A low-temperature vibration-damping epoxy resin, its synthesis method, and its applications

By synthesizing linear aliphatic epoxy resins with oxygen atoms in the main chain and curing agents, the problem of high brittleness of bisphenol A type epoxy resins at low temperatures was solved, and the flexibility and vibration resistance of electrostatic discharger insulation materials at low temperatures were achieved.

CN117229479BActive Publication Date: 2026-11-17LIAONING NORMAL UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311089873.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-28
Publication Date
2026-11-17
Estimated Expiration
2043-08-28

AI Technical Summary

Technical Problem

Traditional bisphenol A type epoxy resin is brittle at low temperatures, which makes the insulating material of electrostatic dischargers prone to breakage or cracking under low-temperature vibration environment.

Method used

A low-temperature vibration-resistant epoxy resin is synthesized through a specific chemical reaction using linear aliphatic epoxy resin adhesive containing oxygen atoms in the main chain and a linear aliphatic diamine curing agent. The epoxy resin molecular chain is designed to avoid rigid groups restricting the movement of the molecular chain, and the number of oxygen atoms is increased to improve low-temperature flexibility.

Benefits of technology

In low-temperature environments, epoxy resin exhibits excellent flexibility and vibration resistance, preventing breakage or cracking and ensuring the stable operation of the electrostatic discharger.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure BDA0004417360150000011
    Figure BDA0004417360150000011
Patent Text Reader

Abstract

This invention discloses a low-temperature vibration-resistant epoxy resin, its synthesis method, and its application. The low-temperature vibration-resistant epoxy resin includes a linear aliphatic epoxy resin adhesive with oxygen atoms in its main chain and a linear aliphatic diamine curing agent. The linear aliphatic molecular chain used effectively avoids the restriction of molecular chain movement by rigid groups. Furthermore, by introducing more oxygen atoms into the molecular main chain, the low-temperature mobility of the molecular chain is maximized, thereby maximizing its low-temperature flexibility. Further still, based on the same design concept, a linear aliphatic diamine is synthesized in conjunction with the epoxy resin curing agent, thus giving the cured epoxy resin good molecular mobility. This effectively solves the problem of insufficient low-temperature flexibility of current bisphenol A type epoxy resins, which leads to the fragility or cracking of insulating rods for electrostatic dischargers used in launch vehicles made from them under low-temperature vibration environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to insulating materials for electrostatic dischargers in launch vehicles, specifically an epoxy resin with good low-temperature flexibility. Background Technology

[0002] Before launch, during the fuel and oxidizer loading process, especially the loading of cryogenic insulating liquids such as liquid oxygen and liquid hydrogen, the high-speed flow of these liquids in the pipelines generates static electricity of up to hundreds of thousands of volts, which can easily lead to electrostatic discharge, posing a significant threat to rocket safety. To protect rocket operation, an electrostatic discharger installed at the rocket's tail end releases the static electricity into the atmosphere.

[0003] Typically, electrostatic dischargers are mounted on the outside of pipes via metal supports. These dischargers are made of insulating material, usually thermosetting resin. During liquid oxygen refueling, even in environments above freezing, the internal temperature of the insulating material can still reach approximately -40°C; during liquid hydrogen refueling, the internal temperature can reach approximately -90°C. Such low temperatures place stringent requirements on the insulating material, as conventional insulating materials would rapidly crumble in such environments, and the vibrations generated during the flow of liquid oxygen or hydrogen would exacerbate this cracking.

[0004] Traditional electrostatic discharger insulation materials are generally made of bisphenol A type epoxy resin, as shown in the following molecular structure formula. This molecular structure containing bisphenol A has high rigidity, which is not conducive to molecular chain movement, so it has very high brittleness at low temperatures.

[0005] Summary of the Invention

[0006] In view of this, the present invention provides a low-temperature vibration-resistant epoxy resin, which solves the problem that the low-temperature flexibility of the current bisphenol A type epoxy resin is insufficient, so that the insulating rod of the electrostatic discharger for launch vehicles made from it is easily broken or cracked in low-temperature vibration environment.

