Electrode slurry composition, electrode sheet and solid-state battery
By using a modifier with a bipolar modifier in a sulfide solid state battery, the problem of reaction of high-polar solvents with sulfide electrolytes and agglomeration of inorganic particles is solved, the stability and dispersion of the electrode slurry are improved, and the improvement of the stability and dispersion of the electrode slurry are improved, and the improvement of the Battery performance.
Patent Information
- Application Number
- CN202210613549.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-05-31
AI Technical Summary
In sulfide solid state batteries, the reaction of high-polar solvents with sulfide electrolytes leads to deterioration of conductivity, and inorganic particles tend to agglomerate and settle in the low-polar dispersion system, resulting in uneven gradients of the composite electrode layer and affecting battery performance.
Introduce bipolar modifiers, the molecular structure contains low polarity group A and medium polarity group B, group A is dissolved in low polarity solvent, group B is pinned to the electrode active material and The surface of the sulfide electrolyte forms a barrier layer to prevent the agglomeration and settlement of inorganic particles and improve the dispersion of the slurry.
Effectively prevent the settlement of inorganic particles, improve the stability and dispersion of the slurry, and enhance the first-circle efficiency and cycle stability of the battery.
Smart Images

Figure BDA0003672687720000031 
Figure BDA0003672687720000051 
Figure BDA0003672687720000091
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of batteries, and in particular, to an electrode slurry composition, an electrode pole piece and a solid-state battery. Background Art
[0002] All-solid-state batteries are considered to be the next generation of highly safe batteries because they use solid electrolytes to replace the electrolytes of traditional batteries and have non-flammable properties. Among them, sulfide solid electrolytes have high ionic conductivity (up to 10 -2 S / cm) and low grain boundary impedance, which has attracted wide attention in the industry. In the process of preparing and coating sulfide solid-state battery electrode slurry, the use of highly polar and protic solvents (such as NMP and H2O commonly used in traditional battery systems) will react with sulfide electrolytes, causing serious deterioration of electrolyte conductivity and failure of battery performance. Therefore, it is necessary to select non-polar and low-polarity solvents.
[0003] The selection of non-polar and weakly polar solvents can inhibit the decomposition of solid electrolytes, but the stability of the slurry itself and the uniformity of the dispersion of solid particles (including active materials, solid electrolytes and conductive agents, etc.) need to be further improved. Due to the weak polarity of solvent molecules, their ability to disperse highly polar inorganic particles, especially oxide-based positive electrode particles, is poor, making inorganic particles prone to agglomeration and sedimentation. In addition, due to the low density of sulfide electrolyte particles (2 g / cm 3 about) and active material density (such as 5.1g / cm for LiCoO2 positive electrode material 2 ), which makes them more likely to be decomposed in low-polarity dispersion systems, resulting in uneven gradients in the composite electrode layer and affecting battery performance. Summary of the invention
[0004] The object of the present disclosure is to provide an electrode slurry composition, an electrode pole sheet and a solid-state battery, wherein the electrode slurry composition can improve the uniformity and stability of the slurry.
[0005] The first aspect of the present disclosure provides an electrode slurry composition, the electrode slurry composition comprising an electrode active material, a sulfide electrolyte, a solvent and a modifier, the modifier comprising a group A and a group B;
[0006] The group A is selected from substituted or unsubstituted hydrocarbon groups, substituted or unsubstituted hydrocarbon groups containing heteroatoms, and the number of carbon atoms in the group A is 1 to 30; the group B is selected from one or more of alkoxy groups, mercapto groups, ester groups, phosphorus-containing groups, silicate groups, alkoxysilane groups, titanate groups and carboxylic anhydride groups.
[0007] Optionally, the modifier has a structure as shown in the following formula (1):
[0008] (A) n -(B) m , formula (1),
[0009] m represents the number of groups B, selected from 1, 2, 3 or 4. When m is greater than 1, each group B is the same or different; n represents the number of groups A, selected from 1, 2, 3 or 4. When n is greater than 1, each group A is the same or different.
[0010] Optionally, the relative molecular mass of the modifier is 100 to 3000; preferably, the molecules of the modifier are in a chain structure, and the length of the main chain of the modifier is 1 to 30 nm.
[0011] Optionally, the group A is selected from a saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, preferably a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, or a substituted or unsubstituted hydrocarbon group containing heteroatoms having 1 to 20 carbon atoms; preferably, the group A is selected from a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted cycloalkyl group having 2 to 20 carbon atoms. One or more of substituted or unsubstituted alkynyl, substituted or unsubstituted aryl having 6 to 20 carbon atoms, substituted or unsubstituted alkyl having 1 to 20 carbon atoms and containing heteroatoms, substituted or unsubstituted cycloalkyl having 3 to 20 carbon atoms and containing heteroatoms, substituted or unsubstituted alkenyl having 2 to 20 carbon atoms and containing heteroatoms, substituted or unsubstituted alkynyl having 2 to 20 carbon atoms and containing heteroatoms, and substituted or unsubstituted aryl having 6 to 20 carbon atoms and containing heteroatoms;
[0012] Optionally, the substituent of the group A is selected from one or more of a halogen group, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, and an alkynyl group having 2 to 5 carbon atoms, and the heteroatom is a boron atom.
[0013] Optionally, the group B is selected from one or more of an alkoxy group having 1 to 40 carbon atoms, a thiol group, an ester group having 2 to 40 carbon atoms, a phosphate group having 1 to 40 carbon atoms, a phosphite group having 1 to 40 carbon atoms, a hypophosphite group having 1 to 40 carbon atoms, a silicate group having 1 to 40 carbon atoms, an alkoxysilane group having 1 to 40 carbon atoms, a titanate group having 1 to 40 carbon atoms, a carboxylic anhydride group having 2 to 40 carbon atoms, a phosphoric anhydride group having 1 to 40 carbon atoms, and a phosphoric acid cyclic anhydride group having 1 to 40 carbon atoms.
[0014] Optionally, the group B is selected from the group consisting of the following groups:
[0015]
[0016] wherein x represents the number of oxygen atoms, which is selected from 0 or 1; R, R' and R" are independently selected from substituted or unsubstituted alkyl having 1 to 20 carbon atoms, substituted or unsubstituted cycloalkyl having 3 to 20 carbon atoms, substituted or unsubstituted alkenyl having 2 to 20 carbon atoms, substituted or unsubstituted alkynyl having 2 to 20 carbon atoms, and substituted or unsubstituted phenyl having 6 to 20 carbon atoms; Z and Z' are independently selected from H, substituted or unsubstituted alkyl having 1 to 18 carbon atoms, substituted or unsubstituted cycloalkyl having 3 to 18 carbon atoms, substituted or unsubstituted alkenyl having 2 to 18 carbon atoms, substituted or unsubstituted alkynyl having 2 to 18 carbon atoms, substituted or unsubstituted phenyl having 6 to 18 carbon atoms, and substituted or unsubstituted alkoxy having 1 to 18 carbon atoms;
[0017] Preferably, the substituents in R, R', R", Z and Z' are independently selected from one or more of a halogen group, a boron-containing group, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms and an alkynyl group having 2 to 5 carbon atoms.
