etching process can completely etch the etching material layer by precisely controlling the etching depth of the first etching process, and after the third etching process is completed, the base layer has a smaller etching depth, which greatly reduces the impact on the next etching process (mainly etching the base layer).
[0007] In order to achieve the above object, the present invention provides a plasma etching method, which is performed in a plasma processing chamber and comprises the following steps:
[0008] Providing a device to be etched, the device to be etched comprising a base layer, an etching material layer and a mask layer sequentially located on the base layer, the mask layer having a first pattern, the first pattern exposing a region to be etched of the etching material layer;
[0009] Applying a first low-frequency bias radio frequency signal to the processing chamber to perform a first etching process, forming a second pattern in the etching material layer, wherein the etching depth of the second pattern is 70% to 98% of the thickness of the etching material layer;
[0010] Applying a high-frequency bias radio frequency signal to the processing chamber to perform a second etching process to form a third pattern; the etching depth of the third pattern is greater than or equal to the thickness of the etching material layer; the critical dimension of the bottom of the third pattern reaches a preset critical dimension;
[0011] A second low-frequency bias RF signal is applied to the processing chamber to perform a third etching process to form a fourth pattern that penetrates the etching material layer and a portion of the thickness of the base layer, and the critical dimension of the bottom of the fourth pattern reaches a preset critical dimension.
[0012] Optionally, the frequencies of the first low-frequency bias RF signal and the second low-frequency bias RF signal are 10 kHz to 2 MHz, and the frequency of the high-frequency bias RF signal is 4 MHz to 15 MHz.
[0013] Optionally, the frequencies of the first low-frequency bias RF signal and the second low-frequency bias RF signal are the same or different.
[0014] Optionally, the aspect ratio of the fourth graphic is in the range of 10:1 to 150:1.
[0015] Optionally, the material of the mask layer is an intermediate phase of silicon oxide and silicon nitride (SiON).
[0016] Optionally, the material of the etching material layer includes any one or more of amorphous carbon (ACL), silicon carbide, polysilicon, and silicon nitride.
[0017] Optionally, the material of the base layer includes any one or more of silicon dioxide and silicon nitride.
[0018] Optionally, the etching depth is controlled by an etching endpoint detection method or process time.
[0019] Optionally, the first pattern includes grooves and / or holes.
[0020] Optionally, after the third etching process is completed, a fourth etching process is performed to remove the mask layer. Optionally, a first process gas is injected into the processing chamber to perform a first etching process, and the flow ratio of the sulfur-containing gas to the oxygen-containing gas in the first process gas is a first flow ratio, and the first flow ratio is less than or equal to 1:5.
[0021] Optionally, a second process gas is injected into the processing chamber to perform a second etching process, and the flow ratio of the sulfur-containing gas to the oxygen-containing gas in the second process gas is a second flow ratio, which is less than the first flow ratio; a third process gas is injected into the processing chamber to perform a third etching process, and the flow ratio of the sulfur-containing gas to the oxygen-containing gas in the third process gas is recorded as a third flow ratio, which is less than the first flow ratio.
[0022] The present invention also provides a plasma etching device for implementing the plasma etching method according to the present invention, the device comprising:
[0023] A processing chamber, wherein a base is provided inside the chamber, and the device to be etched is placed on the base;
[0024] A plurality of bias RF power supplies, used to generate a plurality of bias RF signals and apply them to the base; the plurality of bias RF signals are used to control the energy of plasma in a plurality of etching processes respectively;
[0025] The controller switches the corresponding bias radio frequency power supply to work based on the etching process.
[0026] Optionally, the multiple bias RF signals include at least one low-frequency bias RF signal and at least one high-frequency bias RF signal.
[0027] Optionally, the controller internally stores multiple process durations corresponding to the multiple etching processes and an execution order of the multiple etching processes; the controller switches the corresponding bias RF power supply to operate based on the process durations and the execution order.
