A method for manufacturing an infrared LED chip and an infrared LED chip thereof
By using metal organic chemical vapor deposition, photolithography, solid wax bonding and mathematical model optimization electroplating technology in infrared LED chip manufacturing, the problems of low luminescence efficiency, low bond yield and poor reliability are solved, and more efficient Optical and electrical properties and more reliable chip production.
Patent Information
- Application Number
- CN202411252860.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-09
AI Technical Summary
The existing infrared LED chip manufacturing technology faces the problems of low luminous efficiency, low yield on wafer bonding and poor reliability, mainly due to total internal reflection phenomenon, unevenness of electroplating copper layer and poor material interface compatibility.
The structure is grown by metal organic chemical vapor deposition method, fancy roughened patterns are produced through photolithography, the ITO film thickness and electroplating parameters are optimized, combined with the temporary bonding technology of solid wax, precisely control the etching conditions, and establish a mathematical model to optimize the electroplating process , choose high-compatibility materials to ensure uniformity of the electroplating layer and bonding quality.
It significantly improves luminous efficiency, bond yield and reliability, enhances the optical and electrical properties of ITO films, and ensures long-term stability and yield.
Smart Images

Figure CN118763159B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chips, and in particular, relates to a method for manufacturing an infrared LED chip and the infrared LED chip. Background Art
[0002] Infrared LED chips are widely used in many fields, such as security monitoring, biometrics, etc. However, the existing infrared LED chip manufacturing technology faces some challenges, mainly including:
[0003] Low luminous efficiency: Due to the total internal reflection phenomenon inside the chip, the light cannot be emitted effectively, reducing the luminous efficiency.
[0004] Low wafer bonding yield: This is mainly caused by problems such as the unevenness of the electroplated copper layer and poor bonding between the transition substrate and the epitaxial wafer.
[0005] Poor reliability: This may be caused by poor interface compatibility between materials or insufficient long-term stability.
[0006] Existing technical problems:
[0007] Electroplating technical requirements: The copper electroplating process requires strict control of solution composition, temperature, current and other factors, otherwise it will directly affect product quality.
[0008] Temporary bonding technology: The choice of solid wax and the bonding of the transition substrate may affect the overall performance and yield of the chip.
[0009] ITO film optimization: Further research is needed to optimize the thickness and conductivity of ITO films to achieve optimal optical and electrical properties. Summary of the invention
[0010] The purpose of the present invention is to provide a method for manufacturing an infrared LED chip, and at the same time to provide an infrared LED chip. To achieve the above purpose, the present invention adopts the following technical solutions:
[0011] A method for manufacturing an infrared LED chip, comprising the steps of:
[0012] Using metal organic chemical vapor deposition method, each layer structure is grown sequentially on a GaAs temporary substrate;
[0013] A fancy roughening pattern is produced on the ohmic contact layer by using a photolithography process, and a mixed solution of iodic acid, sulfuric acid, hydrofluoric acid and water is used for room temperature roughening to form a P-GaP optical window layer;
[0014] Use dry ICP etching or wet etching to obtain the conductive hole pattern, ensuring that the etching depth is ≥ the thickness of the ohmic contact layer;
[0015] ITO thin film deposition:
[0016] An ITO film is deposited on the entire surface of the P-GaP optical window layer and the conductive hole. The thickness is adjusted according to the wavelength of the chip. The calculation formula is d=m(1 / 4nλ), where d is the target thickness of the ITO film, m is an odd number and the adjustment coefficient is an odd number, λ is the wavelength of the chip, and n is the refractive index of the ITO film.
[0017] Photolithography of the P-electrode pad pattern is performed on the conductive hole, and a Cr-Pt-Au composite structure is deposited by electron beam evaporation;
[0018] The wafer is photolithographically masked to form a cutting path pattern, and an ICP etching process is performed to form isolation of the P-side die;
[0019] A layer of solid wax is evenly coated on the transition substrate, and the transition substrate is bonded to the P surface of the epitaxial wafer through the solid wax for temporary bonding;
[0020] On the surface of the ohmic layer, an N electrode metal is deposited by electron beam evaporation to form an N electrode;
[0021] Electroplating a layer of metal Cu on the N electrode as a supporting substrate with a thickness of 50-150 μm;
[0022] The transition substrate is removed by heating and dissolving the solid wax for separation;
[0023] The residual solid wax on the surface is removed by soaking in wax removal liquid, and then the transition substrate is peeled off by rinsing with deionized water and cleaning with acetone and ethanol;
[0024] After the wafer is cut, tested, sorted and inspected, infrared LED chips are obtained.
