A kind of microcrystalline glass containing yttrium zirconate nanocrystals and preparation method
By introducing Y2O3 and ZrO2 into soda-aluminosilicate glass, yttrium-containing zirconate nanocrystals are prepared and combined with an ion exchange process, which solves the problems of brittle fracture of traditional cover glass and high cost of lithium-aluminosilicate glass, achieving high hardness and low Low-cost transparent crystallized glass is prepared to meet the needs of thinness, lightness and drop resistance.
Patent Information
- Application Number
- CN202311232221.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-22
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-09-22
AI Technical Summary
Traditional cover glass has brittle fracture problems in terms of mechanical properties, and the production cost of lithium aluminum silica-ceramic glass has increased due to the increase in the price of lithium carbonate, which restricts industrial development. Surface precipitation and poor thermal expansion of sodium aluminum silica-ceramic glass lead to devitrification and Thermal cracking makes it difficult to meet the requirements of thinness and drop resistance.
By introducing Y2O3 and ZrO2, transparent crystallized glass containing yttrium zirconate nanocrystals is prepared, and combined with the ion exchange process, the crystal precipitation in the soda-aluminosilicate glass matrix is controlled to improve the mechanical properties and transparency of the glass.
The uniform and controllable growth of yttrium zirconate nanocrystals in the glass matrix is achieved, which significantly improves the Vickers hardness and fracture toughness of the glass, reduces production costs, and avoids the problems of devitrification and thermal cracking.
Smart Images

Figure CN117228956B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of microcrystalline glass, and in particular to microcrystalline glass containing yttrium zirconate nanocrystals and a preparation method thereof. Background Art
[0002] Glass for information display is a key basic material for the electronic display industry. Screen protection glass (also known as cover glass) must not only meet the requirements of thin and light size, but also meet the requirements of mechanical properties such as drop resistance and scratch resistance. Traditional cover glass usually uses alkali-aluminosilicate glass, and its mechanical properties are enhanced by chemical strengthening of one or two steps of ion exchange, but brittle fracture is still a fatal weakness that plagues its use; therefore, the method of synergistic enhancement of microcrystallization and ion exchange (chemical strengthening) to improve the mechanical properties of glass is considered to be the most promising solution.
[0003] Transparent aluminosilicate glass-ceramics has become a hot spot in scientific research and industrial development as a new cover material for high-end electronic products due to its excellent mechanical strength and physical and chemical properties. Lithium aluminum silicon glass-ceramics is a relatively mature system currently under research. Due to its excellent mechanical and thermal properties, it is currently widely used in civil life, astronomical observation, and electronic information display. However, in recent years, with the rapid growth of demand for lithium batteries in industries such as mobile display terminals and new energy electric vehicles, the price of raw materials such as lithium carbonate has remained high, which has led to a significant increase in the production cost of lithium aluminum silicon glass-ceramics, seriously restricting industrial development.
[0004] Sodium aluminum silicate glass also has good chemical stability and mechanical strength, and one of its main components, sodium oxide, is abundant in resources, with a wide range of raw materials and low cost. At present, researchers have conducted relevant research on transparent sodium nepheline glass-ceramics, including raw materials, nucleating agents, chemical strengthening methods, etc. However, sodium nepheline usually precipitates on the surface of glass, and its own refractive index and thermal expansion coefficient are quite different from those of the base glass, which can easily lead to devitrification and thermal cracking of the glass. Therefore, the development of transparent glass-ceramics composition and chemical strengthening process research based on the sodium aluminum silicate system has important practical significance and broad application prospects. Summary of the invention
[0005] In view of the shortcomings of the existing technology, considering the ZrO 2 It is usually used to strengthen and toughen ceramic matrix or improve glass hardness. 2 As an important nucleating agent, it can be used to control the precipitation of crystals in glass. 2 O 3 The introduction of Y has an impact on the high temperature viscosity and crystallization temperature of the glass, and can refine the grains to a certain extent, thereby realizing the preparation of transparent microcrystalline glass; for this purpose, the present invention provides a microcrystalline glass containing yttrium zirconate nanocrystals and a preparation method thereof, which introduces Y2 O 3 and ZrO 2 , to achieve controllable crystallization in the sodium aluminum silicate glass matrix to prepare transparent microcrystalline glass containing yttrium zirconate nanocrystals; at the same time, it can also be combined with ion exchange technology to improve the mechanical properties of the glass.