[0007] In addition, the present invention also provides a method for synthesizing the low-temperature vibration-resistant epoxy resin and its application.

[0008] In a first aspect, the low-temperature vibration-resistant epoxy resin of the present invention comprises:

[0009] Linear aliphatic epoxy resin adhesives with oxygen atoms in the main chain and linear aliphatic diamine curing agents.

[0010] In this disclosure and possible embodiments, the molecular structural formula of the epoxy resin adhesive is:

[0011]

[0012] In this disclosure and possible embodiments, the molecular formula of the curing agent is:

[0013] H2N-CH2-CH2-CH2-O-CH2-CH2-O-CH2-CH2-CH2-NH2.

[0014] Secondly, the method for synthesizing the low-temperature vibration-resistant epoxy resin described in the first aspect includes synthesizing a linear aliphatic epoxy resin adhesive whose main chain contains oxygen atoms, the synthesis method comprising:

[0015] The diol is generated by chain extension reaction of 3-bromo-1-propanol and disodium ethylene glycol, and the epoxy resin is generated by reaction of the diol with epichlorohydrin.

[0016] In this disclosure and possible embodiments, the disodium ethylene glycol is dissolved in ethylene glycol to obtain a solution with a mass concentration of 10-20%. 3-bromo-1-propanol is added dropwise to the solution under stirring at a rate of 240-360 min, with the total molar amount added being 2.2 times the molar amount of the disodium ethylene glycol. The stirring speed is 30-60 r / min, and the temperature of the reaction system is controlled at 80±1℃. After the reaction is completed, ethylene glycol is separated to obtain the diol.

[0017] In this disclosure and possible embodiments, a suspension polymerization method is used. Epichlorohydrin and diethyl ether are prepared into a solution, and the diol is added dropwise to the solution. The total molar amount of the added diol is 1.1 times the molar amount of the epichlorohydrin. At the same time, a sodium hydroxide aqueous solution with a mass concentration of 50-70% is added dropwise at the same rate and molar amount as the diol. The stirring speed is 120-210 r / min. After the reaction is completed, small molecule organic matter in the reaction product is removed to obtain the epoxy resin adhesive.

[0018] In this disclosure and possible embodiments, the preparation method of the linear aliphatic diamine curing agent includes:

[0019] Iodine is used to replace the hydroxyl group in a diol to generate an iodinated ether. The iodinated ether reacts with silver nitrite to generate a dinitro ether. The dinitro ether is then reacted with hydrochloric acid and iron powder to generate the diamine curing agent.

[0020] In this disclosure and possible embodiments, a diol generated by heating 3-bromo-1-propanol and disodium ethylene glycol is used. Under heating, nitrogen protection, and stirring, a solid mixture of red phosphorus and iodine in a molar ratio of 1:3 is added to the diol, wherein the molar amount of iodine is 1.2 times that of the diol. The system temperature is 60–80°C, the stirring speed is 60–120 r / min, and the reaction time is more than 4 hours to obtain the iodoether.

[0021] In this disclosure and possible embodiments, silver nitrite in a molar amount of 3.2 to 4.5 times the molar amount of the iodide is mixed with the iodide and toluene and ball-milled, wherein the volume of the toluene is twice that of the iodide, and the ball-milling time is 200 to 300 minutes. After removing the toluene, a liquid containing dinitro ether is obtained.

[0022] Under a stirring speed of 30–50 r / min, dilute hydrochloric acid is added to a liquid containing dinitro ether, and iron powder is added in portions. The reaction system temperature is 20–30 °C. The molar amount of HCl in the dilute hydrochloric acid is 6.5–8.5 times the molar amount of nitro in the dinitro ether, and the molar amount of iron powder is 0.8–1.0 times the molar amount of HCl. The iron powder is added every 15 ± 2 min, with each addition being 2–4% of the total amount of iron powder. After the reaction is completed, the oil phase is separated, and the curing agent is obtained by fractional distillation.

[0023] Thirdly, the application of the low-temperature vibration-resistant epoxy resin described in the first aspect in the insulating rod material of rocket or missile electrostatic dischargers.

