High temperature resistant thermal radiation suppression material and preparation method
By controlling the γA/γB ratio in Gd2Zr2O7 material for doping modification, forming a composite structure, the problem of insufficient thermal radiation shielding effect of existing thermal barrier coating materials at high temperatures is solved, and the thermal radiation suppression performance is significantly improved. Aero engines with high turbine inlet temperature.
Patent Information
- Application Number
- CN202410329459.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-03-21
AI Technical Summary
现有热障涂层材料在高温环境下对热辐射的屏蔽效果不足,导致涡轮前进口温度升高时导热-辐射复合热流比增加,影响热防护效果。
AB-position co-doped gadolinium zirconate material Gd2Zr2O7 is used to control the γA/γB ratio to be doped and modified within the range of 1.465±0.005, forming a long-range and short-range ordered composite structure, and improving the spectral reflectivity of the 300nm-2500nm band. Reduce spectral transmittance.
It significantly improves the spectral reflectance of the material, effectively reduces the spectral transmittance, enhances the thermal radiation suppression performance, and is suitable for thermal protection at higher turbine inlet temperatures.
Smart Images

Figure CN118183838B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermal barrier coatings, and in particular to a high-temperature resistant thermal radiation suppression material and a preparation method thereof. Background Art
[0002] As aircraft engines and gas turbines develop towards high thrust-to-weight ratio, high thermal efficiency, low fuel consumption and long life, they are required to have higher turbine inlet temperatures. The extremely harsh high temperature environment poses a severe challenge to the performance of hot end components such as the engine's fuel nozzle, combustion chamber and blades. The current turbine inlet temperature can no longer meet the development needs of aircraft engines with higher thrust-to-weight ratios. Thermal barrier coatings (TBCs), as one of the key thermal protection technologies applied to hot end components of engines, are known as the three key technologies for manufacturing high-performance aircraft engine turbine blades, along with high-temperature structural materials and efficient blade cooling technology. Thermal barrier coatings can effectively reduce the effects of high-temperature gas on thermal damage to metal substrates such as turbine blades, and are currently the only practical and effective way to improve the thrust-to-weight ratio and thermal efficiency of both aircraft.
[0003] As the temperature of the front inlet of the aircraft engine turbine continues to increase, radiation heat conduction has become another major problem affecting the thermal protection effect of thermal barrier coating materials. According to the Stefan-Boltzmann law, as the temperature increases, the thermal radiation energy is positively correlated with the fourth power of the temperature. When the temperature is above 1700°C, the thermal conductivity-radiation composite heat flux is about 30% higher than the thermal conductivity heat flux alone. At present, the most widely used thermal barrier coating ceramic material is yttria partially stabilized zirconia (8YSZ). At high temperatures, its thermal radiation characteristics in the visible light-infrared band (wavelength 0.3μm-8μm) are translucent, and it has almost no shielding effect on thermal radiation. According to Planck's law, when the temperature is 1500℃, more than 90% of the electromagnetic waves emitted by the black body are concentrated in the wavelength band of λ<6μm. According to Wien's displacement law, as the temperature increases, the peak wavelength of the radiation will move to the short wavelength band. For example, at 1000℃, the peak wavelength of the black body's radiation intensity is 2.26μm, at 1600℃ it is 1.55μm, and at 1700℃ it is 1.47μm. Studies have shown that when the combustion chamber gas temperature of an aircraft engine is in the range of 1700K-2000K, 95% of the electromagnetic waves radiated in the combustion chamber are in the 0.5μm-9.5μm band. As a typical porous ceramic dielectric material, thermal barrier coatings have the same properties as light when passing through the coating medium, and spectral reflection, absorption and transmission phenomena will occur on the surface and inside of the coating. The spectral reflectance and spectral transmittance in the coating can be measured by a UV-IR spectrometer and corresponding integrating sphere accessories.
[0004] It is reported that the turbine inlet temperature of the sixth-generation advanced aircraft engine is expected to reach 2400-2600K, when the proportion of thermal conduction-radiation composite heat flux will increase rapidly. Therefore, the design and development of new high-temperature resistant thermal barrier coating materials with thermal radiation suppression is crucial to further improve the thermal protection effect of the coating at higher turbine inlet temperatures. Summary of the invention
[0005] The first object of the present invention is to provide a high temperature resistant thermal radiation suppression material to solve the existing technical problem of low spectral reflectivity and high transmittance.