[0028] Optionally, the plasma etching device further includes multiple air inlet pipelines, which can be respectively connected to multiple process gas sources, and the multiple process gas sources are respectively used to provide corresponding process gases into the processing chamber in the multiple etching processes; the controller opens the corresponding air inlet pipeline based on the etching process.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1) The plasma etching method of the present invention sequentially performs the first to third etching processes during the etching process, and low-frequency, high-frequency, and low-frequency biased RF signals are used in the first to third etching processes, respectively. The first etching process is mainly anisotropic etching, forming a second pattern whose etching depth does not reach the base layer. The second etching process is mainly isotropic etching, completely etches the etching material layer, and generates a third pattern whose bottom critical dimension reaches the preset critical dimension. The third etching process modifies the sidewall morphology of the third etching pattern, and generates a fourth pattern whose upper and lower contours are consistent and whose bottom critical dimension reaches the preset critical dimension. The present invention solves the problem that the key dimension of the bottom of the etching pattern cannot reach the preset critical dimension and the bottom morphology of the etching pattern is difficult to control during the high aspect ratio etching of the etching material layer. The obtained fourth pattern still has good verticality in the case of a high aspect ratio. The etching material layer is used as a hard mask layer of the base layer. Since the fourth pattern has a good etching morphology, it can greatly improve the etching quality of the base layer in the next process.
[0031] The present invention ensures that the second etching process can completely etch the etching material layer by precisely controlling the etching depth of the second pattern to be 70% to 98% of the thickness of the etching material layer. When the bottom size of the third pattern reaches the preset critical size, the etching depth of the third pattern just reaches the upper surface of the base layer or penetrates the smaller thickness of the base layer, and the side wall of the third pattern has a smaller irregularity, thereby reducing the difficulty of modifying the third pattern in the third etching process. After the third etching process is completed, the base layer has a smaller etching depth, reducing the impact on the next process (with the base layer as the main etching target layer).
[0032] 2) The plasma etching device of the present invention can switch the corresponding bias RF signal and the corresponding process gas based on the etching process in the processing chamber, and can accurately control the duration and execution order of each etching process, thereby ensuring the etching effect of the device to be etched and significantly improving the device performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solution of the present invention, the following briefly introduces the drawings required for the description. Obviously, the drawings described below are an embodiment of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work:
[0034] Figure 1 is a schematic diagram of a plasma etching device;
[0035] Figure 2 This is a flow chart of a plasma etching method in Embodiment 1 of the present invention;
[0036] Figure 3 This is a schematic diagram of a device to be etched before etching in Embodiment 1 of the present invention;
[0037] Figure 4 This is a schematic diagram of a device to be etched after the first etching process is completed in Embodiment 1 of the present invention;
[0038] Figure 5 is a schematic diagram of a device to be etched after the second etching process is completed in Embodiment 1 of the present invention;
[0039] Figure 6 is a schematic diagram of a device to be etched after the third etching process is completed in Embodiment 1 of the present invention;
[0040] Figure 7 is a schematic diagram of a device to be etched after the fourth etching process is completed in Embodiment 1 of the present invention;
[0041] Figure 8 Schematic diagram of a plasma etching device of the present invention. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] It should be understood that when used in this specification and the appended claims, the term "comprising" indicates the presence of described features, integers, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof.
[0044] It should also be understood that the terms used in this application specification are only for the purpose of describing specific embodiments and are not intended to limit the application. As used in this application specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0045] It should be further understood that the term “and / or” used in the specification and appended claims refers to any combination and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0046] As used in this specification and the appended claims, the term "if" may be interpreted as "when" or "upon" or "in response to determining" or "in response to detecting," depending on the context. Similarly, the phrases "if it is determined" or "if [described condition or event] is detected" may be interpreted as meaning "upon determination" or "in response to determining" or "upon detection of [described condition or event]" or "in response to detecting [described condition or event]," depending on the context.
[0047] In addition, in the description of the present application, the terms "first", "second", "third", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.