[0025] Furthermore, the thickness d of the ITO film corresponding to different m values is calculated according to the specific wavelength λ and the refractive index n of the ITO film, and the optical properties at these different thicknesses are experimentally tested to find the optimal thickness of the ITO film.
[0026] Furthermore, the Cr-Pt-Au composite structure is deposited by electron beam evaporation. Specifically, the thickness of the first Cr layer is 20-150 nm, the thickness of the second Pt layer is 30-100 nm, and the thickness of the third Au layer is 2000-4000 nm, and a rapid annealing treatment is performed.
[0027] Furthermore, the solid wax is specifically: a solid wax having a melting point higher than 100°C.
[0028] Furthermore, in the process of electroplating a layer of metal Cu on the N electrode as a supporting substrate, a mathematical model of the electroplating process is established to simulate the influence of different electroplating conditions on the quality of the electroplated layer and find the optimal combination of electroplating parameters.
[0029] Furthermore, a mathematical model of the electroplating process is established to simulate the effects of different electroplating conditions on the quality of the electroplated layer and find the optimal combination of electroplating parameters. Specifically:
[0030] 1. Construction of mathematical model:
[0031] Define variables:
[0032] C: solution composition;
[0033] Te: electroplating temperature;
[0034] I: current intensity;
[0035] V: voltage;
[0036] D: thickness of electroplating layer;
[0037] U: uniformity of electroplating layer;
[0038] Q: The quality of the electroplating layer;
[0039] Mathematical model:
[0040] The thickness of the electroplated layer is calculated by Faraday's law: D = k*I*t / A, where k is a constant, t is the electroplating time, and A is the electroplating area;
[0041] The uniformity U of the electroplated layer is expressed using an empirical model of the following form: , where β0, β1, β2, β3, β4 are model coefficients, is the error term;
[0042] The quality Q of the electroplated layer is: Q=α1D+α2U, where α1 and α2 are weight coefficients;
[0043] 2. Optimization goals:
[0044] Maximize the quality Q of the electroplated layer;
[0045] 3. Constraints:
[0046] Solution composition: copper sulfate concentration C∈[150,250]g / L;
[0047] Electroplating temperature: Te = 25 °C;
[0048] Current intensity: I∈[0.1,0.4]A;
[0049] Voltage: V∈[3,6]V;
[0050] Electroplating time: Determined according to thickness requirements;
[0051] Electroplating layer thickness: D∈[50,150]μm;
[0052] 4. Solution method: Use gradient descent or genetic algorithm to solve the optimal combination of electroplating parameters.
[0053] An infrared LED chip is manufactured by the above-mentioned method for manufacturing an infrared LED chip.
[0054] The beneficial effects of the present invention are as follows:
[0055] Improve luminous efficiency: The P-GaP ohmic contact layer is roughened by photolithography, combined with room-temperature roughening using a mixed solution of iodic acid, sulfuric acid, hydrofluoric acid, and water, which effectively reduces total internal reflection and significantly improves luminous efficiency.
[0056] Optimizing ITO film thickness: By precisely controlling ITO film deposition parameters (such as temperature and pressure) and calculating the optimal thickness of the ITO film based on the chip's operating wavelength and the refractive index of the ITO film, the optical properties of the ITO film are improved, thereby enhancing the electrical properties of the chip.
[0057] Improve the quality of the electroplating layer: Numerical optimization algorithms (such as gradient descent, genetic algorithm, etc.) are used to accurately find the optimal parameter combination in the electroplating process, thereby ensuring the uniformity and quality of the electroplating layer and effectively improving the bonding yield.
[0058] Enhanced material compatibility: Through experimental verification of interface compatibility between materials, a material combination with good compatibility is selected to ensure the long-term stability and performance of the device.
[0059] Improve etching quality: Through precise control of etching conditions (such as gas ratio, chamber pressure, power, temperature, etc.), good etching quality and uniformity are ensured, thereby improving bonding yield and reliability.
