Improved method for forming thermoplastic additive manufacturing powders

By preparing thermoplastic polymer foam with a specific microstructure and crushing it at low temperature, the problems of insufficient powder fluidity and high residual stress in 3D printing are solved, efficient grinding and fluidity improvement are achieved, and the application scope of additive manufacturing is expanded. performance.

CN117222510BActive Publication Date: 2024-10-18LUMAS POLYMERS LLC
View PDF 40 Cites 0 Cited by

Patent Information

Application Number
CN202280029550.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-16
Publication Date
2024-10-18
Estimated Expiration
2042-05-16

AI Technical Summary

Technical Problem

Existing powder-based 3D printing technology causes deformation or defects due to excessive residual stress and insufficient powder fluidity when preparing large or complex parts, and the use of flow aids may limit the performance and use of the product.

Method used

By preparing a thermoplastic polymer foam with specific microstructural characteristics, including a porous polymer body with a minimum thickness of pore ribs or cell walls greater than the minimum required particle size, and cooling and pulverizing it below the embrittlement temperature of the thermoplastic polymer, the foam is formed with improved particle size. and size distribution of polymer powders, avoiding the use of glidants.

Benefits of technology

It achieves efficient grinding at a temperature significantly higher than the embrittlement temperature, reduces unnecessary small particles, improves the fluidity and uniformity of powder, reduces the defect rate of products, and expands the application scope and performance of additive manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117222510B_ABST
    Figure CN117222510B_ABST
Patent Text Reader

Abstract

The present disclosure provides a useful thermoplastic polymer powder, the method of forming the powder comprising: cooling a foam composed of thermoplastic foam to below the brittle temperature of the thermoplastic polymer, wherein the foam has an average pore size of 10 to 500 microns; and pulverizing the cooled foam to form a thermoplastic polymer powder. The method achieves efficient grinding of thermoplastic polymers with improved morphology and desired properties (such as dry powder flow without a flow aid).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to methods of forming thermoplastic powders for additive manufacturing. Background Art

[0002] Powder-based additive manufacturing methods include the following. Selective laser sintering (SLS) is a 3D printing technology that uses a laser to fuse powdered material into successive layers (see, e.g., U.S. Patent No. 5,597,589). High-speed sintering (HSS) and multi-jet fusion (MJF) 3D printing employ multi-hole jets that similarly deposit successive layers of infrared absorbing (IR absorbing) ink onto powdered material, followed by exposure to IR energy to selectively fuse the powder layers. Electrophotographic 3D printing employs a rotating photoconductor to build an object layer by layer from a substrate.

[0003] Selective Laser Sintering (SLS), Multi Jet Fusion (MJF), and High Speed ​​Sintering (HSS) 3D printing methods use the same type of free-floating, non-fixed powder bed onto which each successive layer of powder is metered, which requires dry powder flow to ensure good part integrity. They generally have the same material requirements to be compatible with the printing process, as the objects built with additive materials are subject to similar stresses, but with different heating mechanisms to obtain the molten phase. Typically, a free-body diagram of the 3D printed object can be used to determine the residual stresses expected in the printed object. This is required to successfully build the object. If the residual stresses are too high or the powder does not flow adequately, the object will deform or have unacceptable defects.

[0004] For these powder bed based 3D printers, residual stresses are typically minimized by using crystalline or semi-crystalline thermoplastic polymers that have a sufficiently large window between their melting temperature and their recrystallization temperature. Unfortunately, this limits polymers (e.g., polyamides) that have been successfully used to print large or complex parts using SLS and MJF methods, thereby limiting the usefulness of these additive manufacturing methods. Likewise, using semi-crystalline polymers that recrystallize upon heating to prepare additively manufactured articles may limit the performance of the article.

[0005] There have been examples of inducing crystallization of polymers such as polycarbonates, as described in U.S. Pat. Nos. 3,214,407 and 4,853,462; U.S. Pat. Publication No. 2021 / 0277180 and PCT Patent Publication No. WO2017 / 033146. These methods all use volatile organic solvents and separate the powder from the solvent (e.g., precipitate) to form a powder with induced crystallization. Unfortunately, the use of these solvents may limit the use of these polymer articles, for example, those that need to contact food.

[0006] Typically, cryogenic grinding and classification of the polymer is required to achieve the particle size required to allow the powder to melt and fuse into a coherent, continuous layer. Unfortunately, cryogenic grinding is an energy-intensive and laborious process. Also, due to the brittle fracture of polymer materials, the grinding process tends to result in powders with angular protrusions and excessively fine particles that must be heated and reprocessed. Due to the angularity of the particles produced by grinding and the presence of fine particles, the flow and distribution of the particles can lead to defects in the manufactured article. Therefore, flow aids are required in many cases to allow dry powder measurement of powders with the required uniformity to achieve defect-free, non-deformed additively manufactured parts.

[0007] Therefore, it is desirable to provide a method that avoids one or more problems to prepare polymer powders that can be used for additive manufacturing, such as selective laser sintering (SLS), high speed sintering (HSS), multi-jet fusion (MJF). For example, it is desirable to provide a method that does not require a flow aid to more efficiently obtain useful additive manufacturing powders. Summary of the invention

[0008] Applicants have discovered a method that allows for tailoring of particle size, size distribution, and particle morphology, and that is more efficient than existing methods for preparing thermoplastic polymer powders that can be used for additive manufacturing. The method includes forming a polymer foam (porous polymer body) having specific microstructural features that allow efficient grinding and achieving useful powder particle size, size distribution, and microstructure. It has been found that foams (porous thermoplastic polymers) having a minimum thickness of struts or cell walls greater than the minimum desired particle can be crushed more efficiently and have fewer unwanted small particles. The foam can be prepared at ambient or elevated temperatures, and the pores or cells of the foam ideally have an average size that is smaller than the average strut or cell wall size. Typically, the foam has a porosity of about 2% to 50% to achieve the desired properties and efficient grinding to form a polymer powder.