[0006] The high temperature heat radiation resistant suppression material provided by the present invention is AB co-doped gadolinium zirconate - A2B2O7, wherein A includes gadolinium located at the A position and the A co-doping element, and B includes zirconium located at the B position and the B co-doping element; in the AB co-doped gadolinium zirconate; γ A / γ B =1.465±0.005; A is the sum of the products of the ionic radius and the molar proportion of each element at the A position; the γ B It is the sum of the products of the ionic radius and molar proportion of each element at the B position.
[0007] The beneficial effects brought by the high temperature resistant heat radiation suppression material of the present invention are:
[0008] Controlling γ by co-doping Gd2Zr2O7 at A and B sites A / γ B The ratio is in the range of 1.465±0.005, which makes the crystal structure of the doped and modified Gd2Zr2O7 material near the critical value of the pyrochlore structure and the defective fluorite structure. At this time, the material includes a composite structure of long-range order and short-range order on the one hand, and a composite structure of lattice distortion caused by the coexistence of substitutional doping and interstitial doping on the other hand. The combined effect leads to a significant increase in the spectral reflectivity of the doped and modified Gd2Zr2O7 material in the 300nm-2500nm band, and an effective reduction in the spectral transmittance.
[0009] In an optional technical solution, the A-site co-doping element and the B-site co-doping element are any combination of one or more transition elements.
[0010] Among the optional technical solutions, γ Zr is the ionic radius of the zirconium ion; γ Gd is the ionic radius of the gadolinium ion;
[0011] The ionic radius of the A-site co-doping element is larger than γ Gd The ionic radius of the B-site co-doping element is also larger than γ Zr;
[0012] Alternatively, the ionic radius of the A-position co-doping element is smaller than γ Gd The ionic radius of the B-site co-doping element is also smaller than that of γ Zr .
[0013] The second object of the present invention is to provide a preparation method to solve the technical problem of low spectral reflectance and high transmittance.
[0014] The preparation method provided by the present invention is used to prepare the above-mentioned high temperature resistant thermal radiation suppression material, and the preparation method comprises:
[0015] Selecting the A-site co-doping element and the B-site co-doping element;
[0016] According to γ A / γ B The ratio of each element is determined by the ratio of each element.
[0017] According to the A-position co-doping element, the B-position co-doping element and the doping ratio of each element, the chemical formula of the doping-modified material is obtained, the raw materials are weighed according to the chemical formula of the doping-modified material, and the high-temperature resistant thermal radiation inhibition material is synthesized by a powder synthesis method.
[0018] The above-mentioned high-temperature resistant thermal radiation suppression material can be prepared by the above-mentioned preparation method. Accordingly, the preparation method has all the advantages of the above-mentioned high-temperature resistant thermal radiation suppression material, which will not be described in detail here.
[0019] In an optional technical solution, the raw materials are oxides, inorganic salts, and organic salts of the zirconium, gadolinium, the A-site co-doping element, and the B-site co-doping element.
[0020] In an optional technical solution, at least one of the inorganic salts of the zirconium, the gadolinium, the A-site co-doping element and the B-site co-doping element is a nitrate or a chloride.
[0021] In an optional technical solution, at least one of the organic salts of the zirconium, the gadolinium, the A-site co-doping element and the B-site co-doping element is an acetate.