[0060] Improved temporary bonding technology: Solid wax with a melting point above 100°C was selected as the temporary bonding material, and the bonding process was optimized to ensure good bonding between the transition substrate and the epitaxial wafer, thereby improving the yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 The figure is a flow chart of the method of the present invention. DETAILED DESCRIPTION
[0062] Next, in combination with the embodiments of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative efforts shall fall within the protection scope of the present invention.
[0063] This application discloses a manufacturing method of an infrared LED chip, as Figure 1 , the method includes the steps:
[0064] Epitaxial growth:
[0065] Using metalorganic chemical vapor deposition (MOCVD) method, grow each layer structure on the GaAs temporary substrate in sequence, including:
[0066] GaInP cutoff layer;
[0067] N-AlGaAs ohmic layer (AlxGa(1-x)As, where 0.1 < X < 0.4, thickness is 1.5 - 3 μm);
[0068] N-AlGaAs current spreading layer;
[0069] N-AlGaAs confinement layer;
[0070] MQW light-emitting layer;
[0071] P-AlGaAs confinement layer;
[0072] P-AlGaAs current spreading layer;
[0073] P-GaP spreading layer;
[0074] P-GaP ohmic contact layer;
[0075] Optimize the MOCVD growth conditions to ensure the quality and consistency of the epitaxial layer.
[0076] Coarsening of the light-emitting area:
[0077] Use photolithography process to make a fancy coarsening pattern on the P-GaP ohmic contact layer, and use a mixed solution of iodic acid, sulfuric acid, hydrofluoric acid and water for room-temperature coarsening to form a P-GaP light window layer, reduce the total internal reflection phenomenon, and improve the light-emitting efficiency.
[0078] Fabrication of conductive holes:
[0079] Obtain the conductive hole pattern by using dry ICP etching or wet etching (using a mixed solution of HBr and H2O, HBr concentration is 4% - 8% (v / v%)), and ensure that the etching depth ≥ the thickness of the P-GaP ohmic contact layer.
[0080] ITO thin film deposition:
[0081] An ITO film is deposited on the entire surface of the P-GaP optical window layer and the conductive holes. Its thickness is adjusted according to the wavelength of the chip. The calculation formula is d=m(1 / 4nλ), where d is the target thickness of the ITO film, m is the adjustment coefficient and is an odd number, λ is the wavelength of the chip, and n is the refractive index of the ITO film.
[0082] Furthermore, the thickness d of the ITO film corresponding to different m values is calculated according to the specific wavelength λ and the refractive index n of the ITO film, and the optical properties (such as transmittance and reflectivity) at these different thicknesses are tested experimentally. That is, for a given wavelength and refractive index, the optimal thickness is found by changing the value of m.
[0083] The thickness and conductivity of the ITO film are optimized by precisely controlling deposition parameters (such as temperature and pressure) to achieve the best optical and electrical properties.
[0084] P electrode production:
[0085] The P electrode pad pattern is photoetched on the conductive hole, and the Cr-Pt-Au composite structure is evaporated by electron beam evaporation. The thickness of the first Cr layer is 20-150nm, the thickness of the second Pt layer is 30-100nm, and the thickness of the third Au layer is 2000-4000nm, and rapid annealing is performed.
[0086] Optimize annealing temperature and time to ensure good contact resistance and soldering performance.
[0087] P-side die isolation:
[0088] The wafer is photolithographically masked to form a cutting path pattern, and an ICP etching process is performed to isolate the P-side die.
[0089] Temporary Bonding:
[0090] A layer of solid wax is evenly coated on the transition substrate, and the transition substrate is bonded to the P surface of the epitaxial wafer through the solid wax for temporary bonding.
[0091] Select solid wax with a melting point above 100°C, acid and alkali resistance, easy to remove, and high adhesion, and ensure that the transition substrate has the characteristics of high temperature resistance, acid and alkali resistance, and strong hardness.
[0092] By precisely controlling the heating temperature, pressure and time of the waxing machine, good bonding between the transition substrate and the epitaxial wafer is ensured.
[0093] Support substrate preparation:
[0094] On the surface of the N-AlGaAs ohmic layer, an N-electrode metal is deposited by electron beam evaporation to form an N-electrode.
[0095] A layer of metal Cu is electroplated on the N electrode as a supporting substrate with a thickness of 50-150 μm.
[0096] By establishing a mathematical model of the electroplating process, the effects of different electroplating conditions (such as solution composition, temperature, current, and voltage) on the quality of the electroplated layer can be simulated. The optimal combination of electroplating parameters can be found to ensure the uniformity and quality of the electroplated layer.