[0048] Figure 1 Schematic diagram of an inductively coupled plasma processing device 1 . The inductively coupled plasma processing device 1 comprises: a processing chamber 10 , a liner 102 , an insulating window 108 , an inductively coupled coil 112 and a base 105 .
[0049] The processing chamber 10 includes a processing chamber side wall 101 which is roughly cylindrical, and an opening 109 is provided on the processing chamber side wall 101 for accommodating the device W to be etched to enter and exit. The liner 102 is arranged inside the processing chamber 10 to protect the inner wall of the processing chamber 10 from being corroded by plasma. An insulating window 108 is arranged at the top of the processing chamber, and a process gas injection port 103 is provided at one end of the processing chamber side wall 101 close to the insulating window 108. The base 105 is located at the bottom of the processing chamber 10 and is used to carry the device W to be etched.
[0050] The inductive coupling coil 112 is located outside the processing chamber 10 (above the insulating window 108), and the RF power of the RF power supply 116 drives the inductive coupling coil 112 to generate a strong high-frequency alternating magnetic field, which generates a vortex electric field in the processing chamber 10. This electric field accelerates a small amount of electrons existing in the processing chamber 10, causing them to collide with gas molecules of the input process gas. These collisions lead to ionization of the process gas and excitation of plasma, thereby generating plasma in the processing chamber 10. The plasma contains a large number of active particles such as electrons, cations, excited atoms, molecules, and electrically neutral free radicals, which can undergo a variety of physical and chemical reactions with the surface of the device to be etched W, so that the morphology of the surface of the device to be etched changes, that is, the etching process is completed.
[0051] The etching process mainly utilizes cations and free radicals in the plasma, wherein the cations are charged and can move in a specific direction under the action of the electric field, and are anisotropic (suitable for etching in a certain direction), and the free radicals are uncharged and can diffuse in all directions, and are isotropic (suitable for etching in all directions). The bias RF signal applied to the base 105 by the bias RF power supply 107 accelerates the cations to move downward and bombard the area to be etched of the device W to be etched, thereby weakening the binding force between the molecules in the area to be etched. The area to be etched with weakened molecular binding force is captured by free radicals, converted into volatile gas compounds and released, thereby forming an etching pattern in the area to be etched.
[0052] Compared with high-frequency biased RF signals, low-frequency biased RF signals are more conducive to enhancing the bombardment energy and directionality of cations, making it easier for cations to reach the bottom of the etched pattern. Therefore, in high aspect ratio etching processes, low-frequency biased RF signals are usually used to increase the etching rate of the device W to be etched. Under the bombardment of high-energy cations, compared with the molecules on the side walls of the etched pattern, the molecules on the bottom of the etched pattern (whose intermolecular binding force is weakened due to the attack of cations) are more easily captured by free radicals and converted into volatile gas compounds. Although free radicals have isotropic characteristics, anisotropic physical etching has become the mainstream of etching under low-frequency biased RF conditions.
[0053] The device W to be etched usually includes a base layer and an etching material layer located on the base layer. The process involved in the present invention is to etch the etching material layer, and the base layer is the main etching target layer of the next process. Therefore, the present invention needs to completely etch the etching material layer and etch the base layer as little as possible. When a low-frequency biased RF signal is used for the etching process, the etching rate is relatively high. In order to ensure that the etching material layer is completely etched, the etching depth inevitably reaches the base layer. The by-products produced during the plasma bombardment of the base layer are easily sputtered to the side walls of the etching material layer pattern and are difficult to remove. As a result, the lateral etching rate at the bottom of the etching material layer pattern is reduced, and the critical dimension at the bottom of the etching material layer pattern cannot reach the preset critical dimension, resulting in deformation.
[0054] With the advancement of semiconductor process nodes and the continuous reduction of feature sizes, plasma etching using only low-frequency biased RF signals can no longer meet the processing requirements for high aspect ratio etching patterns.