[0018] Optionally, the modifier is selected from one or more of ethylene glycol nonylphenyl ether, dioctyl ether, ethyl laurate, trioctyl phosphate, n-octanoic anhydride, 1-propyl phosphoric acid cyclic anhydride, 2-ethyl-1-hexyl titanium and dodecyltrimethoxysilane.
[0019] Optionally, the solvent is selected from organic solvents having a relative dielectric constant of less than 6; preferably, the organic solvent is selected from one or more of methylcyclohexane, heptane, toluene, xylene, trimethylbenzene, anisole, butyl butyrate and isobutyl isobutyrate.
[0020] Optionally, based on the total weight of solids in the electrode slurry, the content of the electrode active material is 50wt% to 90wt%, and the content of the sulfide electrolyte is 10wt% to 50wt%; based on the total weight of the electrode slurry, the content of the solvent is 25wt% to 75wt%, and the content of the modifier is 0.1wt% to 5wt%; preferably, the weight ratio of the modifier to the solvent is 1:(70-120), and the weight ratio of the modifier to the sulfide electrolyte is 1:(25-100).
[0021] Optionally, the electrode slurry composition further comprises a conductive agent and a binder, and based on the total weight of solids in the electrode slurry, the content of the conductive agent is 0.1wt% to 10wt%, and the content of the binder is 0.1wt% to 10wt%; the conductive agent is selected from one or more of carbon black conductive agents, carbon nanotubes and vapor-grown carbon fibers; the binder is selected from one or more of polyether binders, styrene rubber binders, acrylonitrile rubber binders, polyacrylic acid binders and alkylated cellulose binders.
[0022] A second aspect of the present disclosure provides an electrode plate, comprising a current collector and an electrode material layer, wherein the electrode material layer is prepared using the electrode slurry composition described in the first aspect of the present disclosure.
[0023] The third aspect of the present disclosure provides an electrode plate, the electrode plate comprising a current collector and an electrode material layer covering the current collector, the electrode material layer comprising an electrode active material, a sulfide electrolyte and a modifier, the modifier comprising a group A and a group B;
[0024] The group A is selected from substituted or unsubstituted hydrocarbon groups, substituted or unsubstituted hydrocarbon groups containing heteroatoms, and the number of carbon atoms in the group A is 1 to 30;
[0025] The group B is selected from one or more of an alkoxy group, a mercapto group, an ester group, a phosphorus-containing group, a silicate group, an alkoxysilane group, a titanate group and a carboxylic anhydride group.
[0026] Optionally, based on the total weight of the electrode material layer, the content of the electrode active material is 48wt% to 90wt%, the content of the sulfide electrolyte is 5wt% to 50wt%, and the content of the modifier is 0.1wt% to 5wt%; the weight ratio of the modifier to the sulfide electrolyte is 1:(25 to 100).
[0027] Optionally, the modifier has a structure as shown in the following formula (1):
[0028] (A) n -(B) m , formula (1),
[0029] m represents the number of groups B, selected from 1, 2, 3 or 4, when m is greater than 1, the groups B are the same or different; n represents the number of groups A, selected from 1, 2, 3 or 4, when n is greater than 1, the groups A are the same or different;
[0030] The group A is selected from substituted or unsubstituted hydrocarbon groups with 1 to 20 carbon atoms, substituted or unsubstituted hydrocarbon groups containing heteroatoms; preferably, the group A is selected from substituted or unsubstituted alkyl groups with 1 to 20 carbon atoms, substituted or unsubstituted cycloalkyl groups with 3 to 20 carbon atoms, substituted or unsubstituted alkenyl groups with 2 to 20 carbon atoms, substituted or unsubstituted alkynyl groups with 2 to 20 carbon atoms, substituted or unsubstituted aryl groups with 6 to 20 carbon atoms, substituted or unsubstituted alkane groups with 1 to 20 carbon atoms, The substituent of the group A is selected from one or more of a halogen group, an alkyl group with 1 to 5 carbon atoms, an alkenyl group with 2 to 5 carbon atoms, and an alkynyl group with 2 to 5 carbon atoms, and the heteroatom is a boron atom;
[0031] The group B is selected from the group consisting of the following groups:
[0032]
[0033] wherein x represents the number of oxygen atoms, which is selected from 0 or 1; R, R' and R" are independently selected from substituted or unsubstituted alkyl having 1 to 20 carbon atoms, substituted or unsubstituted cycloalkyl having 3 to 20 carbon atoms, substituted or unsubstituted alkenyl having 2 to 20 carbon atoms, substituted or unsubstituted alkynyl having 2 to 20 carbon atoms, and substituted or unsubstituted phenyl having 6 to 20 carbon atoms; Z and Z' are independently selected from H, substituted or unsubstituted alkyl having 1 to 18 carbon atoms, substituted or unsubstituted cycloalkyl having 3 to 18 carbon atoms, substituted or unsubstituted alkenyl having 2 to 18 carbon atoms, substituted or unsubstituted alkynyl having 2 to 18 carbon atoms, substituted or unsubstituted phenyl having 6 to 18 carbon atoms, and substituted or unsubstituted alkoxy having 1 to 18 carbon atoms;
[0034] Preferably, the substituents in R, R', R", Z and Z' are independently selected from one or more of a halogen group, a boron-containing group, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms and an alkynyl group having 2 to 5 carbon atoms.
[0035] Optionally, the modifier is selected from one or more of ethylene glycol nonylphenyl ether, dioctyl ether, ethyl laurate, trioctyl phosphate, n-octanoic anhydride, 1-propyl phosphoric acid cyclic anhydride, 2-ethyl-1-hexyl titanium and dodecyltrimethoxysilane.
[0036] A fourth aspect of the present disclosure provides a solid-state battery comprising the electrode plates described in the second and third aspects of the present disclosure.