[0097] 1. Construction of mathematical model
[0098] Define variables:
[0099] C: Solution composition (copper sulfate concentration, unit: g / L)
[0100] Te: electroplating temperature (unit: °C)
[0101] I: current intensity (unit: A)
[0102] V: voltage (unit: V)
[0103] D: Thickness of electroplating layer (unit: μm)
[0104] U: Uniformity of electroplating layer (value range: 0~1, 1 means the most uniform)
[0105] Q: Quality of the electroplated layer (considering uniformity and thickness)
[0106] Mathematical model:
[0107] The thickness of the electroplated layer is calculated using Faraday's law: D=k*I*t / A, where k is a constant, t is the electroplating time (unit: s), and A is the electroplating area (unit: cm²).
[0108] The uniformity of the electroplated layer is affected by many factors, including current distribution, solution composition, temperature, etc. It is represented by an empirical model in the following form: , where βi (β0-β4) is the model coefficient, is the error term.
[0109] The quality of the electroplating layer takes into account thickness and uniformity: Q=α1D+α2U, where α1 and α2 are weight coefficients.
[0110] 2. Optimization goals
[0111] Maximize the quality Q of the electroplated layer.
[0112] 3. Constraints
[0113] Solution composition: copper sulfate concentration C∈[150,250]g / L;
[0114] Electroplating temperature: Te = 25 °C;
[0115] Current intensity: I∈[0.1,0.4]A;
[0116] Voltage: V∈[3,6]V;
[0117] Electroplating time: Determined according to thickness requirements;
[0118] Electroplating layer thickness: D∈[50,150]μm;
[0119] 4. Solution method:
[0120] Numerical optimization: Use numerical optimization algorithms (such as gradient descent, genetic algorithm, etc.) to solve the optimal combination of electroplating parameters.
[0121] Solution
[0122] Gradient Descent Algorithm:
[0123] Initialization: Randomly select a set of initial parameter values.
[0124] Objective function: Calculate the quality Q of the electroplating layer based on the mathematical model.
[0125] Gradient calculation: Use numerical methods (such as finite difference method) to calculate the gradient of the objective function with respect to each parameter.
[0126] Iterative update: Update the parameter value in the direction of the gradient until the stopping condition is met (such as the gradient approaches zero or the maximum number of iterations is reached).
[0127] Genetic Algorithm:
[0128] Initialization: Randomly generate an initial population containing multiple individuals (parameter groups).
[0129] Fitness evaluation: Calculate the fitness value of each individual (i.e., the quality Q of the electroplating layer).
[0130] Selection operation: select individuals with high fitness to enter the next generation.
[0131] Crossover operation: Generate new individuals by randomly exchanging part of the genes of two individuals.
[0132] Mutation operation: randomly modify a gene of an individual with a certain probability.
[0133] Iterative update: Repeat the selection, crossover and mutation operations until the stopping condition is met (such as reaching the maximum number of iterations or the fitness value no longer improves significantly).
[0134] Gradient descent algorithm code:
[0135] Python
[0136] def objective_function(C,Te,I,V):
[0137] # Calculate the quality Q of the electroplating layer
[0138] D = k * I * t / A # Plating thickness
[0139] U = beta0 + beta1 * C + beta2 * Te + beta3 * I + beta4 * V # Electroplating uniformity
[0140] Q = alpha1 * D + alpha2 * U # Electroplating quality
[0141] return Q
[0142] def gradient_descent(C, Te, I, V, learning_rate, max_iterations):
[0143] for i in range(max_iterations):
[0144] # Calculate gradients
[0145] grad_C = ...
[0146] grad_Te = ...
[0147] grad_I = ...
[0148] grad_V = ...