[0009] Thermoplastic polymer additive manufacturing powder can be prepared by a method comprising the steps of: cooling a foam consisting of a thermoplastic foam to below the brittle temperature of the thermoplastic polymer, wherein the foam has an average pore size of 10 to 500 microns; and pulverizing the cooled foam to form a thermoplastic polymer powder.

[0010] Thermoplastic polymer powders formed by the following methods may be sintered or melted by applying directed thermal or electromagnetic energy to produce additively manufactured articles. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 is a 300X optical micrograph of the surface of the foam used in the process of the present invention.

[0012] Figure 2 is a 100X optical micrograph of the surface of the foam used in the process of the present invention.

[0013] Figure 3 is a 200X optical micrograph of the surface of the foam used in the process of the present invention.

[0014] Figure 4 is a 200X optical micrograph of a cross section of a foam useful in the process of the present invention. DETAILED DESCRIPTION

[0015] Although the present disclosure has been described in conjunction with specific embodiments, it should be understood that the present disclosure is not limited to the disclosed embodiments, but on the contrary, the present disclosure is intended to cover various modifications and equivalent arrangements included within the scope of the appended claims, the scope of the claims will be given the broadest interpretation so as to cover all such modifications and equivalent structures permitted by law.

[0016] Surprisingly, the method can be carried out at a temperature (i.e., cooling temperature) significantly above the brittle temperature. For example, the temperature can be any temperature below the glass transition temperature of a particular polymer and ideally above the brittle temperature. The glass transition temperature (Tg) can be determined by any known method, such as those known in the art, such as differential scanning calorimetry (DSC), dynamic mechanical analysis (DMA), and thermomechanical analysis (TMA). Exemplarily, Tg can be determined by DSC from the linear deviation of the heating curve (heating rate of 20 ° C / min) using ASTM D3418 or ISO 11357-2, where Tg is the midpoint of the deviation, which is described by WJSichina in " Measurement of Tg by DSC”, PETech-09, Thermal Analysis, PerkinElmer, Inc., 2000, further described. When dense polymers are used, comminution almost always requires a temperature very close to (within ~5% of the brittle temperature expressed in degrees Kelvin) or below the brittle temperature. By using grinding at a temperature above the brittle temperature to Tg, an improved shape can be produced, and an improved morphology can be achieved at a cooling temperature close to Tg, such as within 25%, 20% or 10% of Tg expressed in degrees Kelvin. However, a lower cooling temperature near the brittle temperature (e.g., within 20% or 10% of the brittle temperature) can improve the grinding efficiency. The method generally involves cooling the thermoplastic polymer to below the glass transition temperature to its brittle temperature. The brittle temperature is as specified in ASTM D746 or ISO 974. The temperature may be further below the brittle temperature. Cooling may be performed by any suitable means, such as those known in the art of cryogenic grinding. Exemplarily, cooling may be freezing or exposure to dry ice or liquid nitrogen. Depending on the specific thermoplastic polymer and its glass transition temperature and brittle temperature, the temperature of cryogenic grinding may be any suitable temperature. Typical temperatures are any temperature below or equal to 40°C, 20°C, 0°C, -25°C, -50°C to about -75°C, -100°C, -150°C, or -190°C.

[0017] The thermoplastic polymer may be any thermoplastic polymer that can be used to prepare additively manufactured articles by a suspended bed 3D printing process, such as selective laser sintering (SLS), for example, as described in U.S. Pat. Nos. 6,136,948 and WO96 / 06881. The thermoplastic polymer may also be used to produce articles by the SIB process (selective inhibition of bonding of powders) described in WO 01 / 38061, by 3D printing as described in EP 0431924, or by the microwave process as described in U.S. Pat. No. 10,479,733.

[0018] Exemplary thermoplastic polymers include, but are not limited to, polyamides, polyesters, polycarbonates, polyketones, polysulfones, polyarylates, polyimides, polyolefins, polystyrenes, polyesters, copolymers of the above thermoplastic polymers, and blends of the above thermoplastic polymers. Thermoplastic polymers can be linear or branched. Thermoplastic polymers can be aliphatic or aromatic. It is satisfactory for thermoplastic polymers to have at least a portion of the polymer, which is composed of repeating aromatic units within the polymer backbone. Exemplarily, based on the molar amount of the polymer, 5%, 10%, 25% or 50% of the thermoplastic polymer can be aromatic (e.g., aromatic groups account for 50% or more of the molar mass of the polymer).

[0019] Thermoplastic polymers are generally composed of semi-crystalline polymers, wherein the semi-crystalline polymers exhibit at least about 5% crystallinity to substantially complete crystallinity when heated and cooled at rates generally required when forming or compounding such polymers (e.g., heating and cooling rates from ambient temperature to 25° C. to the melting temperature). That is, the polymer exhibits crystallinity without the use of forced crystallization methods such as those known in the art (e.g., solvent-induced crystallization and the like). Typically, the value of crystallinity is at least about 5%, 10%, 15%, or 20% to about 95%, 75%, 50%, or 30%. Crystallinity can be determined by any suitable method, such as those known in the art. Illustratively, the percent crystallinity can be determined by x-ray diffraction, including, for example, wide angle x-ray diffraction (WAXD), such as by using a Rigaku SmartLab x-ray diffractometer, or differential scanning calorimetry (DSC), such as by using a TA Instruments DSC250 differential scanning calorimeter using ASTM D3418-15, wherein when determining crystallinity by differential scanning calorimetry (DSC), a heating or cooling rate of 20°C / min is used unless otherwise specified. m and T c (Melting temperature and crystallization temperature) are determined by the melting / crystallization peak of DSC as described in ASTM D3418 using the midpoint of the peak. T is also determined according to ASTM D3418 or ISO 11357-2 m and the onset of the Tc peak (ie, the deviation of the scan from linearity).