[0037] Through the above technical scheme, the electrode slurry composition provided by the present disclosure introduces a bipolar modifier, and the molecular structure of the modifier includes a low-polarity group A and a medium-polarity group B, wherein the low-polarity group A can be well dissolved in the low-polarity solvent of the slurry, and the medium-polarity group B can be well pinned on the surface of the electrode active material and the sulfide electrolyte. In this way, the modifier can form a barrier layer that hinders the agglomeration of inorganic particles, increase the steric hindrance of the agglomeration of inorganic particles, effectively prevent the sedimentation of inorganic particles, and play a role in stabilizing the slurry; at the same time, the modifier can enhance the affinity between the low-polarity solvent molecules and the inorganic particles, inhibit the agglomeration and flocculation of inorganic particles, thereby inhibiting the sedimentation and stratification caused by the uneven solid content of the slurry, and play a role in improving the dispersibility of the slurry. The electrode plate provided by the present disclosure has good first-cycle efficiency and cycle stability.
[0038] Other features and advantages of the present disclosure will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0039] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0040] The first aspect of the present disclosure provides an electrode slurry composition, which includes an electrode active material, a sulfide electrolyte, a solvent and a modifier, wherein the modifier includes a group A and a group B; the group A is selected from a substituted or unsubstituted hydrocarbon group, a substituted or unsubstituted hydrocarbon group containing heteroatoms, and the number of carbon atoms of the group A is 1 to 30; the group B is selected from one or more of an alkoxy group, a mercapto group, an ester group, a phosphorus-containing group, a silicate group, an alkoxysilane group, a titanate group and a carboxylic anhydride group.
[0041] Optionally, the phosphorus-containing groups include phosphorus-containing groups with medium polarity such as phosphate groups, phosphite groups, hypophosphite groups, phosphoric acid anhydride groups, phosphoric acid cyclic anhydride groups, etc.; optionally, the phosphate groups may be phosphate triester groups.
[0042] Optionally, the general structural formula of the triester of phosphoric acid is O=P(OR1)3, which means that the three hydroxyl hydrogens on the orthophosphoric acid are replaced by hydrocarbon groups, that is, it has three alkoxy groups; the general structural formula of silicate is Si(OR1)4, wherein each R1 is the same or different hydrocarbon group; the general structural formula of alkoxysilane is R2-Si(OR1)3, (R2)2-Si(OR1)2 or (R2)3-Si(OR1), that is, one or two or three alkoxy groups in the orthosilicate are replaced by hydrocarbon groups, wherein each R2 is the same or different hydrocarbon group; phosphoric anhydride refers to the anhydride of orthophosphoric acid, and the phosphoric acid cyclic anhydride group refers to the group shown below
[0043] The electrode slurry composition disclosed in the present invention has a bipolar modifier, and the molecular structure of the modifier includes a low-polarity group A and a medium-polarity group B, wherein the low-polarity group A can be well dissolved in the low-polarity solvent of the slurry, and the medium-polarity group B can be well pinned on the surface of the electrode active material and the sulfide electrolyte. In this way, the modifier can form a barrier layer that hinders the agglomeration of inorganic particles, increase the steric hindrance of the agglomeration of inorganic particles, effectively prevent the sedimentation of inorganic particles, and play a role in stabilizing the slurry; at the same time, the modifier can enhance the affinity between the low-polarity solvent molecules and the inorganic particles, inhibit the agglomeration and flocculation of the inorganic particles, thereby inhibiting the sedimentation and stratification caused by the uneven solid content of the slurry, and play a role in improving the dispersibility of the slurry.
[0044] In one embodiment of the present disclosure, the modifier has a structure as shown in the following formula (1):
[0045] (A) n -(B) m , formula (1), wherein m represents the number of groups B, selected from 1, 2, 3 or 4, when m is greater than 1, each group B is the same or different; n represents the number of groups A, selected from 1, 2, 3 or 4, when n is greater than 1, each group A is the same or different.
[0046] In one embodiment of the present disclosure, the relative molecular mass of the modifier is 100 to 3000, preferably 200 to 1500; preferably, the molecule of the modifier is in a chain structure, for example, a straight chain or branched structure, and the length of the molecular main chain of the modifier is 1 to 30 nm, preferably 2 to 8 nm. In the above embodiment, "molecular main chain" refers to the longest chain in the molecule, and its testing method is gas chromatography-mass spectrometry, nuclear magnetic resonance, etc.; by selecting a modifier with a relative molecular mass of 100 to 3000, it can have a certain thickening effect on the slurry, inhibit the uneven distribution of the solid content of the slurry and the gradient stratification phenomenon, which can further stabilize the slurry and improve the battery performance.
[0047] In one embodiment of the present disclosure, the group A is selected from a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms, a substituted or unsubstituted hydrocarbon group containing heteroatoms having 1 to 20 carbon atoms; preferably, the group A is selected from a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 2 ... The present invention relates to a substituted or unsubstituted heteroatom-containing alkyl group having 1 to 5 carbon atoms, a substituted or unsubstituted heteroatom-containing cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted heteroatom-containing alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted heteroatom-containing alkynyl group having 2 to 20 carbon atoms, and a substituted or unsubstituted heteroatom-containing aryl group having 6 to 20 carbon atoms; preferably, the substituent of the group A is selected from one or more of a halogen group, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, and an alkynyl group having 2 to 5 carbon atoms, and the heteroatom is a boron atom.
[0048] In the above embodiment, one end of the modifier is a low-polarity group A, and the hydrocarbon skeleton of the group A can be well dissolved in the low-polarity solvent of the slurry, forming a barrier layer that hinders the agglomeration of inorganic particles, effectively preventing the sedimentation of inorganic particles, and playing a role in stabilizing the slurry. The term "substituted or unsubstituted" means that the functional group recorded after the term may or may not have a substituent (hereinafter, for the convenience of description, the substituent is collectively referred to as R c For example, "substituted or unsubstituted aryl" refers to a substituted c The above-mentioned substituents, namely R c , for example, it can be a halogen group, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, or a cycloalkyl group. The number of carbon atoms of the substituted or unsubstituted functional group refers to the total number of carbon atoms. For example, if the group A is selected from a substituted aryl group having 12 carbon atoms, the total number of carbon atoms of the aryl group and the substituents thereon is 12.
[0049] In one embodiment of the present disclosure, the group B is selected from one or more of an alkoxy group having 1 to 40 carbon atoms, a thiol group, an ester group having 2 to 40 carbon atoms, a phosphate group having 1 to 40 carbon atoms, a phosphite group having 1 to 40 carbon atoms, a hypophosphite group having 1 to 40 carbon atoms, a silicate group having 1 to 40 carbon atoms, an alkoxysilane group having 1 to 40 carbon atoms, a titanate group having 1 to 40 carbon atoms, a carboxylic anhydride group having 2 to 40 carbon atoms, a phosphoric anhydride group having 1 to 40 carbon atoms, and a phosphoric acid cyclic anhydride group having 1 to 40 carbon atoms.