[0024] The beneficial effects of this invention are:

[0025] The low-temperature vibration-resistant epoxy resin of this invention is designed with a fully linear aliphatic molecular chain to avoid the restriction of molecular chain movement by rigid groups. Furthermore, since the atoms at both ends of the oxygen atom on the molecular backbone are the easiest to move because the oxygen atom has no other side groups and will not hinder the movement of the atoms on both sides, more oxygen atoms are introduced into the molecular backbone to maximize the low-temperature mobility of the molecular chain and maximize its low-temperature flexibility. Furthermore, based on the same design concept, a linear aliphatic diamine is synthesized as a curing agent for the epoxy resin, so that the cured epoxy resin has good molecular mobility and further ensures that it will not crack or break under low-temperature vibration environment. Detailed Implementation

[0026] The present disclosure is described below based on embodiments; however, it is worth noting that the present disclosure is not limited to these embodiments. In the detailed description of the present disclosure below, certain specific details are described in detail. However, those skilled in the art will fully understand the present disclosure for the parts not described in detail.

[0027] Furthermore, unless the context explicitly requires it, the words "comprising," "including," and similar terms throughout the specification and claims should be interpreted as including rather than exclusive or exhaustive; that is, meaning "including but not limited to."

[0028] The molecular design process and concept of the low-temperature vibration-resistant epoxy resin of this invention are as follows:

[0029] Currently, the insulating rods of the electrostatic dischargers in launch vehicles are made of bisphenol A type epoxy resin, as shown in its molecular structure formula:

[0030]

[0031] Because bisphenol A epoxy resins contain numerous aromatic groups in their molecular chains, they are inherently rigid, which hinders molecular chain movement at low temperatures, resulting in high brittleness in cold environments. To improve the low-temperature mobility of epoxy resin molecular chains, a fully linear aliphatic molecular chain was first designed, thus avoiding the restriction of molecular chain movement by rigid groups. Furthermore, since the atoms at both ends of the oxygen atom in the main molecular chain are the most mobile because the oxygen atom has no other side groups that would impede the movement of the atoms on its sides, more oxygen atoms were introduced into the main molecular chain to maximize the low-temperature mobility of the molecular chain and improve its low-temperature flexibility. Even further, based on the same design concept, a linear aliphatic diamine was synthesized as a curing agent for the epoxy resin, thereby ensuring good molecular mobility of the cured epoxy resin and further preventing fragmentation or cracking at low temperatures.

[0032] Based on the above design concept, the present invention designs the following technical solution, and the following embodiments of the present invention synthesize the low-temperature vibration-resistant epoxy resin according to the following technical solution:

[0033] I. Synthesis of linear aliphatic epoxy resin adhesives with oxygen atoms in the main chain:

[0034] 1. A chain extension reaction is performed by heating 3-bromo-1-propanol with disodium ethylene glycol to produce a diol with an oxygen atom in the main chain, as shown in the chemical reaction equation below:

[0035] 2Br-CH2-CH2-CH2-OH+NaO-CH2-CH2-ONa→HO-CH2-CH2-CH2-O-CH2-CH2-O-CH2-CH2-CH2-OH+2NaBr;

[0036] The specific process used in this disclosure is as follows: dissolving disodium ethylene glycol in ethylene glycol to obtain a solution with a mass concentration of 10-20%, and adding 3-bromo-1-propanol dropwise to the solution at a uniform rate of 240-360 min under stirring. The total molar amount added is 2.2 times the molar amount of disodium ethylene glycol. The stirring speed is 30-60 r / min, and the temperature of the reaction system is controlled at 80±1℃. After the reaction is completed, the ethylene glycol is separated by a distillation column to obtain a diol containing oxygen atoms in the main chain.