[0006] The invention discloses a glass-ceramic containing yttrium zirconate nanocrystals, wherein the glass-ceramic comprises: a sodium aluminum silicate glass matrix, a Y 2 O 3 and ZrO 2 Among them, Al in the sodium aluminum silicate glass matrix 2 O 3 :Na 2 The molar ratio of O is ≥1, based on the total molar amount of sodium aluminum silicate glass matrix, Y 2 O 3 With ZrO 2 The sum of the molar amounts of Y is ≥ 1.5 mol%; that is, when the sum of the molar amounts of the sodium-aluminum-silicon glass matrix is 100 mol, then 2 O 3 and ZrO 2 The sum of the molar contents is greater than 1.5 mol.
[0007] As a further improvement of the present invention, the heat treatment temperature of the microcrystalline glass is 750°C to 850°C.
[0008] As a further improvement of the present invention, the composition of the microcrystalline glass comprises, in terms of mole percentage:
[0009] SiO 2 45-57%;
[0010] Al 2 O 3 15-26%;
[0011] Na 2 O 15–25%;
[0012] B 2 O 3 5-10%;
[0013] ZnO 1~3%;
[0014] Y 2 O 3 0.25~2%;
[0015] ZrO 2 1~2%.
[0016] The present invention also discloses a method for preparing glass-ceramics containing yttrium zirconate nanocrystals, comprising:
[0017] Mixing the components of the glass-ceramics to obtain a mixture;
[0018] The mixed material is sequentially melted, clarified, cast and annealed to obtain a glass sample;
[0019] The glass sample is heat-treated to obtain glass-ceramics containing yttrium zirconate nanocrystals.
[0020] As a further improvement of the present invention, the mixed material is melted at 1500-1550° C. for 4-5 hours.
[0021] As a further improvement of the present invention, the heat treatment temperature is 750° C. to 850° C., and the heat treatment time is 2 to 5 hours.
[0022] As a further improvement of the present invention, it also includes:
[0023] The prepared glass-ceramics were subjected to K + -Na + Chemical strengthening by ion exchange.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The prepared glass-ceramics of the present invention contains yttrium zirconate crystal phase, and the uniform and controllable growth of yttrium zirconate nanocrystals in the sodium-aluminum-silicon glass matrix is achieved by regulating the glass composition and the heat treatment temperature, and the precipitation of yttrium zirconate nanocrystals can promote K + -Na + The increase in the depth of the ion exchange layer significantly improves the Vickers hardness and fracture toughness of the glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the XRD pattern of the glass-ceramics containing yttrium zirconate nanocrystals prepared in Example 1 of the present invention;
[0027] Figure 2 XRD patterns of the samples prepared in Examples 1 to 6 of the present invention and heat treated at 750° C. / 2 h;
[0028] FIG3( a ) is an XRD pattern of the glass-ceramics containing yttrium zirconate nanocrystals prepared in Examples 7 to 12 of the present invention after heat treatment at 780° C. / 2 h;
[0029] FIG3( b ) is an XRD graph of the glass-ceramics containing yttrium zirconate nanocrystals prepared in Examples 13 to 16 of the present invention after heat treatment at 780° C. / 2 h;
[0030] Figure 4 Transmission electron microscope (TEM) image and element distribution map of the glass-ceramics containing yttrium zirconate nanocrystals prepared in Example 1 of the present invention;
[0031] Figure 5 The K of the sample prepared in Example 1 of the present invention was measured by electron probe microanalysis (EPMA) after chemical strengthening. + Distribution curve of ions on the sample surface;