[0050] In one embodiment of the present disclosure, the alkoxy group is the following group 1, the thiol group is the following group 2, the ester group is the following group 3, the phosphorus-containing group can be one or more of the following groups 4, 8 and 9, the silicate group or alkoxysilane group is the following group 5, the titanate group is the following group 6, and the carboxylic anhydride group is the following group 7.
[0051]
[0052] In one embodiment of the present disclosure, the group B is selected from the group consisting of the following groups:
[0053]
[0054] wherein x represents the number of oxygen atoms, which is selected from 0 or 1; R, R' and R" are each independently selected from hydrocarbons or halogenated hydrocarbons with less than 20 carbon atoms, phenyl, etc.; for example, R, R' and R" are each independently selected from substituted or unsubstituted alkyl with 1 to 20 carbon atoms, substituted or unsubstituted cycloalkyl with 3 to 20 carbon atoms, substituted or unsubstituted alkenyl with 2 to 20 carbon atoms, substituted or unsubstituted alkynyl with 2 to 20 carbon atoms, substituted or unsubstituted phenyl with 6 to 20 carbon atoms; Z and Z' are each independently selected from H, substituted or unsubstituted alkyl with 1 to 18 carbon atoms, substituted or unsubstituted cycloalkyl with 3 to 18 carbon atoms, 2 to 18 carbon atoms, substituted or unsubstituted alkenyl having 2 to 18 carbon atoms, substituted or unsubstituted alkynyl having 2 to 18 carbon atoms, substituted or unsubstituted phenyl having 6 to 18 carbon atoms, and substituted or unsubstituted alkoxy having 1 to 18 carbon atoms; in a preferred embodiment, the substituents in R, R', R", Z and Z' are independently selected from one or more of a halogen group, a boron-containing group, an alkyl having 1 to 5 carbon atoms, an alkenyl having 2 to 5 carbon atoms, and an alkynyl having 2 to 5 carbon atoms, and the boron-containing group is, for example, one or more of an alkyl having 1 to 5 carbon atoms containing a boron atom, an alkenyl having 2 to 5 carbon atoms containing a boron atom, and an alkynyl having 2 to 5 carbon atoms containing a boron atom.
[0055] In one embodiment of the present disclosure, group B does not contain a high polar group (such as a carboxyl group, an amine group, a hydroxyl group, a sulfonic acid group, a phosphoric acid group, an aldehyde group, an amide group, etc.).
[0056] In the above embodiment, the other end of the modifier is a moderately polar group B, which can be well pinned to the surface of the electrode active material and the sulfide electrolyte, enhance the affinity between the low-polarity solvent molecules and the inorganic particles, increase the repulsion between the inorganic particles, and improve the dispersibility of the slurry, thereby inhibiting the sedimentation and stratification caused by uneven solid content of the slurry.
[0057] In one embodiment of the present disclosure, the modifier is selected from one or more of ethylene glycol nonylphenyl ether, dioctyl ether (CAS No. 629-82-3), ethyl laurate (CAS No. 106-33-2), trioctyl phosphate (CAS No. 78-42-2), n-octanoic anhydride (CAS No. 623-66-5), 1-propylphosphoric acid cyclic anhydride (CAS No. 68957-94-8), 2-ethyl-1-hexyl titanium (CAS No. 1070-10-6) and dodecyltrimethoxysilane (CAS No. 3069-21-4).
[0058] In one embodiment of the present disclosure, the solvent is a solvent that is stable to the sulfide electrolyte, and the solvent is selected from a non-polar organic solvent and a weakly polar organic solvent. In a preferred embodiment, the solvent is selected from an organic solvent having a relative dielectric constant of less than 6, such as an organic solvent having a relative dielectric constant of 1, 2, 3, 4, 5, or a numerical range between any two of them. The organic solvent does not dissolve the sulfide electrolyte and does not react with the sulfide electrolyte; in a preferred embodiment, the organic solvent is selected from one or more of methylcyclohexane, heptane, toluene, xylene, trimethylbenzene, anisole, butyl butyrate and isobutyl isobutyrate. In the above embodiment, by selecting a solvent, the decomposition of the sulfide electrolyte can be effectively inhibited, while increasing the dispersibility of each component, improving the stability of the slurry, and thus improving the battery performance.
[0059] In one embodiment of the present disclosure, based on the total weight of the solids in the electrode slurry, the content of the electrode active material is 50wt% to 90wt%, preferably 60wt% to 80wt%; the content of the sulfide electrolyte is 10wt% to 50wt%, preferably 20wt% to 40wt%; based on the total weight of the electrode slurry, the content of the solvent is 25wt% to 75wt%, preferably 40wt% to 55wt%; the content of the modifier is 0.1wt% to 5wt%, preferably 0.2wt% to 2wt%; wherein the weight ratio of the modifier to the solvent is 1: (70 to 120), preferably 1: (80 to 100); the weight ratio of the modifier to the sulfide electrolyte is 1: (25 to 100), preferably 1: (35 to 70). In the above embodiment, by selecting the components with the preferred content, the dispersibility and uniformity of each component can be further improved, thereby improving the stability of the slurry.
[0060] In one embodiment of the present disclosure, the electrode slurry composition further comprises a conductive agent and a binder. Based on the total weight of the solids in the electrode slurry, the content of the conductive agent is 0.1wt% to 10wt%, preferably 1wt% to 5wt%; the content of the binder is 0.1wt% to 10wt%, preferably 0.5wt% to 4wt%; the conductive agent is selected from one or more of carbon black conductive agents, carbon nanotubes and vapor-grown carbon fibers; the binder is selected from one or more of polyether binders, styrene rubber binders, acrylonitrile rubber binders, polyacrylic acid binders and alkylated cellulose binders. In the above embodiment, by selecting the preferred content of the conductive agent and binder, the stability and conductivity of the slurry can be further improved, thereby improving the battery performance.
[0061] In a preferred embodiment, the electrode active material includes a positive electrode active material or a negative electrode active material, and the positive electrode active material includes one or more of an olivine positive electrode material, a layered oxide positive electrode material, a spinel positive electrode material, a sulfur positive electrode material, and a sulfide positive electrode material; the negative electrode active material includes one or more of a graphite negative electrode material, a silicon negative electrode material, a silicon-carbon negative electrode material, and a silicon-oxygen negative electrode material; in a preferred embodiment, the electrode active material includes a positive electrode active material, and the positive electrode active material includes LiFePO4, NCM, NCA, LiCoO2, LiMn2O4, Li4Ti5O 12 , one or more of S8, FeS2 and CuS;
[0062] In one embodiment of the present disclosure, the sulfide electrolyte is a sulfide solid electrolyte. In one embodiment of the present disclosure, the lithium ion conductivity of the sulfide electrolyte is higher than 10 -4 S / cm; preferably, the sulfide electrolyte includes one or more of a fast ion conductor solid electrolyte, a argyrodite solid electrolyte, a glass ceramic solid electrolyte and a thiophosphate system solid electrolyte; in a preferred embodiment, the sulfide electrolyte includes Li3PS4, LGPS, Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 , Li6PS5Cl, LiI-(70Li2S-30P2S5), Li7P3S 11 , Li4PS4I and Li7P2S8I. By selecting the preferred types of electrode active materials and sulfide electrolytes, the agglomeration and flocculation of inorganic particles can be further suppressed, the slurry stability can be improved, and the battery performance can be improved.