[0020] As used herein, semi-crystalline includes an amorphous thermoplastic polymer having induced crystallinity that reverts to an amorphous state when heated above its melting temperature, such as described in co-pending US Application No. 63 / 289,465, which is incorporated herein by reference.

[0021] Examples of useful polycarbonates include those described in paragraphs 49 to 56 of U.S. Patent No. 2021 / 0277192, which are incorporated herein by reference.

[0022] Examples of useful polysulfones may include polyarylethersulfone (PAES), which may be represented by:

[0023]

[0024] Wherein, n is any integer value that makes the weight average molecular weight (Mw) of PAES be 1kDa, 10kDa or 20kDa to 1000kDa, 500kDa or 200kDa, m generally varies from 0 to 10, R1 represents an aromatic ring or condensed ring of about 5-10 carbon atoms each time it appears, such as but not limited to: 1,2-phenylene, 1,3-phenylene or 1,4-phenylene; or biphenyl, such as but not limited to 4,4'-biphenyl, and R2 is independently C1-C20 alkyl, C5-C18 aromatic ring or C5-C12 aromatic ring or condensed ring composed of 5-10 carbon atoms, or a combination thereof each time it appears. The fragment structure -R1-S(=O)2-R1- can also represent any one of the condensed heterocyclic structures shown in Formulas 2 and 3; and wherein at least 60% of the total number of R1 groups are aromatic, or each R2 contains at least one C6-30 aromatic group. The fragment structure -R1-S(=O)2-R1- can also represent any of the fused heterocyclic structures shown in Formulae 2 and 3:

[0025]

[0026] In one embodiment, R 1 and R 2 It can be the residue of an aryl or diaryl compound:

[0027]

[0028] In another embodiment, the PAES of formula (1) has an integer value greater than or equal to zero (typically 1 to 10, 6, 5, 4, 3 or 2), and each R 2 is the residue of a dihydroxy compound such as an aromatic dihydroxy compound:

[0029]

[0030] In formulas (3), (4) and (5), R 3 , R 4 and R 5 Each independently is, for example, but not limited to: a halogen atom (e.g., chlorine or bromine), C 3-20 Alkoxy, C 1-20 Hydrocarbyl groups (e.g., C 1-20 Alkyl, halogen substituted C 1-10 Alkyl, C 6-10 Aryl or halogen substituted C 6-10wherein p, q and r are each independently an integer from 0 to 4, such that when p, q or r is less than 4, the valence of each unsubstituted carbon of the ring is filled with hydrogen; and X represents a bridging group connecting two phenolic groups, wherein the bridging group and the hydroxy substituent of each C6 arylene group are located in the ortho, meta or para position (preferably para position) relative to each other on the C6 arylene group, and the X group is composed of, for example, a single bond, -O-, -S-, -S(=O)-, -S(=O)2- (for example, bisphenol-S), -C(=O)-, or C 1-20 The organic group may be cyclic or acyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogens, oxygen, nitrogen, sulfur, silicon, or phosphorus.

[0031] Specific dihydroxy compounds include, but are not limited to, resorcinol; 2,2-bis(4-hydroxyphenyl)propane ("bisphenol A" or "BPA", wherein in formula (3), each aromatic ring is para-substituted and X is isopropylidene); 3,3-bis(4-hydroxyphenyl)phthalimide; 2-phenyl-3,3-bis(4-hydroxyphenyl)phthalimide (also known as "N-phenylphenolphthalein bisphenol", "PPPBP" or 3,3-bis(4-hydroxyphenyl)-2-phenylisoindolin-1-one); 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane; 1,1-bis(4-hydroxy-3-methylphenyl)-3,3,5-trimethylcyclohexane (also known as "isophorone bisphenol").

[0032] Examples of suitable polyarylethersulfones may be any one or more of the following:

[0033]

[0034] Examples of useful PAES polymers are: polyethersulfone (PSU, CAS #25667-42, Formula 7), poly(1,4-phenylene-ether-ether-sulfone) (PES or PEES, CAS #28212-68-2, Formula 8), polyphenylsulfone (PPSU, CAS #25839-81-0, Formula 9), and poly(bisphenol A sulfone) (PSF, CAS #25135-51-7, Formula 10), which can be purchased, for example, from Curbel Plastics Inc., Arlington TX under the trade name RADEL, from UJU New Materials, Ltd., under the trade name PARYLS, and from Solvay Specialty Polymers USA, LLC, Alpharetta, GA under the trade name UDEL.