[0032] Figure 6 is the XRD pattern of the glass of Comparative Example 1; wherein, Y 2 O 3 0mol%ZrO 2 1 mol%;
[0033] Figure 7 This is the XRD pattern of the glass of Comparative Example 2. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0036] The present invention provides a glass-ceramic containing yttrium zirconate nanocrystals. The glass-ceramic is a transparent glass-ceramic. The glass-ceramic comprises: a sodium aluminum silicate glass matrix, a Y 2 O 3 and ZrO 2 Among them, Al in the sodium aluminum silicate glass matrix 2 O 3 :Na 2 The molar ratio of O is ≥1, based on the total molar amount of sodium aluminum silicate glass matrix, Y 2 O 3 with ZrO 2 The sum of the molar amounts of Y is ≥ 1.5 mol%; that is, when the sum of the molar amounts of the sodium-aluminum-silicon glass matrix is 100 mol, then 2 O 3 and ZrO 2 The sum of the molar contents of is greater than 1.5 mol, and the heat treatment temperature is 750℃≤T≤850℃; based on this, it is ensured that yttrium zirconate nanocrystals are precipitated in the microcrystalline glass; at the same time, the composition of Na 2 O does not participate in the precipitation of nanocrystals, Na + Can be realized with K + After ion exchange is carried out and yttrium zirconate nanocrystals are precipitated, the depth of the ion exchange layer can be increased.
[0037] Specifically, in terms of mole percentage, the composition of the microcrystalline glass includes:
[0038] SiO 2 45-57%;
[0039] Al 2 O 3 15-26%;
[0040] Na 2 O 15–25%;
[0041] B 2 O 3 5-10%;
[0042] ZnO 1~3%;
[0043] Y 2 O 3 0.25~2%;
[0044] ZrO 2 1~2%.
[0045] The present invention also provides a method for preparing glass-ceramics containing yttrium zirconate nanocrystals, comprising:
[0046] Step 1, calculating the weight of the raw materials according to the molar percentage of the transparent microcrystalline glass components, weighing and mixing them to form a mixture;
[0047] Step 2, melting, clarifying, casting and annealing the mixture in sequence to obtain a glass sample; wherein the mixture is melted at 1500-1550° C. for 4-5 hours;
[0048] Step 3, heat treating the glass sample at 750° C. to 850° C. for 2 to 5 hours to obtain a glass-ceramic containing yttrium zirconate nanocrystals;
[0049] Step 4: K + -Na + Chemical strengthening by ion exchange.
[0050] Example:
[0051] The compositions of the glass-ceramics of Examples 1 to 16 are shown in Table 1, in mol;
[0052] Table 1
[0053]
[0054]
[0055] in,
[0056] The XRD pattern of the glass-ceramics containing yttrium zirconate nanocrystals prepared in Example 1 is as follows: Figure 1 As shown; the XRD patterns of the glass-ceramics containing yttrium zirconate nanocrystals prepared in Examples 1 to 6 after heat treatment at 750°C / 2h, as Figure 2 As shown; the XRD patterns of the glass-ceramics containing yttrium zirconate nanocrystals prepared in Examples 7 to 12 after heat treatment at 780°C / 2h are shown in FIG3(a); the XRD patterns of the glass-ceramics containing yttrium zirconate nanocrystals prepared in Examples 13 to 16 after heat treatment at 780°C / 2h are shown in FIG3(b); the transmission electron microscope (TEM) pattern and element distribution pattern of the glass-ceramics containing yttrium zirconate nanocrystals prepared in Example 1 are shown in FIG3(c). Figure 4 As shown; after the sample prepared in Example 1 was chemically strengthened, the K measured by electron probe (EPMA) + The distribution curve of ions on the sample surface is as follows: Figure 5 As shown. It can be seen that the glass-ceramics prepared by the present invention contains yttrium zirconate nanocrystals.