[0149] # Update parameters
[0150] C -= learning_rate * grad_C
[0151] Te -= learning_rate * grad_Te
[0152] I -= learning_rate * grad_I
[0153] V -= learning_rate * grad_V
[0154] # Check stop condition
[0155] if abs(grad_C) < tol and abs(grad_Te) < tol and abs(grad_I) <tol and abs(grad_V) < tol:
[0156] break
[0157] return C, Te, I, V;
[0158] Genetic algorithm code:
[0159] Python
[0160] def genetic_algorithm(population_size, num_generations):
[0161] # Initialize the population
[0162] population = initialize_population(population_size)
[0163] for gen in range(num_generations):
[0164] # Fitness evaluation
[0165] fitness_values = evaluate_fitness(population)
[0166] # Select Operation
[0167] selected_population = selection(population, fitness_values)
[0168] # Crossover Operation
[0169] offspring = crossover(selected_population)
[0170] # Mutation Operation
[0171] mutated_offspring = mutation(offspring)
[0172] # Update population
[0173] population = mutated_offspring
[0174] # Return the best individual
[0175] best_individual = select_best_individual(population)
[0176] return best_individual;
[0177] By constructing a mathematical model, we can systematically explore the impact of electroplating conditions on the quality of the electroplated layer and find the optimal combination of electroplating parameters to ensure the uniformity and quality of the electroplated layer and improve the overall bonding yield and reliability;
[0178] Transition substrate peeling:
[0179] The transition substrate is removed by heating and dissolving the solid wax.
[0180] The residual solid wax on the surface is removed by immersing in a wax removal solution, and then the transition substrate is peeled off by rinsing with deionized water and cleaning with acetone and ethanol.
[0181] Final treatment:
[0182] After the wafer is cut, tested, sorted and inspected, infrared LED chips are obtained.
[0183] Cutting:
[0184] Equipment selection: Use a laser scriber for cutting to ensure smooth cutting edges and reduce cracks.
[0185] Cutting Program: Program precise cutting paths to ensure consistent chip size and no damage.
[0186] Cooling method: Use coolant during the cutting process to prevent the chip from being damaged by thermal stress.
[0187] test:
[0188] Electrical testing: Use a semiconductor parameter analyzer to perform IV curve testing on the chip to confirm that the chip's forward voltage and reverse leakage current meet the design requirements.
[0189] Optical testing: Use an integrating sphere or spectrum analyzer to measure the chip’s luminous intensity, spectral characteristics, and luminous angle.
[0190] Temperature test: Test under different temperature conditions to ensure the chip has stable performance over a wide temperature range.
[0191] Sorting:
[0192] Appearance inspection: Check whether there are defects (such as scratches, cracks, etc.) on the chip surface through a microscope or an automatic visual inspection system.
[0193] Performance grading: Chips are divided into different grades according to the test results, such as Grade A, Grade B, Grade C, etc., to facilitate subsequent packaging and sales.
[0194] test:
[0195] Reliability testing: Conduct high-temperature aging tests, thermal shock tests, etc. to verify the long-term reliability and stability of the chip.
[0196] Quality Control: In accordance with ISO 9001 and other international quality management system standards, a strict quality control system is established to ensure that each batch of chips meets the quality requirements.
[0197] Package:
[0198] Chip mounting: Use a die bonder to mount qualified chips onto the bracket, and use silver paste or gold wire for bonding.
[0199] Packaging material selection: Choose packaging materials suitable for the infrared spectrum, such as transparent epoxy resin, to ensure that light can be transmitted effectively.
[0200] Packaging process: The packaging material is covered on the chip by dispensing or molding, and a protective layer is formed after curing.
[0201] Finish:
[0202] Final inspection: Final inspection of the packaged chip, including appearance, electrical performance, and optical performance.
[0203] Packaging and shipment: Qualified infrared LED chips are packaged in anti-static packaging and shipped according to customer requirements.
[0204] In addition, the etching conditions, such as gas ratio, chamber pressure, and power, are optimized to ensure good etching quality and uniformity. Specifically, the following are included:
[0205] Gas ratio:
[0206] ICP etching: When isolating the P-side die, use ICP (inductively coupled plasma) etching method. Select Cl2 and BCl3 as the main etching gas, and the etching gas ratio is 16:1.
[0207] Wet etching: When making conductive holes, use a mixed solution of HBr and H2O for wet etching with an HBr concentration of 4%-8% (v / v%) to ensure that the etching depth reaches or exceeds the thickness of the P-GaP ohmic contact layer.
[0208] Cavity pressure:
[0209] For ICP etching, the chamber pressure was set to 3 mTorr to maintain a stable plasma state and ensure etching uniformity.
[0210] power:
[0211] The ICP power supply was set to 900W and the bias power was set to 400W.
[0212] Etching temperature:
[0213] The etching temperature is set to -10°C. Low temperature helps to improve etching selectivity and reduce the impact of thermal effects.