[0022] In an optional technical solution, the powder synthesis method is selected from one of the solid phase synthesis method, chemical coprecipitation method or sol-gel method. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the background technology, the drawings required for use in the embodiments or the background technology description will be briefly introduced below. Obviously, the drawings in the following description are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0024] Figure 1 A schematic flow chart of a method for preparing a high temperature resistant thermal radiation suppression material according to an embodiment of the present invention;
[0025] Figure 2 The XRD spectrum of the Yb and Hf co-doped Gd2Zr2O7 ceramic material prepared in Example 1 of the present invention;
[0026] Figure 3 A schematic diagram of the spectral reflectance of the Yb and Hf co-doped Gd2Zr2O7 ceramic material prepared in Example 1 of the present invention;
[0027] Figure 4 A schematic diagram of the spectral transmittance of the Yb and Hf co-doped Gd2Zr2O7 ceramic material prepared in Example 1 of the present invention;
[0028] Figure 5 The XRD spectrum of the Yb, Hf and Ti ternary co-doped Gd2Zr2O7 ceramic material prepared in Example 3 of the present invention;
[0029] Figure 6 A schematic diagram of the spectral reflectance of the Yb, Hf, and Ti co-doped Gd2Zr2O7 ceramic material prepared in Example 3 of the present invention;
[0030] Figure 7 This is a schematic diagram of the spectral transmittance of the Yb, Hf and Ti co-doped Gd2Zr2O7 ceramic material prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0031] The high temperature resistant thermal radiation suppression material provided by the embodiment of the present invention is AB co-doped gadolinium zirconate - A2B2O7, A includes gadolinium at the A position and the A co-doping element, B includes zirconium at the B position and the B co-doping element; AB co-doped gadolinium zirconate; γ A / γ B =1.465±0.005;γ A is the sum of the products of the ionic radius and molar proportion of each element at the A position; γ B It is the sum of the products of the ionic radius and molar proportion of each element at the B position.
[0032] Among them, for the γ in the present invention A The calculation of γB The calculation of can be referred to γ A The combination of the product of the ionic radius and molar proportion of each element at the A position indicates that: Taking the A position with two elements, gadolinium and element A, as an example, γ A =γ Gd *Molar ratio of gadolinium + gamma 甲 * The molar ratio of element A, that is, the ionic radius of gadolinium multiplied by the molar ratio of gadolinium in all elements at position A, is multiplied to obtain a product, and the ionic radius of element A multiplied by the molar ratio of element A in all elements at position A is multiplied to obtain another product, and then the two products are added to obtain γ A .
[0033] For example, the A position has three elements: gadolinium, element A and element B. A =γ Gd *Molar ratio of gadolinium + gamma 甲 *Molar ratio of element A+γ 乙 * The molar ratio of element B, that is, the ionic radius of gadolinium multiplied by the molar proportion of gadolinium in all elements at position A, is multiplied by the ionic radius of element A multiplied by the molar proportion of element A in all elements at position A, and another product is obtained by multiplying the ionic radius of element B multiplied by the molar proportion of element B in all elements at position A, and then adding the three products together to obtain γ A . And so on.
[0034] Controlling γ by co-doping Gd2Zr2O7 at A and B sites A / γ B The ratio is in the range of 1.465±0.005, which makes the crystal structure of the doped and modified Gd2Zr2O7 material near the critical value of the pyrochlore structure and the defective fluorite structure. At this time, the material includes a composite structure of long-range order and short-range order on the one hand, and a composite structure of lattice distortion caused by the coexistence of substitutional doping and interstitial doping on the other hand. The combined effect leads to a significant increase in the spectral reflectivity of the doped and modified Gd2Zr2O7 material in the 300nm-2500nm band, and an effective reduction in the spectral transmittance.
[0035] The following examples are given to specifically illustrate the preparation method of the high temperature resistant thermal radiation suppression material of the present application:
[0036] In the following embodiments, the γ A , γ B and γ A / γ B ratio, and then powder synthesis, ceramic block preparation, material performance testing and other processes to verify the γ A / γB The change in the ratio leads to periodic changes in the crystal structure and spectral properties of the material, indicating that γ A / γ B The ratio is optimal in the range of 1.465±0.005. It should be noted that in actual operation, the sequence of each step is not limited to the following expression, as long as the prepared material γ A / γ B The ratio is within the range of 1.465±0.005, and the material doping forms include coexistence of substitutional doping and interstitial doping.
[0037] Embodiment 1:
[0038] In this embodiment, the high temperature resistant thermal radiation suppression material prepared is a ceramic material, specifically (Gd 0.9375 Yb 0.0625 )2(Zr 0.8125 Hf 0.1875 )2O7, the main process is as follows:
[0039] Table 1 is the γ-ray diffraction patterns of Yb and Hf co-doped Gd2Zr2O7 ceramic materials prepared in Example 1 of the present invention. A With γ B Ionic radius and γ A / γ B As shown in Table 1, determine the doping ratio of each element: select Yb and Hf to dope the A and B positions of Gd2Zr2O7 material respectively, and calculate the ionic radius γ of the A position A and the B-site ionic radius γ B , calculated (Gd 0.9375 Yb 0.0625 )γ of 2Zr2O7 material A / γ B The ratio is 1.4566, with the B position Hf 4+ The incorporation of γ A / γ B The ratio gradually increases, γ A / γ B When the ratio increases to 1.4604, the chemical formula of the material is (Gd 0.9375 Yb 0.0625 )2(Zr 0.8125 Hf 0.1875 )2O7.