[0035] The crystallizable polymer may be a polyketone, including a polyketone having an ether repeating unit, such as polyetherketone, polyetheretherketone, polyetherketoneketone. Exemplary polyketones without ether repeating units may be formed by the reaction of carbon monoxide, olefin monomers in the presence of a Group 8-10 transition metal catalyst. In particular, the method may be those described in U.S. Patents Nos. 4,835,250; 4,894,435 and 5,138,032 and U.S. Patent Publication No. 2008 / 0058494, the entire contents of which are incorporated herein by reference. In particular, the method, reaction conditions and monomers are such as those described in U.S. Patent No. 5,138,032, Column 2, Line 52 to Column 5, Line 17, in particular, which are incorporated herein by reference. Such polyketones are generally composed of repeating units represented by the following formula:

[0036]

[0037] Wherein A is the residue of the olefin monomer converted into saturated hydrocarbon radical, m is from about 1 to 6, and n is at least about 2 to achieve any feasible amount of the desired number average molecular weight (Mn) that can be used for the present invention.Ideally, olefin monomer includes olefins with from 2 to 12, 8 or 6 carbons.Illustratively, olefin monomer is ethylene, or olefin monomer includes ethylene and at least one other olefin monomer such as propylene.When polyketone is the copolymer of ethylene and another olefin monomer (for example, propylene), the amount of ethylene and other olefins is as described in the 17th row of the 2nd column to the 14th row of the 3rd column of U.S. Patent No. 5,138,032.Polyketone is ideally a terpolymer of carbon monoxide, ethylene and another olefin monomer (for example, olefins of 3 to 12, 8 or 6 carbons, and particularly propylene).Such polyketone can be represented by random repeating units:

[0038]

[0039] Wherein G is the saturated residue of olefin of 3 to 12,8 or 6 carbon atoms polymerized by double bond, and x / y is at least 2 to 100 or 50 or 20.Ideally, G is propylene.Polyketone can be terminated with any useful group, such as alkyl group, hydroxyl group, ester, carboxylic acid, ether or their combination.Specific end-capping group can be produced by using solvent such as low molecular alcohol (such as methanol or water or its combination).The example of commercially available polyketone includes the polyketone that can be purchased from Hyosung, Korea with trade name POKETONE.

[0040] Typically, the polyketone may be a polyaryletherketone (PAES), such as those known in the art. Exemplarily, the PAES may be a polyetherketoneketone (PEKK), such as those known in the art, and in particular amorphous PEKK, as described in U.S. Pat. No. 10,364,349, col. 2, lines 13-55, which is incorporated herein by reference. PEKK may be prepared by known methods, such as described in U.S. Pat. Nos. 3,065,205, 3,441,538, 3,442,857, 3,516,966, 4,704,448, 4,816,556, and 6,177,518.

[0041] The polyamide may be any polyamide known in the art, and is typically semi-crystalline, as described in U.S. Pat. No. 5,391,640 at column 4, line 7 to column 5, line 22, which is incorporated herein by reference. In particular, the polyamide may be amorphous, as described in U.S. Pat. No. 5,391,640 at column 5, line 23 to column 8, line 12, which is incorporated herein by reference. Examples of conventional polyamides include polypyrrolidone (nylon 4), polycaprolactam (nylon 6), polyheptanoyl lactam (nylon 7), polycapryllactam (nylon 8), polynonanoyl lactam (nylon 9), polyundecalactam (nylon 11), polylaurolactam (nylon 12), poly(tetramethylethylenediamine-co-oxalic acid) (nylon 4,2), poly(tetramethylethylenediamine-co-adipate) (nylon 4,6), poly(tetramethylethylenediamine-co-isophthalic acid) (nylon 4,1), polyhexamethylene azelaic acid amide (nylon 6,9), polyhexamethylene sebacic acid amide (nylon 6,10), polyhexa-5-methylene isophthalamide (nylon 6,IP), polymethylene adipamide (nylon MXD6), n-dodecyl phthalamide (nylon MXD6), poly(tetramethylethylenediamine-co-oxalic acid) (nylon 4,2), poly(tetramethylethylenediamine-co-adipate) (nylon 4,6), poly(tetramethylethylenediamine-co-isophthalic acid) (nylon 4,1), polyhexamethylene azelaic acid amide (nylon 6,9), polyhexamethylene sebacic acid amide (nylon 6,10), polyhexamethylene isophthalamide (nylon 6,IP), polymethylene adipamide (nylon MXD6), n-dodecyl phthalamide (nylon MXD6), polymethylene iso ... Polyamides of tantalum dicarboxylic acid and hexamethylene diamine (nylon 6,12), polyamides of dodecamethylene diamine and n-dodecanedioic acid (nylon 12,12), and their copolymer-decamers, which include: hexamethylene adipamide-caprolactam (nylon 6,6 / 6), hexamethylene adipamide / -hexamethylene-isophthalamide (nylon 6,6 / 6IP), hexamethylene adipamide / hexamethylene-terephthalamide (nylon 6,6 / 6T), trimethylene adipamide-hexamethylene-15-nonazelamide (nylon trimethylene 6,2 / 6,2) and hexamethylene adipamide-hexamethylene-nonazelamide-caprolactam (nylon 6,6 / 6,9 / 6) and other decamers not specifically described herein.

[0042] The polyimide can be any polyimide known in the art, and desirably is a known aromatic polyimide. Illustratively, potentially suitable aromatic polyimides are described in US Pat. Nos. 3,179,631, 3,249,588, and 4,755,555, which are incorporated herein by reference.

[0043] Thermoplastic foam is a foam with an average pore-strut or bubble wall thickness of 10 to 500 microns. Any suitable technique can be used, such as an optical microscope or scanning electron microscope to a cross section of a cut or fracture, to determine average pore-strut or bubble wall thickness through a microphotograph of the cross section of foam, if desired the cross section of foam can be filled with resin. Average pore-strut or bubble wall thickness can be determined by measuring at least about 25 randomly selected bubble wall thicknesses on one or more 100X microphotographs of a cross-sectional area of ​​about 2 square millimeters of foam. Ideally, the average pore-strut size is at least 20 microns, 30 microns or 50 microns to 400 microns, 300 microns or 250 microns.