[0055] The present invention sequentially performs the first to third etching processes in the process of etching the etching material layer, and uses low-frequency, high-frequency, and low-frequency biased RF power supplies in the first to third etching processes, respectively. The first etching process is mainly based on physical bombardment in the longitudinal direction (the depth direction of the etching pattern), which is used to complete the main etching task, and its etching depth does not reach the base layer. The second etching process is mainly based on chemical etching in the transverse direction (the width direction of the etching pattern), which is used to completely etch the etching material layer and make the key dimension at the bottom of the etching material layer pattern reach the preset key dimension. The third etching process is still mainly based on physical bombardment in the longitudinal direction, which is used to modify the morphology of the side wall of the etching material layer pattern. The present invention can obtain high-quality, high-aspect-ratio etching patterns in the etching material layer of the device W to be etched, and has a high etching speed. In addition, the present invention can achieve complete etching of the etching material layer by accurately controlling the etching depth of the first etching process, while also making the base layer have a smaller etching depth, reducing the impact on the next process (with the base layer as the main etching target layer).
[0056] Embodiment 1
[0057] The present invention provides a plasma etching method, which is performed in a plasma processing chamber. Figure 2 As shown, it includes the following steps:
[0058] S100, providing a device W to be etched. Figure 3As shown, the device W to be etched includes a base layer 150, an etching material layer 140 and a mask layer 130 sequentially located on the base layer 150. In the present embodiment, the etching material layer 140 exists as a hard mask layer of the base layer 150, and the mask layer 130 exists as a mask layer of the etching material layer 140. Before the process involved in the present invention starts, the mask layer 130 has a first pattern 161, and the first pattern 161 exposes the area to be etched of the etching material layer 140.
[0059] In this embodiment, the material of the mask layer 130 is an intermediate phase of silicon oxide and silicon nitride (SiON). The first pattern 161 includes grooves and / or holes. The first pattern 161 can be obtained by conventional photolithography and etching, which will not be described in detail here.
[0060] In this embodiment, the material of the etching material layer 140 includes one or more of amorphous carbon (ACL), silicon carbide, polysilicon, and silicon nitride. The etching material layer 140 can be a single layer structure or a multi-layer stacked structure. The present invention does not limit the number of layers of the stacked structure.
[0061] In this embodiment, the material of the base layer 150 includes any one or more of silicon dioxide and silicon nitride. In a preferred embodiment, the base layer 150 is an overlapping layer of silicon oxide and silicon nitride.
[0062] S200, applying a first low-frequency bias RF signal to the processing chamber to perform a first etching process, forming a second pattern 162 (such as Figure 4 As shown), the etching depth of the second pattern 162 is 70% to 98% of the thickness of the etching material layer. Optionally, the etching depth of the second pattern 162 is 90% to 98% of the thickness of the etching material layer to improve the efficiency of the etching process.
[0063] In this embodiment, a first process gas is injected into the processing chamber to perform a first etching process, and the first process gas generates a corresponding first plasma under the action of a radio frequency electric field. The first process gas is mainly composed of sulfur-containing gas (such as hydroxysulfide COS) and oxygen-containing gas (such as oxygen O2). The flow ratio of the sulfur-containing gas to the oxygen-containing gas in the first process gas is recorded as the first flow ratio, and the first flow ratio in this embodiment is less than or equal to 1:5. Experiments have shown that the first flow ratio is conducive to the ionization of sulfur-containing gas and can produce more cations. In this embodiment, the frequency of the first low-frequency biased radio frequency signal is 10kHz~2MHz, which can provide greater energy for the cations in the first plasma, so the first etching process is mainly anisotropic physical etching.
[0064] As the etching depth increases, the energy and quantity of the cations reaching the bottom of the second pattern gradually decrease, resulting in a weakening of the cation bombardment force and a deterioration of the collimation of the cation bombardment. Figure 4 As shown, the sidewall of the bottom of the second pattern is inwardly tapered. The critical dimension of the bottom of the second pattern does not reach the preset critical dimension.