[0214] Etching time:
[0215] The etching time is adjusted according to the etching depth requirement to ensure that the etching depth reaches the predetermined requirement while avoiding over-etching.
[0216] Implementation details
[0217] ICP etching
[0218] Gas selection: Cl2 and BCl3 are used as the main etching gases in a ratio of 16:1.
[0219] Chamber pressure: 3mTorr.
[0220] ICP power supply power: 900W.
[0221] Bias power: 400W.
[0222] Etching temperature: -10℃.
[0223] Etching time: adjusted according to the etching depth requirements, generally several minutes to more than ten minutes.
[0224] Wet etching
[0225] Etching solution: HBr concentration is 4%-8% (v / v%), mixed with H2O.
[0226] Etching conditions: Adjust the etching time according to the etching depth requirements, generally a few minutes to tens of minutes.
[0227] Gas ratio: By optimizing the ratio of Cl2 and BCl3, the etching rate and selectivity are adjusted to ensure the etching quality.
[0228] Chamber pressure: Lower chamber pressure helps to form a stable plasma, thereby improving etching uniformity.
[0229] Power: The selection of ICP power supply power and bias power balances the etching rate and etching quality.
[0230] Etching temperature: Low temperature helps reduce thermal damage and improve etching selectivity.
[0231] Etching time: Precisely control the etching time according to the required etching depth to avoid over-etching or under-etching.
[0232] The above optimization measures can ensure the consistency and repeatability of the etching process, thereby improving the bonding yield and reliability. In addition, these parameters can be further fine-tuned through experiments to adapt to different process requirements and material properties.
[0233] The present invention proposes a method for manufacturing an infrared LED chip, aiming to solve the problems of low luminous efficiency, low bonding yield and poor reliability in the prior art. Through a series of optimization measures, the present invention achieves higher luminous efficiency, better bonding yield and more reliable performance.
[0234] Improve luminous efficiency: The fancy roughening treatment of the P-GaP ohmic contact layer made by photolithography process, combined with room temperature roughening using a mixed solution of iodic acid, sulfuric acid, hydrofluoric acid and water, effectively reduces the total internal reflection phenomenon and significantly improves the luminous efficiency.
[0235] Optimizing ITO film thickness: By precisely controlling ITO film deposition parameters (such as temperature and pressure) and calculating the optimal thickness of the ITO film based on the chip's operating wavelength and the refractive index of the ITO film, the optical properties of the ITO film are improved, thereby enhancing the electrical properties of the chip.
[0236] Improve the quality of the electroplating layer: Numerical optimization algorithms (such as gradient descent, genetic algorithm, etc.) are used to accurately find the optimal parameter combination in the electroplating process, thereby ensuring the uniformity and quality of the electroplating layer and effectively improving the bonding yield.
[0237] Enhanced material compatibility: Through experimental verification of interface compatibility between materials, a material combination with good compatibility is selected to ensure the long-term stability and performance of the device.
[0238] Improve etching quality: Through precise control of etching conditions (such as gas ratio, chamber pressure, power, temperature, etc.), good etching quality and uniformity are ensured, thereby improving bonding yield and reliability.
[0239] Improved temporary bonding technology: Solid wax with a melting point above 100°C was selected as the temporary bonding material, and the bonding process was optimized to ensure good bonding between the transition substrate and the epitaxial wafer, thereby improving the yield.
[0240] It should be noted that the present application also claims protection for the infrared LED chip manufactured by the above-mentioned method for manufacturing the infrared LED chip.