[0063] A second aspect of the present disclosure provides an electrode plate, comprising a current collector and an electrode material layer, wherein the electrode material layer is prepared using the electrode slurry composition provided in the first aspect of the present disclosure.
[0064] The above-mentioned “the electrode material layer is prepared by using the electrode slurry composition provided by the first aspect of the present disclosure” can be understood as that, in the electrode material layer, except for the removal of the solvent in the electrode slurry composition provided by the first aspect of the present disclosure, the composition and relative content of other substances remain unchanged.
[0065] In one embodiment of the present disclosure, the preparation method of the electrode plate is as follows: the above-mentioned electrode slurry composition containing the modifier is uniformly coated on the current collector, dried and pressed; wherein the coating method can be spraying, scraping and extrusion coating; the drying conditions include: in a vacuum environment or an Ar gas environment, the drying temperature is 60 to 150°C, and the time is 2 to 24 hours; the pressing conditions include: the pressure is 5 to 500 MPa, and the pressing method is flat plate pressing or equal-diameter pressing, wherein the thickness of the electrode plate is 10 to 100 μm.
[0066] The third aspect of the present disclosure provides an electrode plate, which includes a current collector and an electrode material layer covered on the current collector, wherein the electrode material layer includes an electrode active material, a sulfide electrolyte and a modifier, and the modifier includes a group A and a group B; the group A is selected from a substituted or unsubstituted hydrocarbon group, a substituted or unsubstituted hydrocarbon group containing heteroatoms, and the number of carbon atoms of the group A is 1 to 30; the group B is selected from one or more of an alkoxy group, a mercapto group, an ester group, a phosphorus-containing group, a silicate group, an alkoxysilane group, a titanate group and a carboxylic anhydride group.
[0067] The electrode plate provided by the present invention contains a bipolar modifier, and the medium-polar group B of the modifier can be well "pinned" on the surface of the electrode active material and the sulfide electrolyte, and the low-polar group A can be well dissolved in the low-polarity solvent of the slurry to form a barrier layer that hinders the agglomeration of inorganic particles, thereby hindering the agglomeration and flocculation of inorganic particles, avoiding the sedimentation and stratification phenomenon caused by uneven solid content of the slurry, and increasing the first-cycle efficiency and cycle stability of the electrode plate.
[0068] In one embodiment of the present disclosure, based on the total weight of the electrode material layer, the content of the electrode active material is 48wt% to 90wt%, preferably 60wt% to 80wt%; the content of the sulfide electrolyte is 5wt% to 50wt%, preferably 20wt% to 40wt%; the content of the modifier is 0.1wt% to 5wt%, preferably 0.2wt% to 2wt%; the weight ratio of the modifier to the sulfide electrolyte is 1:(25 to 100), preferably 1:(35 to 70).
[0069] The modifier is the modifier in the electrode slurry composition provided in the first aspect of the present disclosure. In one embodiment of the present disclosure, the modifier may have a structure as described in formula (1): (A) n -(B) m , formula (1), wherein m represents the number of groups B, selected from 1, 2, 3 or 4, when m is greater than 1, the groups B are the same or different; n represents the number of groups A, selected from 1, 2, 3 or 4, when n is greater than 1, the groups A are the same or different; the groups A are selected from substituted or unsubstituted hydrocarbon groups with 1 to 20 carbon atoms, substituted or unsubstituted hydrocarbon groups containing heteroatoms; the groups B are selected from the group consisting of the following groups:
[0070]
[0071] In one embodiment of the present disclosure, the modifier is selected from one or more of ethylene glycol nonylphenyl ether, dioctyl ether, ethyl laurate, trioctyl phosphate, n-octanoic anhydride, 1-propyl phosphoric acid cyclic anhydride, 2-ethyl-1-hexyl titanium and dodecyltrimethoxysilane.
[0072] A fourth aspect of the present disclosure provides a solid-state battery comprising the electrode plates described in the second and third aspects of the present disclosure.
[0073] The electrode slurry composition provided by the present disclosure introduces a bipolar modifier, and the molecular structure of the modifier includes a low-polarity group A and a medium-polarity group B, wherein the low-polarity group A can be well dissolved in the low-polarity solvent of the slurry, and the medium-polarity group B can be well pinned on the surface of the electrode active material and the sulfide electrolyte. In this way, the modifier can form a barrier layer that hinders the agglomeration of inorganic particles, increase the steric hindrance of the agglomeration of inorganic particles, effectively prevent the sedimentation of inorganic particles, and play a role in stabilizing the slurry; at the same time, the modifier can enhance the affinity between the low-polarity solvent molecules and the inorganic particles, inhibit the agglomeration and flocculation of inorganic particles, thereby inhibiting the sedimentation and stratification caused by the uneven solid content of the slurry, and play a role in improving the dispersibility of the slurry. The electrode plate provided by the present disclosure has good first-cycle efficiency and cycle stability.
[0074] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.
[0075] In the following examples and comparative examples, unless otherwise specified, the raw materials used are commercially available products.
[0076] The molecular main chain length was tested by nuclear magnetic resonance, and the instrument model was GY-PNMR12-6HF;
[0077] The battery electrode thickness is tested using an inductive thickness meter, and the instrument model is Mahr C1202.
[0078] Example 1
[0079] (1) LiNbO3@LiCoO2 (LiNbO3 coated LiCoO2, purchased from Xiamen Tungsten Industry) was used as the positive electrode active material, Li6PS5Cl and Li7P3S 11 It is a sulfide electrolyte, acetylene black is a conductive agent, polystyrene-butadiene is a binder, heptane is a solvent, and ethylene glycol nonylphenyl ether is a modifier;
[0080] 37.74g of LiNbO3@LiCoO2 positive electrode material, 16.17g of Li6PS5Cl sulfide electrolyte, 1.08g of acetylene black, 11g of heptane solution containing 10% polystyrene-butadiene and 36g of heptane were mixed, and 0.51g of ethylene glycol nonylphenyl ether was added as a modifier. A vortex mixer (AS ONE test tube shakers) was used to disperse at 2000RPM for 10min to obtain a positive electrode slurry 1, in which the modifier was a chain structure with a relative molecular mass of 264, the length of the molecular main chain of the modifier was 2.3nm, the solid content in the positive electrode slurry 1 was 55.2%, and the mass of heptane was 44.8% of the total mass.