[0065] In this embodiment, the etching depth can be controlled by an etching endpoint detection method or a process time. By accurately controlling the etching depth of the first etching process to be 70% to 98% of the thickness of the etching material layer, on the one hand, it is possible to avoid the byproducts generated by the cationic bombardment of the base layer 150 from being sputtered on the sidewalls of the second pattern 162 and causing adverse effects on the critical dimensions at the bottom of the second pattern. On the other hand, a suitable unetched thickness (2% to 30% of the thickness of the etching material layer) can be reserved in the etching material layer 140 for the subsequent etching process, so as to realize the formation of a high-quality, high-aspect-ratio etching pattern on the device W to be etched through the subsequent etching process, and the etching depth of the base layer 150 will not exceed a preset depth threshold (described in detail later).
[0066] S300, applying a high frequency bias RF signal to the processing chamber to perform a second etching process to form a third pattern 163. Figure 5 As shown, the etching depth of the third graphic 163 is greater than or equal to the thickness of the etching material layer 140. In the second etching process, the bottom of the third graphic is laterally etched so that the critical dimension of the bottom of the third graphic reaches a preset critical dimension.
[0067] In this embodiment, a second process gas is injected into the processing chamber to perform a second etching process, and the second process gas generates a corresponding second plasma under the action of the radio frequency electric field. The second process gas is mainly composed of sulfur-containing gas (such as hydroxysulfide COS) and oxygen-containing gas (such as oxygen O2). The flow ratio of the sulfur-containing gas to the oxygen-containing gas in the second process gas is recorded as the second flow ratio, which is less than the first flow ratio. The second flow ratio in this embodiment is 1:10, which is only used as an example and is not a limitation of the present invention.
[0068] In this embodiment, the frequency of the high frequency bias radio frequency signal is 4 MHz to 15 MHz. Since the bombardment force of the cations in the second plasma is relatively low, the second etching process is mainly isotropic chemical etching.
[0069] Under the bombardment of cations, the binding force between the molecules of the bombarded layer is reduced, and the molecular bonds are opened. Under the collision of electrons in the RF electric field, oxygen dissociates to obtain oxygen free radicals o (o2+e→o+o+e, e represents electrons). The volume of oxygen in the second process gas is increased, and more oxygen free radicals o can be dissociated, thereby increasing the probability of oxygen free radicals combining with the molecules whose molecular bonds are opened, thereby increasing the speed of chemical etching.
[0070] In the second etching process, since the bombardment energy of the cations is small, the etching depth of the etching material layer 140 is limited. The present invention precisely controls the etching depth of the first etching process so that in the second etching process, the etching depth of the etching material layer 140 does not exceed 30% of the thickness of the etching material layer, thereby ensuring that the etching material layer 140 is completely etched.
[0071] When the etching depth of the first etching process is 70% to 98% of the thickness of the etching material layer, it can ensure that the bottom size of the third pattern 163 reaches the preset critical size, and the etching depth of the third pattern 163 just reaches the upper surface of the base layer or penetrates the smaller thickness of the base layer 150, preventing the base layer 150 from being etched too deeply and reducing the reaction byproducts generated by bombarding the base layer 150. In addition, the side wall of the third pattern 163 has a small irregularity, which can reduce the difficulty of modifying the side wall of the third pattern in the later stage.
[0072] S400, applying a second low-frequency bias RF signal to the processing chamber to perform a third etching process, forming a fourth pattern 164 that penetrates the etching material layer 140 and a portion of the thickness of the base layer 150, and the fourth pattern 164 has a depth-to-width ratio ranging from 10:1 to 150:1. Figure 6 As shown, the critical dimension of the bottom of the fourth graphic reaches the preset critical dimension, and the sidewall of the fourth graphic has good verticality.