[0040] Table 1
[0041] serial number Element <![CDATA[γ A / nm]]> <![CDATA[γ B / nm]]> <![CDATA[γ A / c B ]]> GZO <![CDATA[Gd2Zr2O7]]> 0.1053 0.072 1.4625 GYZO <h2 style=";text-align:left;direction:ltr"><![CDATA[(Gd <h2 style=";text-align:left;direction:ltr"> 0.9375 <h2 style=";text-align:left;direction:ltr"> Yb<h2 style=";text-align:left;direction:ltr"> 0.0625 <h2 style=";text-align:left;direction:ltr"> )2Zr2O7]]><h2 style=";text-align:left;direction:ltr"> 0.104875 0.072 1.4566 1GYZHO <h2 style=";text-align:left;direction:ltr"><![CDATA[(Gd <h2 style=";text-align:left;direction:ltr"> 0.9375 <h2 style=";text-align:left;direction:ltr"> Yb<h2 style=";text-align:left;direction:ltr"> 0.0625 <h2 style=";text-align:left;direction:ltr"> )2(Zr<h2 style=";text-align:left;direction:ltr"> 0.9375 <h2 style=";text-align:left;direction:ltr"> Hf<h2 style=";text-align:left;direction:ltr"> 0.0625 <h2 style=";text-align:left;direction:ltr"> )2O7]]><h2 style=";text-align:left;direction:ltr"> 0.104875 0.0719375 1.45786 2G <h2 style=";text-align:left;direction:ltr"><![CDATA[(Gd <h2 style=";text-align:left;direction:ltr"> 0.9375 <h2 style=";text-align:left;direction:ltr"> Yb<h2 style=";text-align:left;direction:ltr"> 0.0625 <h2 style=";text-align:left;direction:ltr"> )2(Zr<h2 style=";text-align:left;direction:ltr"> 0.875 <h2 style=";text-align:left;direction:ltr"> Hf<h2 style=";text-align:left;direction:ltr"> 0.125 <h2 style=";text-align:left;direction:ltr"> )2O7]]><h2 style=";text-align:left;direction:ltr"> 0.104875 0.071875 1.45913 3GZ <h2 style=";text-align:left;direction:ltr"><![CDATA[(Gd <h2 style=";text-align:left;direction:ltr"> 0.9375 <h2 style=";text-align:left;direction:ltr"> Yb<h2 style=";text-align:left;direction:ltr"> 0.0625 <h2 style=";text-align:left;direction:ltr"> )2(Zr<h2 style=";text-align:left;direction:ltr"> 0.8125 <h2 style=";text-align:left;direction:ltr"> Hf<h2 style=";text-align:left;direction:ltr"> 0.1875 <h2 style=";text-align:left;direction:ltr"> )2O7]]><h2 style=";text-align:left;direction:ltr"> 0.104875 0.0718125 1.4604
[0042] Preparation of raw material powder: The raw material powders are Gd2O3, ZrO2, Yb2O3, HfO4, and the purity is ≥99.9%. The powder is first heat treated at 1000°C for 2 hours before use.
[0043] Powder synthesis: weigh the powder according to the chemical formula ratio, put the weighed powder into a grinding jar, add zirconium oxide grinding media into the jar, the ball-to-material ratio is 5:1, and then add solvent into the grinding jar to ensure that the solid content of the slurry is 50%. Turn on the ball mill, set the speed to 160 rpm, and grind for 10 hours. Put the ground slurry into a 120°C oven and bake for 24 hours. The dried powder is heat treated at 1400°C for 5 hours, and then sieved through a 150-mesh sieve for standby use.
[0044] Material performance testing: After the synthetic powder is formed, XRD (X-ray diffraction) and UV-infrared spectroscopy tests are performed.