[0044] Ideally, the distribution of pore-strut or cell wall thickness can achieve the desired flow without the use of a flow aid as described below. Generally, it is desirable that the D10 pore-strut size is at least 1 micron, 5 microns, or 10 microns. The D10 pore-strut size is a size in which at least 90% of the pore-struts are larger than the D10 size determined herein. Similarly, it is desirable that the D90 pore-strut size is at most about 1 mm, 750 microns, or 500 microns.

[0045] The foam also desirably has a low porosity while achieving the desired pore-strut size, which is considered (but not limited to) to improve the efficiency of grinding thermoplastic polymers to form thermoplastic polymer powders that can be used for additive manufacturing. Exemplarily, the porosity can be at least 2%, 5%, 10% to a maximum of 70%, 60% or 50%. Porosity can be determined by any suitable method, such as those known in the art, such as by mercury, helium specific gravity method or Archimedes method (for low porosity; method AISO 18754:2020) or by measuring the mass and volume of the foam (which can be promoted by coating irregular foam to seal open pores and measuring the volume by liquid displacement). The pores of the foam can be open or closed, but it is ideally composed of open pores. Exemplarily, at least 5%, 10%, 25%, 50%, 75%, 90% or substantially all of the pores are open pores.

[0046] The cell size can be any size as long as the pore-strut size is as described herein. However, it may be advantageous for the cell size to be smaller than the pore-strut size. For example, the average cell size may be 10%, 20%, or 50% smaller than the average pore-strut size. The pore size may be determined photomicrographically in a manner similar to the determination of pore-strut size, or may be determined using mercury porosimetry.

[0047] The cross-sectional shape of the foam formed can be any useful shape, and is not limited. For example, the foam can be a small ball, symmetrical or asymmetrical microbeads, fibers (chopped), pellets, flakes, slices, cut rods and tubes and the like of any cross-sectional shape. The foam can be any effective size that can be crushed. The size of the foam can be any effective size that is crushed into the required thermoplastic polymer powder. Exemplarily, it has an average particle size of 0.5 mm to 50 mm equivalent spherical diameter. The foam can be larger than this initially, and can be reduced in size before crushing by known methods, such as cutting the extruded foam by a known cutter (such as a wire cutter or a saw). The foam can be spherical, symmetrical or asymmetrical, such as any of the above-mentioned shapes. Typically, the foam to be crushed has an equivalent spherical diameter of about 0.5 mm to 50 mm, 25 mm or 10 mm equivalent spherical diameter. The aspect ratio of the foam before crushing can be 1 or more, 1.5, 2 to 50, 75 or 100. The aspect ratio is measured from micrographs of the longest and shortest axes of randomly selected foam particles (-100) using commonly available digital vision software; or measured manually using known methods.

[0048] Thermoplastic polymer foam can be prepared by any suitable method, such as those methods known in the art. The method can be any method of applying a foaming agent or using mechanical induction foaming. Ideally, foaming is achieved by molten polymer particles, such as when precipitating from a solvent, when polymerizing to form a polymer, or when dissolving and inducing precipitation by any suitable method such as known in the art. It has been found that these foams (porous bodies) are particularly suitable for the method of the present invention, and required dry powder particle flow characteristics can be obtained without using a flow aid. That is, the powder without adding any flow aid can have at least about 0.5 g / sec, 1 g / sec or 2 g / sec to any rate (e.g. 50 g / sec) that can be actually achieved using a 15 mm nozzle The flowability (flow rate) is confirmed by the method A of ASTM D 1895.

[0049] Foams or porous bodies having the desired properties may be demonstrated by polymerization of a polymer precipitated from a reaction medium, such as described in US Pat. No. 5,138,032 at column 2, line 17 to column 3, line 14, which is incorporated herein by reference.

[0050] The foam may be formed by dissolving the thermoplastic polymer in a solvent and precipitating it from solution while providing sufficient agitation or introducing a blowing agent (eg, a chemical or physical blowing agent). Air or any gaseous component of air may be used.

[0051] Exemplarily, the foam can be prepared by heating the thermoplastic polymer dissolved in the solvent. Typically, heating is above 50°C to below the initial melting temperature of the thermoplastic polymer to form a solution consisting of dissolved thermoplastic polymers. Typically, the solvent is heated to a temperature above 100°C to below the initial melting temperature of the specific thermoplastic polymer, which is measured by differential scanning calorimetry (DSC) as described herein. Exemplarily, the solvent is heated to a temperature above 75°C or 100°C to a temperature 5%, 10% or 20% lower than the initial melting temperature of the thermoplastic polymer, with examples being up to about 200°C, 180°C, 170°C or 160°C.

[0052] The time at which the maximum heating temperature (dissolution temperature) occurs is any time (usually from 3 or 4 minutes to 3 or 4 hours) to achieve the desired dissolution of the thermoplastic polymer. More than one temperature increase can be used (maintained) in the process. For example, a higher temperature can be used to dissolve the thermoplastic polymer (dissolution temperature), and a lower temperature (precipitation temperature) can be used when the thermoplastic polymer is precipitated. The precipitation temperature is the temperature at which the thermoplastic polymer begins to precipitate when cooled or the temperature at which precipitation is initiated by adding a non-solvent. The precipitation temperature can be from ambient temperature to 20°C above ambient temperature to the dissolution temperature (when precipitation is performed by adding a non-solvent), to any temperature below the dissolution temperature (for example, to 130°C, 125°C, 100°C, 75°C or 50°C). The precipitation temperature is ideally lower than the temperature at which the non-solvent begins to boil (the boiling temperature confirmed by DSC in a manner similar to the determination of the melting peak described herein). Stirring can be used in any part or the entire process, and shear varies according to the desired foam properties at different stages of the process.