[0081] Among them, the structural formula of ethylene glycol nonylphenyl ether is The preparation method is as follows: select excess ethylene glycol, mix it evenly with phenol and nonanol, add sodium peroxide as a catalyst, control the reaction temperature to 190°C and the reaction pressure to 300 kPa, and after sufficient reaction, remove the excess ethylene glycol by reduced pressure distillation to obtain ethylene glycol nonylphenyl ether.
[0082] (2) Preparation of electrode plate: The positive electrode slurry 1 is mixed and coated on the Al current collector. The coating thickness is controlled to be 30 μm, and then placed in a vacuum oven at 60° C. for 5 h to obtain the electrode plate 1.
[0083] Example 2
[0084] The same as Example 1, the only difference is that the modifier ethylene glycol nonylphenyl ether is replaced by the same weight of dioctyl ether (structural formula: CAS No.: 629-82-3), wherein dioctyl ether has a chain structure, a relative molecular mass of 242, and a molecular main chain length of 2.8 nm, to obtain a positive electrode slurry 2 and an electrode plate 2.
[0085] Example 3
[0086] The same as Example 1, the only difference is that the modifier ethylene glycol nonylphenyl ether is replaced by the same weight of ethyl laurate (i.e. ethyl dodecanoate, structural formula: CAS number: 106-33-2), 36g of heptane was replaced by 36g of butyl butyrate, and 11g of heptane solution containing 10% polystyrene-butadiene was replaced by 11g of butyl butyrate solution containing 10% polyisobutyl methacrylate, wherein ethyl laurate was in a chain structure with a relative molecular mass of 228 and a main chain length of 2.6nm, to obtain a positive electrode slurry 3 and an electrode plate 3.
[0087] Example 4
[0088] The same as Example 1, the only difference is that the modifier ethylene glycol nonylphenyl ether is replaced by the same weight of trioctyl phosphate (structural formula: CAS No.: 78-42-2), 36g of heptane was replaced by 36g of butyl butyrate, and 11g of heptane solution containing 10% polystyrene-butadiene was replaced by 11g of butyl butyrate solution containing 10% polyisobutyl methacrylate, wherein trioctyl phosphate had a chain structure, a relative molecular mass of 434, and a molecular main chain length of 3.2nm, to obtain a positive electrode slurry 4 and an electrode plate 4.
[0089] Example 5
[0090] The same as Example 1, the only difference is that the modifier ethylene glycol nonylphenyl ether is replaced by the same weight of dodecyl trimethoxy silane (structural formula: CAS number: 3069-21-4), wherein dodecyltrimethoxysilane is in a chain structure, with a relative molecular mass of 291 and a main chain length of 2.6 nm, to obtain a positive electrode slurry 5 and an electrode plate 5.
[0091] Example 6
[0092] The same as Example 1, the only difference is that the modifier ethylene glycol nonylphenyl ether is replaced by the same weight of n-octanoic anhydride (structural formula: CAS number: 623-66-5), wherein n-octanoic anhydride is in a chain structure, with a relative molecular mass of 270 and a molecular main chain length of 2.6 nm, to obtain a positive electrode slurry 6 and an electrode plate 6.
[0093] Example 7
[0094] The same as Example 1, the only difference is that the modifier ethylene glycol nonylphenyl ether is replaced by the same weight of 1-propyl phosphoric acid cyclic anhydride (structural formula: CAS No.: 68957-94-8), the relative molecular mass is 318, the length of the molecular main chain is 2.7nm, and the positive electrode slurry 7 and the electrode plate 7 are obtained.
[0095] Example 8
[0096] The same as Example 1, the only difference is that the modifier ethylene glycol nonylphenyl ether is replaced by the same weight of 2-ethyl-1-hexyl titanium (structural formula: CAS No.: 1070-10-6), its relative molecular mass is 565, the length of the molecular main chain is 5.1nm, and the positive electrode slurry 8 and the electrode plate 8 are obtained.
[0097] Example 9
[0098] The same as Example 1, the only difference is that the positive electrode active material LiNbO3@LiCoO2 is replaced with LiNbO3@NCM622 (LiNbO3-coated NCM622, purchased from Xiamen Tungsten Industry) of the same weight to obtain a positive electrode slurry 9 and an electrode plate 9.
[0099] Example 10
[0100] Same as Example 1, except that the sulfide electrolyte Li6PS5Cl is replaced by the same weight of Li7P3S 11 , and obtain a positive electrode slurry 10 and an electrode sheet 10.
[0101] Embodiment 11
[0102] The same as Example 1, the only difference is that the mass of the modifier ethylene glycol nonylphenyl ether in Example 1 is changed to 0.78g, and the mass of the positive electrode active material LiNbO3@LiCoO2 is changed to 37.47g, to obtain a positive electrode slurry 11 and an electrode plate 11.
[0103] Example 12
[0104] The same as Example 1, the only difference is that the mass of the modifier ethylene glycol nonylphenyl ether in Example 1 is changed to 1.15g, and the mass of the positive electrode active material LiNbO3@LiCoO2 is changed to 37.10g, to obtain a positive electrode slurry 12 and an electrode plate 12.
[0105] Example 13
[0106] The same as Example 1, the only difference is that the modifier ethylene glycol nonylphenyl ether is replaced by the same weight of mono-n-dodecyl phosphate (structural formula: CAS number: 12751-23-4), wherein monododecyl phosphate has a chain structure, a relative molecular mass of 266, and a molecular main chain length of 2.7 nm, to obtain a positive electrode slurry 13 and an electrode plate 13.
[0107] Comparative Example 1
[0108] The same as Example 1, the only difference is that no modifier is added to obtain a comparative slurry 1 and a comparative electrode 1.
[0109] Comparative Example 2
[0110] The same as Example 1, the only difference is that the modifier ethylene glycol nonylphenyl ether is replaced with the same weight of dodecylbenzenesulfonic acid (CAS No.: 27176-87-0), wherein the dodecylbenzenesulfonic acid has a chain structure, a relative molecular mass of 326, and a molecular main chain length of 3.2nm, to obtain a comparative slurry 2 and a comparative electrode 2.
[0111] Comparative Example 3
[0112] The same as Example 1, the only difference is that the modifier ethylene glycol nonylphenyl ether is replaced by the same weight of ethylene glycol, the relative molecular mass of ethylene glycol is 66, and the molecular length is 0.52nm, to obtain comparative slurry 3 and comparative electrode 3.