[0073] In this embodiment, a third process gas is injected into the processing chamber to perform a third etching process, and the third process gas generates a corresponding third plasma under the action of the radio frequency electric field. The third process gas is mainly composed of sulfur-containing gas (such as hydroxysulfide COS) and oxygen-containing gas (such as oxygen O2). The flow ratio of the sulfur-containing gas to the oxygen-containing gas in the third process gas is recorded as a third flow ratio, which is less than the first flow ratio.
[0074] The frequency of the second low-frequency bias RF signal is 10kHz to 2MHz, and the frequencies of the first low-frequency bias RF signal and the second low-frequency bias RF signal can be the same or different. The third etching process is still mainly anisotropic physical etching, which is mainly used to modify the side wall of 163 after the second etching process. Compared with the first process gas, the sulfur-containing gas in the third process gas is reduced, and the number of cations in the third plasma is less than the number of cations in the first plasma. The reduction in the number of cations can reduce the reaction byproducts generated by bombarding the base layer 150. Since the side wall of the third figure 163 has a small irregularity, the modification of the side wall of the third figure is low. Even if the number of cations in the third plasma is reduced, it is sufficient to generate a fourth figure 164 with a good side wall morphology. And because the modification of the side wall of the third figure is low, after the third etching process is completed, the etching depth of the base layer 150 is small (less than the preset depth threshold), which reduces the impact on the next process (mainly etching the base layer).
[0075] S500 , performing a fourth etching process to remove the mask layer 130 .
[0076] A fourth process gas is injected into the processing chamber to perform a fourth etching process. The fourth process gas generates a corresponding fourth plasma under the action of the radio frequency electric field. The mask layer 130 is etched and removed by the fourth plasma. Figure 7 The device W to be etched is shown as completing high aspect ratio etching of the etching material layer 140 of the device W to be etched.
[0077] The fourth process gas in this embodiment is a mixed gas of oxygen and fluorine-containing gas, which is used to remove the SiON-based mask layer 130 , which will not be described in detail here.
[0078] like Figure 8 As shown, the present invention further provides a plasma etching device 2 for implementing the plasma etching method of the present invention.
[0079] The plasma etching device 2 includes: a processing chamber 20 , a plurality of bias RF power supplies 207 , a controller 230 and a plurality of gas inlet pipes 220 .
[0080] A susceptor 205 is provided inside the processing chamber 20 , and the device W to be etched is placed on the susceptor 205 .
[0081] The multiple bias RF power supplies 207 are used to generate multiple bias RF signals and apply them to the base 205. The multiple bias RF signals are used to control the energy of plasma in multiple etching processes. In the present invention, the multiple bias RF power supplies include at least one low-frequency bias RF power supply 207a and one high-frequency bias RF power supply 207b.
[0082] The controller 230 stores a plurality of process durations corresponding to the plurality of etching processes and the execution order of the plurality of etching processes. The controller 230 switches the corresponding bias RF power supply 270 to operate based on the process duration and execution order of the etching process.
[0083] The multiple air inlet pipelines 220 are connected to the multiple process gas sources 204 through the multiple flow regulating valves 221. The multiple process gas sources 204 are respectively used to provide corresponding process gases to the processing chamber 20 in multiple etching processes. The controller 230 opens the corresponding air inlet pipeline 220 and adjusts the valve opening of the corresponding flow regulating valve 221 based on the etching process.
[0084] It should be understood that the size of the serial numbers of the steps in the above embodiments does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0085] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed by the present invention, and these modifications or replacements should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A plasma etching method, the method being performed in a plasma processing chamber, characterized in that: The following steps are included: Providing a device to be etched, the device to be etched comprising a base layer, an etching material layer and a mask layer sequentially located on the base layer, the mask layer having a first pattern, the first pattern exposing a region to be etched of the etching material layer; Applying a first low-frequency bias radio frequency signal to the processing chamber to perform a first etching process, forming a second pattern in the etching material layer, wherein the etching depth of the second pattern is 70% to 98% of the thickness of the etching material layer; Applying a high-frequency bias radio frequency signal to the processing chamber to perform a second etching process to form a third pattern with an etching depth greater than or equal to the thickness of the etching material layer; The critical dimension at the bottom of the third figure reaches the preset critical dimension; A second low-frequency bias RF signal is applied to the processing chamber to perform a third etching process to form a fourth pattern that penetrates the etching material layer and a portion of the thickness of the base layer, and the critical dimension of the bottom of the fourth pattern reaches a preset critical dimension.