[0053] Agitation is generally understood as the stirring of components in a liquid or pasty mixture under conditions of generating shear forces, generally using an impeller rotating in a stator to produce a flow pattern of flow and turbulence. Agitation can be any agitation useful for achieving a shear rate that results in the formation of foam or porous bodies. Once the impeller has sucked the mixture in, it subjects the mixture to a sudden change of direction and acceleration, causing the mixture to contact the walls of the stator under the action of centrifugal force, or to be forced through the holes in the stator under the action of pressure and velocity, thereby ultimately changing direction and acceleration, which can result in foaming and the inclusion of air.

[0054] Any suitable stirring method such as those known in the art may be used, including, for example, using an impeller, a magnetic stirrer, a homogenizer, a colloid mill, ultrasonic stirring, cavitation, and the like to achieve the desired shear. Examples of useful stirring may be achieved by any commercially available mixer.

[0055] Ideally, the atmosphere is any atmosphere in which the solvent and other chemicals do not react harmfully with the atmosphere. Typically, dissolution is carried out in a closed container at ambient pressure or near ambient pressure (e.g., ± 10%, ± 1% or ± 0.1% of atmospheric pressure) under applied pressure to minimize volatile losses. Boosting can be used, and boosting is desirable and necessary (e.g., using supercritical carbon dioxide) depending on the solvent. Exemplary atmospheres may include nitrogen or an inert gas (e.g., argon) or a combination thereof or air (e.g., any individual component or combination in dry air and air).

[0056] The amount of thermoplastic polymer dissolved in the solvent can be any useful amount that can subsequently precipitate from solution upon cooling, introduction of a non-solvent, or a combination thereof. Exemplarily, the amount of dissolved thermoplastic polymer can be from 1%, 5%, 10% to any practical amount (not gelled), 50%, 40%, 30% or 25% by weight.

[0057] Solvent can be any useful solvent for dissolving thermoplastic polymer, such as, polar aprotic solvent.Usually, solvent has volatility or low viscosity, which makes it easy to remove in subsequent processing steps, such as separating the precipitated thermoplastic polymer from solvent.Usually, the viscosity of solvent falls within the order of magnitude of the viscosity of water under ambient conditions (e.g., about 1 centipoise at about 20°C to 25°C and 1 atmosphere), or is similar to the viscosity at dilution temperature and pressure (e.g., supercritical fluid).That is, at the dissolution temperature, viscosity is usually less than 10 centipoise to 0.1 centipoise (cp).The volatility measured by boiling point (or boiling range) at 1 atmosphere is usually from about 30°C, 50°C or 75°C to 150°C, 200°C or 250°C.The molecular weight (weight average Mw) of solvent is usually at most about 500 g / mol, 200 g / mol or even 150 g / mol to at least about 30 g / mol. It should be understood that in some cases, the solvent may be solid at ambient conditions, but have the above boiling point temperature and useful viscosity (e.g., less than about 100 cp or 10 cp) at the elevated temperature at which dissolution occurs. Likewise, the solvent may be gaseous at ambient conditions and liquid at the dissolution temperature and pressure.

[0058] The solvent can be a mixture of solvents. As an example, the solvent can be a mixture of a liquid solvent at room temperature and another solvent that is solid at room temperature and dissolves in the liquid solvent, wherein the dissolved solvent imparts one or more desired properties (e.g., improved solubility of the thermoplastic polymer or particle formation when a non-solvent is used to precipitate the polymer from solution).

[0059] Exemplary solvents are described in paragraphs 26 to 34 of co-pending U.S. patent application filed on the same day as T. Fry and J. Eue et al., entitled " Polyketone powder for laser sintering ”, which is incorporated herein by reference. The method can also be carried out in a supercritical fluid (such as carbon dioxide as described in co-pending 63 / 289,465) at temperatures, concentrations and pressures dissolved in carbon dioxide or other solvents as previously described, whereby precipitation occurs by adding a non-solvent (if carbon dioxide or other solvent). Agitation can be varied during precipitation to promote the formation and agglomeration of particles in the desired foam. For example, during the nucleation of the precipitating particles, during the initial injection of the non-solvent, the shear may be high in intensity, then reduced to promote agglomeration of the initial precipitating particles, and then increased again to achieve the desired foam porosity and structure.

[0060] Based on the solvent and thermoplastic polymer used, the non-solvent for inducing precipitation at the precipitation temperature can be any suitable non-solvent. Exemplarily, when precipitating aliphatic polyketone, the solvent can be methyl pyrrolidone (NMP), N, N'-dimethyl propylene urea (DMPU), propylene glycol methyl ether acetate (PGMEA) or hexamethyl phosphoric triamide (HMPA), and the non-solvent can be a protic solvent, such as water, a low molecular weight alcohol (e.g., C1-C4 alcohol) or a mixture thereof. The amount of the non-solvent can be any amount necessary to induce precipitation at a given precipitation temperature, which is any amount useful for obtaining the desired precipitated thermoplastic polymer particle size, particle size distribution and morphology. Typically, the concentration of the added non-solvent can be 0.1%, 1%, 5% or 10% of the solvent and the non-solvent by volume, typically 75%, 50% or 25%.