[0113] Comparative Example 4
[0114] The same as Example 1, the only difference is that the modifier ethylene glycol nonylphenyl ether is replaced by the same weight of n-octadecane (CAS No.: 593-45-3), wherein n-octadecane has a chain structure, a relative molecular mass of 254, and a molecular main chain length of 2.3nm, to obtain a comparative slurry 4 and a comparative electrode 4.
[0115] Test Case
[0116] (1) Slurry stability test:
[0117] The positive electrode slurry and reference slurry prepared in Examples 1 to 13 and Comparative Examples 1 to 4 were placed in a 100 mL beaker and allowed to stand for 1 h. 1 mL of slurry was taken from the area close to the slurry liquid surface (upper layer), the middle layer (middle layer) and the bottom of the beaker (lower layer) with a pipette, and the mass M was weighed. The slurry was then placed in a vacuum oven at 60°C for 5 h. After being fully dried, the mass m was weighed again. The solid content of the upper / middle / lower layers of slurry was calculated as m / M×100%, and the difference in solid content of the upper / middle / lower layers was compared. The upper layer of the slurry refers to 2 / 3 of the slurry height to the slurry liquid surface, the middle layer of the slurry refers to 1 / 3 to 2 / 3 of the slurry height, and the lower layer of the slurry refers to the bottom of the cup to 1 / 3 of the slurry height.
[0118] (2) Preparation of half-cell and electrochemical performance test:
[0119] The electrochemical performance of the electrode sheet was characterized by using a powder cake-shaped half-cell with a counter electrode of lithium-indium alloy. The electrode sheets, comparative sheets and lithium-indium alloy sheets prepared in Examples 1 to 13 and Comparative Examples 1 to 4 were cut into small discs of φ15 mm, 200 mg of electrolyte powder was weighed in a glove box with an argon atmosphere, and the electrolyte powder was pressed into an electrolyte sheet using a φ15 mm mold at 120 MPa. The cut electrode disc was placed on one side of the electrolyte sheet, and a pressure of 380 MPa was applied to obtain a working electrode. The cut lithium-indium alloy sheet was placed on the other side of the electrolyte sheet as a counter electrode to assemble into a half-cell.
[0120] The half-cell assembled as a mold battery by the above method was subjected to constant current charge and discharge test using a Landian multi-channel charge and discharge test system (LAND CT2001A): the half-cell was charged to 3.7V at a constant current rate of 0.1C at room temperature, and then discharged to 2.0V at a constant current rate of 0.1C. The first discharge capacity and first charge capacity of the battery were recorded. The first-cycle discharge capacity of the half-cell can be obtained by dividing the recorded first discharge capacity by the mass of the positive electrode active material in the battery. The first-cycle efficiency (%) was calculated as follows: first charge capacity / first discharge capacity × 100%.
[0121] The test results are as follows:
[0122]
[0123]
[0124] From the above data, it can be seen that Examples 1 to 13 use the electrode slurry composition disclosed in the present invention, and the upper, middle and lower layers of the obtained electrode slurry have uniform solid content distribution, good slurry dispersibility, and no sedimentation and stratification phenomenon. The solid-state battery obtained thereby has high discharge specific capacity and first-cycle efficiency, and good cycle stability; Comparative Examples 1 to 4 do not use the electrode slurry composition disclosed in the present invention, and the upper, middle and lower layers of the obtained electrode slurry have uneven solid content distribution, and sedimentation and stratification phenomenon is prone to occur, or although the slurry does not show obvious stratification phenomenon, the discharge specific capacity and first-cycle efficiency of the obtained solid-state battery are low. Therefore, the electrode slurry composition provided by Examples 1 to 13 of the present disclosure has better performance than the composition provided by Comparative Examples 1 to 4.
[0125] Comparison of the data of Example 1 with Examples 11 and 12 shows that when the weight ratio of the modifier to the solvent used in Example 1 is 1:(70-120) and the weight ratio of the modifier to the sulfide electrolyte is 1:(25-100), the prepared electrode slurry not only has uniform solid content distribution in the upper, middle and lower layers and better dispersion, but also has a higher first-cycle discharge specific capacity of the coated electrode. This is because excessive amounts of modifiers are added in Examples 11 and 12. Although excessive amounts of modifiers can stabilize the electrode slurry, they will hinder the transmission of lithium ions or electrons between the electrode particles, causing the battery performance to deteriorate. Comparison of the data in Example 1 with that in Example 13 shows that, compared with selecting mono-n-dodecyl phosphate as a modifier, Example 1 selects a modifier that does not contain a hydroxyl group with a strong polarity, which can further improve the slurry stability, the battery's first charge capacity and efficiency, and avoid the hydroxyl groups on the polar phosphorus-containing end groups from corroding the sulfide solid electrolyte, thereby further improving the battery performance. In Comparative Example 2, dodecylbenzene sulfonic acid is selected as a modifier. Although it also plays a role in stabilizing the slurry, the battery's first charge capacity and efficiency are very low. The reason is that the polar end group of the octadecyl sulfonic acid molecule is a sulfonic acid group, which will corrode the sulfide solid electrolyte, thereby deteriorating the battery performance.
[0126] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0127] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0128] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. An electrode slurry composition, characterized in that: The electrode slurry composition comprises an electrode active material, a sulfide electrolyte, a solvent and a modifier, wherein the modifier comprises a group A and a group B; The group A is one or more selected from a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted alkyl group containing heteroatoms having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group containing heteroatoms having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group containing heteroatoms having 2 to 20 carbon atoms, and a substituted or unsubstituted aryl group containing heteroatoms having 6 to 20 carbon atoms; The substituent of the group A is selected from one or more of a halogen group, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, and an alkynyl group having 2 to 5 carbon atoms, and the heteroatom is a boron atom; The group B is selected from one or more of an alkoxy group, an ester group, a phosphorus-containing group, a silicate group, an alkoxysilane group, a titanate group and a carboxylic anhydride group; The structure of the ester group includes R is selected from a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, and a substituted or unsubstituted phenyl group having 6 to 20 carbon atoms; The weight ratio of the modifier to the solvent is 1:(70-120), and the weight ratio of the modifier to the sulfide electrolyte is 1:(25-100); The solvent is selected from organic solvents having a relative dielectric constant of less than 6; The modifier has a structure as shown in the following formula (1): (A) n -(B) m , formula (1), m represents the number of groups B, selected from 1, 2, 3 or 4. When m is greater than 1, each group B is the same or different; n represents the number of groups A, selected from 1, 2, 3 or 4. When n is greater than 1, each group A is the same or different.
2. The electrode slurry composition according to claim 1, characterized in that: The relative molecular mass of the modifier is 100-3000.
3. The electrode slurry composition according to claim 1, characterized in that: The molecules of the modifier are in a chain structure, and the length of the main chain of the molecule of the modifier is 1 to 30 nm.