[0037] 2. The above-mentioned diol containing oxygen atoms in its main chain is reacted with epichlorohydrin to produce a linear aliphatic epoxy resin adhesive containing oxygen atoms in its main chain, as shown in the following chemical reaction equation:

[0038]

[0039] The specific process employed in this disclosure is as follows: Suspension polymerization is used. Since epichlorohydrin and diethyl ether are miscible, epichlorohydrin and diethyl ether are prepared into a solution, with the volume ratio of epichlorohydrin in the solution being 10–40%. The aforementioned diol containing oxygen atoms in its main chain is slightly soluble in diethyl ether. This diol is added dropwise to the above solution, with the total molar amount of the added diol being 1.1 times the molar amount of epichlorohydrin. Simultaneously, a 50–70% sodium hydroxide aqueous solution is added dropwise at the same rate and molar amount as the diol. Under the catalysis of sodium hydroxide, the diol exists in a dispersed droplet state in the solution. During mechanical stirring, the droplets are broken up and then merged back into smaller droplets. During this breaking / merging process, the droplets come into contact with the epichlorohydrin in the solution and, under the action of the alkaline solution, the molecular chains gradually lengthen, and the viscosity of the droplets gradually increases. The stirring speed is 120–210 r / min. After the reaction is complete, oil-liquid separation is performed, and small molecule organic matter is removed by vacuum distillation of the oil phase to obtain the epoxy resin adhesive.

[0040] The molecular structure of the generated epoxy resin shows that it is a linear aliphatic molecular chain with numerous oxygen atoms on the main chain and no interference from side groups. Theoretically, this gives the molecular chain excellent mobility in low-temperature environments.

[0041] II. Synthetic linear aliphatic diamine curing agents:

[0042] 1. A diol is used, preferably the diol generated by the heating reaction of 3-bromo-1-propanol and disodium ethylene glycol. Under heating conditions, the hydroxyl group of red phosphorus and iodine is replaced by iodine to form an iodoether, as shown in the following chemical reaction equation:

[0043]

[0044] The specific process used in this disclosure is as follows: the molar ratio of red phosphorus to iodine is 1:3, the solid mixture of red phosphorus and iodine is added to the diol in one step, and the molar amount of iodine is 1.2 times that of the diol. Under heating and stirring, the liquid temperature is maintained at 60-80°C, the stirring speed is 60-120 r / min, and the reaction is carried out under dry nitrogen protection for more than 4 hours.

[0045] 2. Iodoethers react with silver nitrite, where the iodine atom is replaced by a nitro group to form dinitroethers, as shown in the chemical reaction equation below:

[0046]

[0047] The specific process used in this disclosure is as follows: silver nitrite with a molar amount of 3.2 to 4.5 times that of iodide is loaded into a planetary ball mill along with iodide. Alumina grinding balls coated with polytetrafluoroethylene are used as the grinding medium. Toluene is used as an auxiliary liquid, with a volume of toluene twice that of iodide. The planetary ball mill rotates at a speed of 60 to 120 r / min. After planetary ball milling for 200 to 300 min, the mixture is allowed to stand for solid-liquid separation. The liquid after removing toluene by vacuum distillation contains a large amount of dinitroether.

[0048] 3. Dinitro ether reacts with hydrochloric acid and iron powder under heating conditions to generate a diamine, a curing agent for epoxy resin adhesive. See the chemical equation below for details:

[0049]

[0050] The specific process used in this disclosure is as follows: dilute hydrochloric acid is added to the above liquid while stirring at a speed of 30-50 r / min. The temperature of the reaction system is maintained at 20-30℃. The molar amount of HCl in the hydrochloric acid is 6.5-8.5 times the molar amount of nitro in the dinitro ether, and the molar amount of iron powder is 0.8-1.0 times the molar amount of HCl. Micron-sized iron powder is preferably used. The iron powder is added every 15±2 min, and each time 2-4% of the total amount of iron powder is added. After the reaction is completed, the oil is separated, and the oil phase is fractionated by a distillation column to obtain the curing agent.

[0051] 3. Calculate the ratio of the two according to 0.50 to 0.52 moles of diamine corresponding to 1 mole of epoxy resin adhesive, and react the linear aliphatic epoxy resin adhesive containing oxygen atoms in the main chain with the linear aliphatic diamine curing agent to generate the low-temperature vibration-resistant epoxy resin of the present invention.