[0045] Figure 2 is the XRD pattern of the above materials, such as Figure 2 As shown, with Yb 3+ , Hf 4+ As the doping amount increases, the diffraction peak shifts to a small angle first and then to a large angle, indicating that substitutional doping is dominant in the early stage of doping. As the doping amount increases, substitutional doping and interstitial doping coexist, among which γ A / γ B When the ratio is 1.4604, substitutional doping and interstitial doping coexist, which is near the critical value of pyrochlore structure and defective fluorite structure.
[0046] Figure 3 is a schematic diagram of the spectral reflectance of the above materials; Figure 4 is a schematic diagram of the spectral transmittance of the above materials; Figure 3 and Figure 4 The horizontal axis is the wavelength, Figure 3 The ordinate is the reflectivity, Figure 4 The vertical axis is the transmittance. Figure 3 , Figure 4 As shown, after doping γ A / γ B The spectral reflectivity of the material with a ratio of 1.4604 is significantly improved, and the spectral transmittance is significantly reduced. Compared with the Gd2Zr2O7 substrate, the spectral reflectivity is increased by about 10.6 percentage points, and the spectral transmittance is reduced by about 6 percentage points.
[0047] Embodiment 2:
[0048] The materials prepared in this embodiment are the same as those in Example 1, and the difference from Example 1 is the selection of raw materials and the powder synthesis method. The powder synthesis method of this embodiment is a chemical coprecipitation method. Specifically, the raw materials used are Gd(NO3)3·6H2O, Yb(NO3)3·5H2O, Zr(NO3)4·5H2O, HfCl4 and ammonia water. The raw materials are weighed in proportion, dissolved in water and stirred thoroughly, and the mixed solution is slowly added to a beaker containing ammonia water while stirring vigorously. During the whole process, the pH value of the system is controlled to be above 10 to completely precipitate. The precipitate is washed with deionized water and filtered at a pH value of about 7. The filtered precipitate is dried in an oven at 120°C for more than 12 hours, and then loaded into an alumina crucible and sintered at 1400°C for 5 hours to obtain the target powder.
[0049] Embodiment 3:
[0050] The high temperature resistant thermal radiation suppression material prepared in this embodiment is a ceramic material, specifically (Gd 0.875 Yb 0.125 )2(Zr 0.875 Hf 0.0625 Ti 0.0625 )2O7, the main process is as follows:
[0051] Table 2 is the γ-ray diffraction patterns of Yb, Hf and Ti co-doped Gd2Zr2O7 ceramic materials prepared in Example 3 of the present invention. A With γ B Ionic radius and γ A / γ B As shown in Table 2, determine the doping ratio of each element: select Yb, Hf, and Ti to dope the A and B positions of Gd2Zr2O7 materials respectively, and calculate the ionic radius γ of the A position A and the B-site ionic radius γ B , calculated (Gd 0.875 Yb 0.125 )2(Zr 0.875 Hf 0.0625 Ti 0.0625 )2O7 materials A / γ B The ratio is 1.46661, and γ is designed for comparison performance. A / γ B Materials with other doping ratios near 1.46661.
[0052] Table 2
[0053]
[0054]
[0055] Preparation of raw material powder: The raw material powders are selected from Gd2O3, ZrO2, Yb2O3, HfO4, and TiO2 oxide powders with a purity of ≥99.9%. The powders are first heat treated at 1000°C for 2 hours before use.
[0056] Powder synthesis: weigh the powder according to the chemical formula ratio, put the weighed powder into a grinding jar, add zirconium oxide grinding media into the jar, the ball-to-material ratio is 5:1, and then add solvent into the grinding jar to ensure that the solid content of the slurry is 50%, turn on the ball mill, set the speed to 160rpm, and grind for 10 hours. Put the ground slurry into a 120℃ oven and bake for 24 hours. The dried powder is heat treated at 1400℃ for 5 hours, and then sieved through a 150-mesh sieve for use.
[0057] Material performance testing: After the synthetic powder is formed, XRD and UV-IR spectroscopy tests are performed.
[0058] Figure 5 is the XRD pattern of the above materials, such as Figure 5 As shown, with Yb 3+ , Hf 4+ 、Ti 4+ As the doping amount increases, the diffraction peak shifts to a small angle first and then to a large angle, indicating that substitutional doping is dominant in the early stage of doping. As the doping amount increases, substitutional doping and interstitial doping coexist, among which γ A / γ B When the ratio reaches 1.46661, the material becomes a coexistence of substitutional doping and interstitial doping, which is near the critical value between the pyrochlore structure and the defective fluorite structure.