[0061] Foam can be prepared by a phase inversion method for forming a foam / porous body. Typically, the phase inversion method includes dissolving a thermoplastic polymer in a solvent to form a spinning solution (dope), contacting the spinning solution with an anti-solvent in an amount sufficient to phase-invert the solvent and the anti-solvent, and removing the anti-solvent to form a foam. The spinning solution may have the characteristics of a paste that allows continuous formation of foam, for example, by forming an extrudate of the spinning solution and throwing it into a non-solvent, which is common when a polyimide membrane is formed to form a gas separation membrane (for example, U.S. Patent Publication No. 2015 / 0011815). Phase inversion can be performed using liquid or supercritical carbon dioxide, such as described in Part B of Volume 19, Issue 3, 2013 of Tissue Engineering.

[0062] The foam can be prepared by extruding a polymer having a chemical or physical blowing agent therein, which causes foaming when leaving the mold. The volatile liquid or gas can be carbon dioxide. Exemplary methods are described in U.S. Patents Nos. 4,824,720 and 6,284,810 and U.S. Patent Publications Nos. 2017 / 0282430 and 2005 / 0276967, all of which are incorporated herein by reference. In some cases, it has been found that thermoplastic polymer powders have a morphology that improves fluidity without the use of flow aids. Ideally, the polyketone has a sphericity sufficient to achieve the necessary independent flow. In terms of particle shape, the particle roundness that contributes to fluidity, in particular, and as obtained from a microphotograph image of a single particle, can be represented by a circular feature or roundness, where the roundness of a single particle is defined as 4πA / P 2 , where A is the area of ​​the particle and P is the perimeter of the particle, both of which are observed from a random angle. The related parameter sphericity is derived as the square root of roundness. Roundness is a numerical value greater than zero and less than or equal to one. A perfectly round particle refers to a roundness of 1.00. The table of overall roundness data is represented as follows: various roundness levels (e.g., 0.65, 0.75, 0.85, 0.90, and 0.95) are accompanied by a percentage of the overall particle sample with a roundness greater than the table value. Circularity is determined at a reliability filter level of 0.9 or 0.95. The reliability filter is a filter for removing overlapping particles in two-dimensional micrographs, which can be obtained in commercial image analysis software. Reliability is essentially the particle area (particle area) on the entire region defined by the major axis and minor axis of the particle region of the two-dimensional micrograph. Particle size and shape can be measured by any suitable method known in the art to measure particle size by diameter. In some embodiments, particle size and shape are determined by laser diffraction known in the art. For example, particle size can be determined using a laser diffractometer (such as a Microtrac S3500) with a static image analysis accessory, using PartAnSI software to analyze captured particle images. Ideally, for powders separated and classified from a reactor without further processing other than purification, at least about 65%, 70%, 80%, 95%, or 99% of the particles (by number) have a roundness of at least about 0.8, 0.85, 0.9, or 0.95.

[0063] Likewise, the method can allow for the formation of useful powders without the need for further classification or separation of undesirable small or large particles. Exemplarily, the thermoplastic polymer powders generally have a particle size and particle size distribution useful for making additive articles, and generally have an average or median particle size (D ) of about 1 micron (μm), 10 microns, 20 microns, 30 microns, or 40 microns to 150 microns, 125 microns, 110 microns, or 100 microns by volume. 50). Similarly, in order for the powder to heat and melt consistently, the powder desirably has a D of at most 300 microns, 200 microns, or 150 microns. 90 To aid flowability, the thermoplastic polymer powder desirably has a D of at least 0.1 microns, 0.5 microns, or 1 micron by volume. 10 . "D 90 ” refers to the particle size (equivalent spherical diameter) in a particle size distribution, where 90% of the particles by volume are smaller than or equal to this size; similarly, D 50 refers to the particle size (equivalent spherical diameter) in a particle size distribution where at least 50% of the particles by volume are smaller than this size, and D 10 Refers to the particle size (equivalent spherical diameter) in a particle size distribution where at least 10% of the particles by volume are smaller than this size. Particle size can be determined by any suitable method, such as those known in the art, including, for example, laser diffraction or image analysis of a photomicrograph of a sufficient number of particles (-100 to -200 particles). A representative laser diffractometer is produced by Microtrac, such as the Microtrac S3500.

[0064] Example

[0065] Embodiment 1:

[0066] The polyketone powder was prepared by a process in the manner described in US Pat. No. 5,138,032 at column 2, line 52 to column 5, line 17. The theoretical density of the flakes was about 90-99%. The glass transition temperature of the polyketone was about 27°C.

[0067] The thermoplastic foam was ground using a counter-rotating pin mill operating at 75% of maximum and gravity fed into the mill with a slight vacuum at the center discharge outlet and then added to the air flow of 1700 m 3 / h, and a classifying speed of 1100 rpm in an air classifier. The foam and the apparatus were cooled to -35°C and maintained at this temperature during the grinding of the foam. The average feed rate was 97.5 kg / hour. The average product discharge rate was 77 kg / hour, and the oversized product was recycled to the mill. By mass, 98.5% of the particles in the product were less than 106 microns. The effective product output reaching the upper size limit of less than 106 microns was 75.89 kg / hour.

[0068] Comparative Example 1:

[0069] Polyketone extrusion pellets prepared in the same manner as described in Example 1 were crushed in the same manner, except as follows. The feed pellets were substantially dense and were typically pellets of about 2 mm diameter x 2 mm long. The pellets were cooled to -40°C. The feed rate was 28.5 kg / hour. The feed was reduced due to the production of a large amount of recycled oversized material. The average discharge rate was 22 kg / hour. The product had about 34.8% of the particles by mass less than 106 microns. The total effective product reaching a particle size of less than 106 microns was about 7.6 kg / hour. From this, it is clear that even at a lower feed rate, the powder produced cannot be effectively ground to the desired size. That is, the use of the thermoplastic polymer foam of the present invention is more than 10 times more efficient in achieving the desired thermoplastic polymer powder that can be used for additive manufacturing.