[0052] Regarding the low-temperature flexibility of the low-temperature vibration-resistant epoxy resin synthesized in the following embodiments of the present invention, this disclosure specifically tests its tensile strength at liquid nitrogen temperature, room temperature tensile strength, and low-temperature vibration resistance to detect its low-temperature flexibility. Furthermore, through the low-temperature vibration resistance test, it examines the degree of influence of vibration generated during the liquid flow process of adding liquid oxygen or liquid hydrogen on the epoxy resin of the present invention when it is used as an insulating rod for an electrostatic discharger in a low-temperature environment, thereby further identifying its low-temperature flexibility.

[0053] Among them, the room temperature and low temperature tensile strength tests were performed in accordance with the national standard GBT 1040.1-2018;

[0054] The method for vibration resistance testing is as follows: For actual application environments, the sample is immersed in liquid nitrogen and ultrasonic vibration is applied simultaneously. According to GB / T 1040.2-2006, the tensile sample is subjected to a vibration frequency of 35kHz, an amplitude of 60μm, and a vibration time of 10min. Immediately after the vibration is completed, the tensile strength test at liquid nitrogen temperature is performed. Five samples are tested under each of the above performance test conditions.

[0055] Furthermore, this disclosure implements the synthesis method described in the above technical solution through the following embodiments 1 and 2, as follows:

[0056] Example 1:

[0057] I. Synthesis of linear aliphatic epoxy resin adhesives with oxygen atoms in the main chain:

[0058] 1. Disodium ethylene glycol is dissolved in ethylene glycol to obtain a 10% disodium ethylene glycol solution. 3-Bromo-1-propanol is added dropwise to the solution at a uniform rate of 360 min under stirring. The total molar amount added is 2.2 times the molar amount of disodium ethylene glycol. The stirring speed is 30 r / min. After the reaction is completed, oil-liquid separation is performed. Ethylene glycol is separated by a distillation column to obtain a diol with oxygen atoms in the main chain.

[0059] Further experimental results show that: a low concentration of disodium ethylene glycol solution results in a slower reaction rate but is beneficial for improving the purity of the product; however, a concentration below 10% has little effect on the reaction purity. A slow dropping rate is beneficial for reducing residual sodium ethylene glycol, but when the dropping time exceeds 360 min, the effect on the purity of the product is relatively low. A slow stirring rate is beneficial for a stable reaction; however, when the stirring rate is below 30 r / min, effective stirring cannot be achieved, preventing sufficient contact between the components in the reaction system.

[0060] 2. Prepare a 10% solution of epichlorohydrin and diethyl ether. While stirring at 120 r / min, add dropwise a diol containing oxygen atoms in the main chain from step 1 above. The total molar amount of this diol is 1.1 times the molar amount of epichlorohydrin. Simultaneously, add a 50% sodium hydroxide aqueous solution, with the molar amount of sodium hydroxide being the same as the amount of diol. After the reaction is complete, perform oil-liquid separation. Remove small molecule organic matter by vacuum distillation of the oil phase to obtain a linear aliphatic epoxy resin adhesive containing oxygen atoms in the main chain.

[0061] Further experimental results show that rapid stirring facilitates the dispersion of the diol into smaller liquids, thus increasing the probability of contact and reaction with epichlorohydrin. Lower stirring speeds result in a more uniform degree of polymerization in the final product. However, when the stirring speed is below 120 r / min, the low probability of contact between components of different viscosities within the reaction system leads to a significant decrease in the reaction rate. Lower alkali concentrations result in a more stable reaction and a more uniform polymer, but this effect tends to remain unchanged when the alkali concentration is below 50%.

[0062] II. Synthetic linear aliphatic diamine curing agents:

[0063] 1. Under stirring, a solid mixture of red phosphorus and iodine in a molar ratio of 1:3 is added at once to the above-mentioned diol containing oxygen atoms in the main chain, wherein the molar amount of iodine is 1.2 times that of the diol. The liquid temperature is maintained at 60°C and the stirring speed is 60 r / min. The reaction is carried out under the protection of dry nitrogen to obtain iodoether.