[0241] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for manufacturing an infrared LED chip, It is characterized in that Includes steps: Using metal organic chemical vapor deposition method, each layer structure is grown sequentially on a GaAs temporary substrate; A fancy roughening pattern is produced on the ohmic contact layer by using a photolithography process, and a mixed solution of iodic acid, sulfuric acid, hydrofluoric acid and water is used for room temperature roughening to form a P-GaP optical window layer; Use dry ICP etching or wet etching to obtain the conductive hole pattern, ensuring that the etching depth is ≥ the thickness of the ohmic contact layer; ITO thin film deposition: An ITO film is deposited on the entire surface of the P-GaP optical window layer and the conductive hole. The thickness is adjusted according to the wavelength of the chip. The calculation formula is d=m(1 / 4nλ), where d is the target thickness of the ITO film, m is an odd number and the adjustment coefficient is an odd number, λ is the wavelength of the chip, and n is the refractive index of the ITO film. Photolithography of the P-electrode pad pattern is performed on the conductive hole, and a Cr-Pt-Au composite structure is deposited by electron beam evaporation; The wafer is photolithographically masked to form a cutting path pattern, and an ICP etching process is performed to form isolation of the P-side die; A layer of solid wax is evenly coated on the transition substrate, and the transition substrate is bonded to the P surface of the epitaxial wafer through the solid wax for temporary bonding; On the surface of the ohmic layer, an N electrode metal is deposited by electron beam evaporation to form an N electrode; Electroplating a layer of metal Cu on the N electrode as a supporting substrate with a thickness of 50-150 μm; The transition substrate is removed by heating and dissolving the solid wax for separation; The residual solid wax on the surface is removed by soaking in wax removal liquid, and then the transition substrate is peeled off by rinsing with deionized water and cleaning with acetone and ethanol; After the wafer is cut, tested, sorted and inspected, infrared LED chips are obtained; In the process of electroplating a layer of metal Cu on the N electrode as a supporting substrate, a mathematical model of the electroplating process is established to simulate the influence of different electroplating conditions on the quality of the electroplated layer and find the optimal combination of electroplating parameters. Specifically: Construction of mathematical model: Define variables: C: solution composition; Te: electroplating temperature; I: current intensity; V: voltage; D: thickness of electroplating layer; U: uniformity of electroplating layer; Q: The quality of the electroplating layer; Mathematical model: The thickness of the electroplated layer is calculated by Faraday's law: D = k*I*t / A, where k is a constant, t is the electroplating time, and A is the electroplating area; The uniformity U of the electroplated layer is expressed using an empirical model of the following form: Among them, β0, β1, β2, β3, β4 are model coefficients, is the error term; The quality Q of the electroplated layer is: Q=α1D+α2U, where α1 and α2 are weight coefficients; Optimization goal: Maximize the quality Q of the electroplated layer; Constraints: Solution composition: copper sulfate concentration C∈[150,250]g / L; Electroplating temperature: Te = 25 °C; Current intensity: I∈[0.1,0.4]A; Voltage: V∈[3,6]V; Electroplating time: Determined according to thickness requirements; Electroplating layer thickness: D∈[50,150]μm; Solution method: Use gradient descent or genetic algorithm to solve the optimal combination of electroplating parameters; The gradient descent algorithm includes: Initialization: Randomly select a set of initial parameter values; Objective function: Calculate the quality Q of the electroplating layer according to the mathematical model; Gradient calculation: Use the finite difference method to calculate the gradient of the objective function with respect to each parameter; Iterative update: Update the parameter value in the direction of the gradient until the stopping condition that the gradient reaches the maximum number of iterations is met; Genetic algorithms include: Initialization: Randomly generate an initial population containing multiple individuals; Fitness evaluation: Calculate the fitness value of each individual, which is the quality Q of the electroplating layer; Selection operation: select individuals with high fitness to enter the next generation; Crossover operation: Generate new individuals by randomly exchanging some genes of two individuals; Mutation operation: randomly modify a gene of an individual with a fixed probability; Iterative update: Repeat the selection, crossover, and mutation operations until the stopping condition of reaching the maximum number of iterations is met.
2. A method for manufacturing an infrared LED chip according to claim 1, It is characterized in that The thickness d of the ITO film corresponding to different m values is calculated according to the specific wavelength λ and the refractive index n of the ITO film, and the optical properties at these different thicknesses are tested experimentally to find the optimal thickness of the ITO film.
3. A method for manufacturing an infrared LED chip according to claim 1, It is characterized in that The Cr-Pt-Au composite structure is deposited by electron beam evaporation. Specifically, the thickness of the first Cr layer is 20-150nm, the thickness of the second Pt layer is 30-100nm, and the thickness of the third Au layer is 2000-4000nm, and a rapid annealing treatment is performed.
4. The method for manufacturing an infrared LED chip according to claim 1, It is characterized in that The solid wax is specifically: a solid wax with a melting point higher than 100°C.
Citation Information
Patent Citations
Graphene film and surface metallization method thereof
CN116043221A
Infrared LED chip and manufacturing method thereof
CN117199209A
Bonding aluminum wire with nickel-coated layer and preparation method and application of bonding aluminum wire
CN117779141A
Electrolytic copper plating solution analyzer, and electrolytic copper plating solution analysis method
US20160377573A1