[0057] Comparative Example 1:
[0058] On the basis of Example 1, Y 2 O 3 The amount of addition was changed to 0 mol, and its XRD pattern is as follows Figure 6 As shown. It can be seen that when Y 2 O 3 +ZrO 2 If the content is less than 1.5 mol, the sample cannot precipitate yttrium zirconate nanocrystals as shown in the figure above. Yttrium oxide and zirconium oxide are the components of yttrium zirconate nanocrystals precipitated from glass, so a certain content is required to grow the nanocrystals during the heat treatment process. If the content is too low, it cannot grow through supersaturated precipitation.
[0059] Comparative Example 2:
[0060] The formula of Comparative Example 2 is shown in Table 2 below;
[0061] Table 2
[0062] Serial number <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> <![CDATA[Na 2 The]]> ZnO <![CDATA[B 2 THE 3 ]]> <![CDATA[Y 2 THE 3 ]]> <![CDATA[ZrO 2 ]]> Comparative Example 2 45.00 21.00 24.00 1.25 8.75 1.00 1.00
[0063] In this recipe, Al 2 O 3 / Na 2 The molar ratio of O is less than 1; its XRD pattern is as follows Figure 7 As shown. It can be seen that when Al 2 O 3 / Na 2 O<1, although Y 2 O 3 +ZrO 2When the concentration is 2 mol, sodium nepheline is easily precipitated on the surface, causing devitrification and cracking, and yttrium zirconate nanocrystals cannot be precipitated, thereby making it impossible to prepare transparent microcrystalline glass.
[0064] In addition, based on Example 1, when a heat treatment temperature lower than 750°C or higher than 850°C is selected, the experiment shows that if the heat treatment temperature is too low, crystallization cannot occur, and if the heat treatment temperature is too high, excessive crystallization is likely to occur, resulting in overall devitrification of the glass and failure to obtain transparent microcrystalline glass.
[0065] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A glass-ceramic containing yttrium zirconate nanocrystals, It is characterized in that The microcrystalline glass comprises: a sodium aluminum silicate glass matrix, a Y 2 O 3 and ZrO 2 Among them, Al in the sodium aluminum silicate glass matrix 2 O 3 :Na 2 The molar ratio of O is ≥1, based on the total molar amount of sodium aluminum silicate glass matrix, Y 2 O 3 with ZrO 2 The sum of the molar amounts of ≥1.5mol%; specifically: In terms of mole percentage, the composition of the microcrystalline glass includes: Not. 2 45~57%; <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 15-26% So 2 15~25% B 2 O 3 5~10%; ZnO 1~3%; AND 2 EITHER 3 0.25~2%; ZrO 2 1~2%。 2. The glass-ceramics containing yttrium zirconate nanocrystals according to claim 1, It is characterized in that The heat treatment temperature of the microcrystalline glass is 750°C to 850°C.
3. A method for preparing glass-ceramics containing yttrium zirconate nanocrystals as claimed in any one of claims 1 to 2, It is characterized in that include: Mixing the components of the glass-ceramics to obtain a mixture; The mixed material is sequentially melted, clarified, cast and annealed to obtain a glass sample; The glass sample is heat-treated to obtain glass-ceramics containing yttrium zirconate nanocrystals.
4. The method for preparing glass-ceramics containing yttrium zirconate nanocrystals according to claim 3, It is characterized in that The mixed material is melted at 1500-1550° C. for 4-5 hours.
5. The method for preparing glass-ceramics containing yttrium zirconate nanocrystals according to claim 3, It is characterized in that The heat treatment temperature is 750° C. to 850° C., and the heat treatment time is 2 to 5 hours.
6. A method for preparing glass-ceramics containing yttrium zirconate nanocrystals according to any one of claims 3 to 5, It is characterized in that Also includes: The prepared glass-ceramics were subjected to K + -Na + Chemical strengthening by ion exchange.
Citation Information
Patent Citations
Method for one-step chemical strengthening of sodium nepheline microcrystalline glass and chemically strengthened sodium nepheline microcrystalline glass
CN113149444A
Glass ceramic containing hard stone crystal phase and glass ceramic product
CN115583798A