[0064] Further experimental results show that a lower reaction temperature results in a more stable reaction, but requires a longer reaction time, especially when the reaction temperature is below 60℃. Temperature has a weak effect on the stability of the reaction but significantly increases the reaction time. In addition, a low rotation speed is not conducive to the rapid dissolution of the solid mixture in the diol, especially when the rotation speed is below 60 r / min.

[0065] 2. Silver nitrite with a molar amount 3.2 times that of iodide was loaded into a planetary ball mill along with iodide. Polytetrafluoroethylene-coated alumina grinding balls were used as the grinding media. Toluene was used as an auxiliary liquid, with a volume of toluene twice that of iodide. The planetary ball mill was rotated at 60 r / min. After 200 min of planetary ball milling, the mixture was allowed to stand for solid-liquid separation. The liquid after removing toluene by vacuum distillation contained a large amount of dinitroether.

[0066] Further experimental results show that the impact of the grinding balls during planetary ball milling can generate an instantaneous GPa impact force. This intensity of impact force can induce the decomposition of silver nitrite. The reaction is stable at low rotation speed, but slow, especially when the rotation speed is below 60 r / min. In addition, the reaction is incomplete when the ball milling time is short. When the ball milling time is less than 200 min, iodoether residues are present.

[0067] 3. Add dilute hydrochloric acid to the liquid containing a large amount of dinitro ether, and add micron-sized iron powder in batches while stirring at a speed of 30 r / min to 50 r / min. Maintain the reaction system temperature at 20℃. The molar amount of HCl in the hydrochloric acid is 6.5 times the molar amount of nitro in the dinitro ether, and the molar amount of iron powder is 0.8 times the molar amount of HCl. The iron powder is added every 15 ± 2 min, and each time 2% of the total amount of iron powder is added. After the reaction is completed, the oil and liquid are separated. The oil phase is fractionated by a distillation column to obtain a linear aliphatic diamine curing agent.

[0068] Further experimental results show that stirring facilitates the contact between iron powder and hydrochloric acid to produce hydrogen gas. Low stirring speeds, especially below 20 r / min, prevent sufficient contact between the two. Low reaction temperatures help retain hydrogen gas in the liquid, but these temperatures, particularly below 20℃, result in a very slow reaction rate. Adding too little iron powder slows the reaction, while adding too much leads to a rapid reaction with excess hydrogen gas that cannot evaporate.

[0069] 3. The above-mentioned linear aliphatic epoxy resin adhesive containing oxygen atoms in its main chain reacts with the above-mentioned linear aliphatic diamine curing agent to obtain the low-temperature vibration-resistant epoxy resin of Example 1.

[0070] IV. Performance testing of the low-temperature vibration-resistant epoxy resin in Example 1:

[0071] For comparison, bisphenol A type epoxy resin was cured using the same curing process (using the same curing agent and the same curing temperature and time) to obtain bisphenol A type epoxy resin. The tensile strength test results of the two at room temperature, low temperature and after vibration at low temperature are shown in Table 1 below:

[0072] Table 1. Tensile strength test results at room temperature and low temperature

[0073]

[0074] As shown in Table 1, the tensile strength of the low-temperature vibration-resistant epoxy resin of Example 1 at room temperature is slightly lower than that of the bisphenol A type epoxy resin currently used as an insulating rod for electrostatic dischargers. This is mainly because there are no more rigid aromatic groups on the molecular chain. However, the tensile strength test results at liquid nitrogen temperature show a significant difference between the two. Firstly, the low temperature environment makes it difficult for molecular chain segments to move, resulting in a significant increase in tensile strength. In particular, the tensile strength of the samples in Example 1 is generally more than 10% higher than that at room temperature, with an average value of 35.6 MPa. This is because the epoxy resin main chain does not have aromatic groups, which gives it good mobility at low temperatures. However, the bisphenol A type epoxy resin, due to the inability of the rigid aromatic groups on the main chain to spin, will shrink at low temperatures, forming many microscopic defects or cracks. This results in a large deviation in the test data, with the highest tensile strength being 29.3 MPa and the lowest being only 7.1 MPa. This also makes the average value much lower than the room temperature tensile strength.