[0070] Embodiment 2:

[0071] Polyetherketoneketone (PEKK) foam was ground in a counter-rotating pin mill in a similar manner as in Example 1, but at a temperature in the range of 0°C to 20% of the brittle temperature of PEKK. Figure 1-4 As shown. The typical size of the foam is irregular flakes ranging from about 100 microns to 3 mm thick. The average pore size is about 82 microns. It is easy to see from the figure that there is a significant porosity of at least 10% (i.e., less than about 90% of theoretical density). The foam is quickly ground in a manner similar to Example 1 with high efficiency and the desired particle size without significant oversized material. The polyetherketoneketone has a Tg of about 160°C, a melting temperature of about 305°C, and a T:l ratio of about 60:40.

Claims

1. A method of forming a thermoplastic polymer powder, include: (i) cooling a foam composed of a thermoplastic polymer having a glass transition temperature to a cooling temperature below the glass transition temperature, wherein the foam has an average cell strut size of 10 micrometers to 500 micrometers and an average cell size smaller than the average cell strut size to form a cooled foam, wherein the average cell size is at least 10% smaller than the average cell strut size and the foam has a porosity of 2% to 70%, and (ii) comminuting the cooled foam to form a thermoplastic polymer powder.

2. The method according to claim 1, in, The porosity is 2% to 50%.

3. The method according to claim 1, in, The average pore size of the foam is 20 micrometers to 300 micrometers.

4. The method according to claim 1, in, The foam has a D of at least 10 microns 10 Hole edge size.

5. The method according to claim 4, in, The foam has a D of at most 500 microns. 90 Hole edge size.

6. The method according to claim 1, in, The porosity is 5% to 60%.

7. The method according to claim 1, in, The average cell size is at least 20% smaller than the average cell strut size.

8. A method of forming a thermoplastic polymer powder, include: (i) cooling a foam composed of a thermoplastic polymer having a glass transition temperature to a cooling temperature below the glass transition temperature, wherein the foam has an average cell strut size of 10 micrometers to 500 micrometers and an average cell size smaller than the average cell strut size to form a cooled foam, wherein the average cell size is at least 10% smaller than the average cell strut size and the foam has a porosity of 2% to 70%, and (ii) comminuting the cooled foam to form a thermoplastic polymer powder, wherein the thermoplastic polymer powder has: (i) D less than about 150 microns 90 Particle size, (ii) D of at least 10 microns 10 and (iii) an average particle size of about 20 microns to about 150 microns, and at least 80% by number of the thermoplastic polymer powder has a roundness of at least about 0.

8.

9. The method according to claim 1, in, The foam has an average size of 0.5 mm to 50 mm equivalent spherical diameter.

10. A method of forming a thermoplastic polymer powder, include: (i) cooling a foam composed of a thermoplastic polymer having a glass transition temperature to a cooling temperature below the glass transition temperature, wherein the foam has an average cell strut size of 10 micrometers to 500 micrometers and an average cell size smaller than the average cell strut size to form a cooled foam, wherein the average cell size is at least 10% smaller than the average cell strut size and the foam has a porosity of 2% to 70%, and (ii) comminuting the cooled foam to form a thermoplastic polymer powder, wherein the foam is formed by a process comprising: The first method comprises: incorporating a blowing agent into a thermoplastic polymer at a temperature and pressure at which the thermoplastic polymer melts, and reducing the pressure sufficiently to cause the blowing agent to become gaseous, thereby forming the foam; The second method comprises: dissolving the thermoplastic polymer in a solvent to form a spinning dope, contacting the spinning dope with an anti-solvent in an amount sufficient to phase invert the solvent and the anti-solvent and removing the anti-solvent to form the foam; and The third method includes dissolving the thermoplastic polymer in a solvent to form a solution, precipitating the thermoplastic polymer by adding a non-solvent to form precipitated thermoplastic polymer particles, agglomerating the precipitated thermoplastic polymer particles to form a microparticulate foam slurry, and removing the solvent and the non-solvent to form a foam.

11. The method according to claim 1, in, The foam is formed by polymerization of the thermoplastic polymer and precipitation of the thermoplastic polymer from a reaction medium.

12. The method according to claim 10, in, The foaming agent is composed of one or more of a chemical foaming agent and a physical foaming agent.

13. A method of forming a thermoplastic polymer powder, include: (i) cooling a foam composed of a thermoplastic polymer having a glass transition temperature to a cooling temperature below the glass transition temperature, wherein the foam has an average pore-strut size of 10 micrometers to 500 micrometers and an average cell size smaller than the average pore-strut size to form a cooled foam, wherein the average cell size is at least 10% smaller than the average pore-strut size and the foam has a porosity of 2% to 70%, and the thermoplastic polymer has a brittle temperature, and the cooling temperature is below the glass transition temperature of the thermoplastic polymer and above the brittle temperature, and (ii) comminuting the cooled foam to form a thermoplastic polymer powder.

14. The method according to claim 13, in, The cooling temperature is within 20% of the embrittlement temperature.

15. The method according to claim 13, in, The cooling temperature is within 20% of the glass transition temperature.

Citation Information

Patent Citations

  • Assemblies containing polyetherketoneketone tie layers

    US10364349B1

  • Powder comprising polymer-coated core particles comprising metals, metal oxides, metal nitrides or semimetal nitrides

    US10479733B2

  • Surface textured microporous polishing pads

    US20050276967A1

  • Process for preparing polyketone

    US20080058494A1

  • Composite hollow fiber membranes useful for co2 removal from natural gas

    US20150011815A1