2. The plasma etching method according to claim 1, characterized in that: The frequencies of the first low-frequency biased RF signal and the second low-frequency biased RF signal are 10 kHz to 2 MHz, and the frequency of the high-frequency biased RF signal is 4 MHz to 15 MHz.
3. The plasma etching method according to claim 1, characterized in that: The frequencies of the first low-frequency biased RF signal and the second low-frequency biased RF signal are the same or different.
4. The plasma etching method according to claim 1, characterized in that: The fourth graphic has a depth-to-width ratio ranging from 10:1 to 150:
1.
5. The plasma etching method according to claim 1, characterized in that: The material of the mask layer is an intermediate phase of silicon oxide and silicon nitride.
6. The plasma etching method according to claim 1, characterized in that: The material of the etching material layer includes any one or more of amorphous carbon, silicon carbide, polysilicon, and silicon nitride.
7. The plasma etching method according to claim 1, characterized in that: The material of the base layer includes any one or more of silicon dioxide and silicon nitride.
8. The plasma etching method according to claim 1, characterized in that: The etching depth is controlled by an etching endpoint detection method or process time.
9. The plasma etching method according to claim 1, characterized in that: The first pattern includes grooves and / or holes.
10. The plasma etching method according to claim 1, wherein: After the third etching process is completed, a fourth etching process is performed to remove the mask layer.
11. The plasma etching method according to claim 1, characterized in that: A first process gas is injected into the processing chamber to perform a first etching process, wherein a flow ratio of the sulfur-containing gas to the oxygen-containing gas in the first process gas is a first flow ratio, and the first flow ratio is less than or equal to 1:
5.
12. The plasma etching method according to claim 11, characterized in that: Injecting a second process gas into the processing chamber to perform a second etching process, wherein a flow ratio of the sulfur-containing gas to the oxygen-containing gas in the second process gas is a second flow ratio, which is less than the first flow ratio; A third process gas is injected into the processing chamber to perform a third etching process, and a flow ratio of the sulfur-containing gas to the oxygen-containing gas in the third process gas is recorded as a third flow ratio, which is smaller than the first flow ratio.
13. A plasma etching device, used to implement the plasma etching method according to any one of claims 1 to 12, characterized in that: Include: A processing chamber, wherein a base is provided inside the chamber, and the device to be etched is placed on the base; A plurality of bias radio frequency power supplies, used for generating a plurality of bias radio frequency signals and applying the signals to the base; The plurality of bias RF signals are respectively used to control the energy of plasma in a plurality of etching processes; The controller switches the corresponding bias radio frequency power supply to work based on the etching process.
14. The plasma etching device according to claim 13, characterized in that: The plurality of bias RF signals include at least one low-frequency bias RF signal and at least one high-frequency bias RF signal.
15. The plasma etching device according to claim 13, characterized in that: The controller internally stores a plurality of process durations corresponding to the plurality of etching processes and an execution order of the plurality of etching processes; The controller switches the corresponding bias RF power supply to operate based on the process duration and the execution sequence.
16. The plasma etching device according to claim 13, characterized in that: It also includes a plurality of gas inlet pipelines, which can be respectively connected to a plurality of process gas sources, and the plurality of process gas sources are respectively used to provide corresponding process gases into the processing chamber in the plurality of etching processes; The controller opens the corresponding intake pipe based on the etching process.
Citation Information
Cited By
Semiconductor processing equipment and direct current voltage signal control system thereof
CN119182310A
Semiconductor processing equipment and DC voltage signal control system thereof
CN119182310B