[0059] Figure 6 is a schematic diagram of the spectral reflectance of the above materials; Figure 7 is a schematic diagram of the spectral transmittance of the above materials; Figure 6 and Figure 7 The horizontal axis is the wavelength, Figure 6 The ordinate is the reflectivity, Figure 7 The vertical axis is the transmittance. Figure 6 , Figure 7 As shown, after doping γ A / γ B The spectral reflectivity of the material with a ratio of 1.46661 is significantly increased, and the spectral transmittance is significantly reduced, which is similar to the γ A / γ B Compared with 3GYZHTO and 5GYZHTO materials with similar ratios, the spectral reflectance increases by about 12.9 percentage points and 11.5 percentage points, and the spectral transmittance decreases by about 9.8 percentage points and 11.4 percentage points.
[0060] Embodiment 4:
[0061] The difference between this embodiment and embodiment 3 lies in the selection of raw materials and the powder synthesis method. The powder synthesis method of this embodiment is the sol-gel method. Specifically, the raw materials used are Gd(NO3)3·6H2O, Yb(NO3)3·5H2O, Zr(NO3)4·5H2O, HfCl4, Ti(OC3H7)4, citric acid and ammonia water. After weighing the raw materials, dissolve them with deionized water, mix them with citric acid in a ratio of 2:3, stir them evenly, adjust the pH value of the solution to about 9 with ammonia water, and then heat the solution to 80°C. Stir continuously during the process until the solution is in a gel state. Let the gel stand at room temperature for 12 hours to become a dry gel, dry it in an oven at 120°C for more than 12 hours, and then put it into an alumina crucible and sinter it at 1400°C for 5 hours to obtain the target powder.
[0062] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
[0063] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the term "comprises" or any other variant thereof is intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprises a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0064] In the above embodiments, the descriptions of directions such as “upper” and “lower” are all based on the drawings.
[0065] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0066] Thus, the present invention will not be limited to the embodiments shown herein but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A high temperature resistant heat radiation suppression material, characterized in that: The high temperature resistant thermal radiation suppression material is AB co-doped gadolinium zirconate - A2B2O7, wherein A includes gadolinium at the A position and the A co-doping element, and B includes zirconium at the B position and the B co-doping element; in the AB co-doped gadolinium zirconate; γ A / γ B =1.465±0.005; A is the sum of the products of the ionic radius and the molar proportion of each element at the A position; the γ B is the sum of the products of the ionic radius and molar proportion of each element at the B position; the ionic radius of the co-doped element at the A position is smaller than γ Gd , the ionic radius of the B-site co-doping element is smaller than γ Zr , the doping ions at the A and B positions need to coexist in the material to form substitutional doping and interstitial doping.
2. The high temperature resistant heat radiation suppression material according to claim 1, characterized in that: The A-site co-doping element and the B-site co-doping element are any combination of one or more transition elements.
3. A preparation method for preparing the high temperature resistant heat radiation suppression material according to claim 1, characterized in that: The preparation method comprises: Selecting the A-site co-doping element and the B-site co-doping element; According to γ A / γ B The ratio of each element is determined by the ratio of each element. According to the A-position co-doping element, the B-position co-doping element and the doping ratio of each element, the chemical formula of the doping-modified material is obtained, the raw materials are weighed according to the chemical formula of the doping-modified material, and the high-temperature resistant thermal radiation suppression material is synthesized by a powder synthesis method.
4. The preparation method according to claim 3, characterized in that: The raw materials are oxides, inorganic salts and organic salts of the zirconium, gadolinium, the A-site co-doping element and the B-site co-doping element.
5. The preparation method according to claim 3, characterized in that: At least one of the inorganic salts of the zirconium, the gadolinium, the A-site co-doping element, and the B-site co-doping element is a nitrate or a chloride.
6. The preparation method according to claim 3, characterized in that: At least one of the organic salts of the zirconium, the gadolinium, the A-site co-doping element and the B-site co-doping element is an acetate.
7. The preparation method according to claim 4, characterized in that: The powder synthesis method is selected from one of a solid phase synthesis method, a chemical coprecipitation method or a sol-gel method.