4. The electrode slurry composition according to claim 1, characterized in that: The group B is selected from one or more of an alkoxy group having 1 to 40 carbon atoms, an ester group having 2 to 40 carbon atoms, a phosphate group having 1 to 40 carbon atoms, a phosphite group having 1 to 40 carbon atoms, a hypophosphite group having 1 to 40 carbon atoms, a silicate group having 1 to 40 carbon atoms, an alkoxysilane group having 1 to 40 carbon atoms, a titanate group having 1 to 40 carbon atoms, a carboxylic anhydride group having 2 to 40 carbon atoms, a phosphoric anhydride group having 1 to 40 carbon atoms, and a phosphoric acid cyclic anhydride group having 1 to 40 carbon atoms.
5. The electrode slurry composition according to claim 1, characterized in that: The group B is selected from the group consisting of the following groups: wherein x represents the number of oxygen atoms, which is selected from 0 or 1; R, R' and R" are independently selected from substituted or unsubstituted alkyl having 1 to 20 carbon atoms, substituted or unsubstituted cycloalkyl having 3 to 20 carbon atoms, substituted or unsubstituted alkenyl having 2 to 20 carbon atoms, substituted or unsubstituted alkynyl having 2 to 20 carbon atoms, and substituted or unsubstituted phenyl having 6 to 20 carbon atoms; and Z and Z' are independently selected from H, substituted or unsubstituted alkyl having 1 to 18 carbon atoms, substituted or unsubstituted cycloalkyl having 3 to 18 carbon atoms, substituted or unsubstituted alkenyl having 2 to 18 carbon atoms, substituted or unsubstituted alkynyl having 2 to 18 carbon atoms, substituted or unsubstituted phenyl having 6 to 18 carbon atoms, and substituted or unsubstituted alkoxy having 1 to 18 carbon atoms.
6. The electrode slurry composition according to claim 5, characterized in that: The substituents in R, R', R", Z and Z' are independently selected from one or more of a halogen group, a boron-containing group, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms and an alkynyl group having 2 to 5 carbon atoms.
7. The electrode slurry composition according to claim 1, characterized in that: The modifier is selected from one or more of ethylene glycol nonylphenyl ether, dioctyl ether, ethyl laurate, trioctyl phosphate, n-octanoic anhydride, 1-propyl phosphoric acid cyclic anhydride, 2-ethyl-1-hexyl titanium and dodecyltrimethoxysilane.
8. The electrode slurry composition according to claim 1, characterized in that: The solvent is selected from one or more of methylcyclohexane, heptane, toluene, xylene, trimethylbenzene, anisole, butyl butyrate and isobutyl isobutyrate.
9. The electrode slurry composition according to claim 1, characterized in that: Based on the total weight of solids in the electrode slurry, the content of the electrode active material is 50wt% to 90wt%, and the content of the sulfide electrolyte is 10wt% to 50wt%; Based on the total weight of the electrode slurry, the content of the solvent is 25wt% to 75wt%, and the content of the modifier is 0.1wt% to 5wt%.
10. An electrode plate, comprising a current collector and an electrode material layer, wherein the electrode material layer is made of the electrode slurry composition according to any one of claims 1 to 9.
11. An electrode plate, characterized in that: The electrode plate includes a current collector and an electrode material layer covering the current collector, the electrode material layer includes an electrode active material, a sulfide electrolyte and a modifier, and the modifier includes a group A and a group B; The group A is one or more selected from a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted alkyl group containing heteroatoms having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group containing heteroatoms having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group containing heteroatoms having 2 to 20 carbon atoms, and a substituted or unsubstituted aryl group containing heteroatoms having 6 to 20 carbon atoms; The substituent of the group A is selected from one or more of a halogen group, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, and an alkynyl group having 2 to 5 carbon atoms, and the heteroatom is a boron atom; The group B is selected from one or more of an alkoxy group, an ester group, a phosphorus-containing group, a silicate group, an alkoxysilane group, a titanate group and a carboxylic anhydride group; The structure of the ester group includes R is selected from a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, and a substituted or unsubstituted phenyl group having 6 to 20 carbon atoms; The weight ratio of the modifier to the sulfide electrolyte is 1:(25-100); The modifier has a structure as shown in the following formula (1): (A) n -(B) m , formula (1), m represents the number of groups B, selected from 1, 2, 3 or 4, when m is greater than 1, the groups B are the same or different; n represents the number of groups A, selected from 1, 2, 3 or 4, when n is greater than 1, the groups A are the same or different; The group A is selected from substituted or unsubstituted hydrocarbon groups having 1 to 20 carbon atoms, and substituted or unsubstituted hydrocarbon groups containing heteroatoms.
12. The electrode plate according to claim 11, characterized in that: Based on the total weight of the electrode material layer, the content of the electrode active material is 48wt% to 90wt%, the content of the sulfide electrolyte is 5wt% to 50wt%, and the content of the modifier is 0.1wt% to 5wt%.
13. The electrode plate according to claim 11, characterized in that: The group B is selected from the group consisting of the following groups: wherein x represents the number of oxygen atoms, which is selected from 0 or 1; R, R' and R" are independently selected from substituted or unsubstituted alkyl having 1 to 20 carbon atoms, substituted or unsubstituted cycloalkyl having 3 to 20 carbon atoms, substituted or unsubstituted alkenyl having 2 to 20 carbon atoms, substituted or unsubstituted alkynyl having 2 to 20 carbon atoms, and substituted or unsubstituted phenyl having 6 to 20 carbon atoms; and Z and Z' are independently selected from H, substituted or unsubstituted alkyl having 1 to 18 carbon atoms, substituted or unsubstituted cycloalkyl having 3 to 18 carbon atoms, substituted or unsubstituted alkenyl having 2 to 18 carbon atoms, substituted or unsubstituted alkynyl having 2 to 18 carbon atoms, substituted or unsubstituted phenyl having 6 to 18 carbon atoms, and substituted or unsubstituted alkoxy having 1 to 18 carbon atoms.
14. The electrode plate according to claim 13, characterized in that: The substituents in R, R', R", Z and Z' are independently selected from one or more of a halogen group, a boron-containing group, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms and an alkynyl group having 2 to 5 carbon atoms.
15. The electrode sheet according to any one of claims 11 to 14, characterized in that: The modifier is selected from one or more of ethylene glycol nonylphenyl ether, dioctyl ether, ethyl laurate, trioctyl phosphate, n-octanoic anhydride, 1-propyl phosphoric acid cyclic anhydride, 2-ethyl-1-hexyl titanium and dodecyltrimethoxysilane.
16. A solid-state battery, characterized in that: An electrode sheet comprising the electrode sheet according to any one of claims 10 to 15.