[0075] Most importantly, regarding the low-temperature tensile strength after vibration, the low-temperature vibration-resistant epoxy resin of Example 1 exhibits a uniform distribution of tensile strength after vibration, which is slightly higher than its room temperature tensile strength. In contrast, the bisphenol A type epoxy resin currently used as an insulating rod for electrostatic dischargers shows a significant deviation in low-temperature tensile strength after vibration, with the highest tensile strength reaching 17.1 MPa, while the tensile strength of the remaining samples is below 10 MPa, and the lowest tensile strength is only 0.8 MPa, resulting in an average value far lower than the room temperature tensile strength. These data indicate that the main-chain oxygen-containing linear aliphatic epoxy resin of Example 1 possesses excellent low-temperature resistance and low-temperature vibration resistance.

[0076] Example 2:

[0077] I. Synthesis of linear aliphatic epoxy resin adhesives with oxygen atoms in the main chain:

[0078] 1. Disodium ethylene glycol is dissolved in ethylene glycol to form a 20% disodium ethylene glycol solution. 3-Bromo-1-propanol is added dropwise to the solution at a constant rate of 240 min under stirring. The total molar amount added is 2.2 times the molar amount of disodium ethylene glycol. The stirring speed is 60 r / min. After the reaction is completed, oil-liquid separation is performed. Ethylene glycol is separated using a distillation column to obtain a diol with oxygen atoms in the main chain.

[0079] Further experimental results show that: a high concentration of disodium ethylene glycol results in a fast reaction rate, but it is easy to generate byproducts. When the concentration is higher than 20%, residual sodium ethylene glycol does not react. A fast dropping rate results in a fast reaction rate, and a dropping rate faster than 240 min will lead to an increase in byproducts.

[0080] 2. Prepare a 40% solution of epichlorohydrin and diethyl ether. While stirring at 210 r / min, add dropwise a diol containing oxygen atoms in the main chain from step 1. The total molar amount of this diol is 1.1 times the molar amount of epichlorohydrin. Simultaneously, add a 70% sodium hydroxide aqueous solution, with the molar amount of sodium hydroxide being the same as the amount of diol. After the reaction is complete, perform oil-liquid separation. Remove small molecule organic matter by vacuum distillation of the oil phase to obtain a linear aliphatic epoxy resin adhesive containing oxygen atoms in the main chain.

[0081] Further experimental results show that rapid stirring facilitates the dispersion of the diol into smaller liquids, thereby increasing the probability of contact and reaction with epichlorohydrin. However, high stirring speeds significantly reduce the viscosity of the polymer in the initial stage of the reaction, especially when the stirring speed exceeds 210 r / min, resulting in a high degree of polymerization in the final polymer, which is detrimental to subsequent use. High alkali concentrations lead to rapid reaction rates; when the alkali concentration exceeds 70%, epoxy resin adhesives with significantly different degrees of polymerization are obtained, which is unfavorable for subsequent overall performance.

[0082] II. Synthetic linear aliphatic diamine curing agents:

[0083] 1. Under stirring, a solid mixture of red phosphorus and iodine in a molar ratio of 1:3 is added at once to the above-mentioned diol containing oxygen atoms in the main chain. The molar amount of iodine is 1.2 times that of the diol. The liquid temperature is maintained at 80°C and the stirring speed is 120 r / min. The reaction is carried out under the protection of dry nitrogen to obtain iodoether.

[0084] Further experimental results show that high reaction temperatures produce byproducts, while excessively high rotation speeds have little impact on the system and only increase power output costs.

[0085] 2. Silver nitrite with a molar amount 4.5 times that of iodide was loaded into a planetary ball mill along with iodide. Polytetrafluoroethylene-coated alumina grinding balls were used as the grinding media. Toluene was used as an auxiliary liquid, with a volume of toluene twice that of iodide. The planetary ball mill was rotated at 120 r / min. After 300 min of planetary ball milling, the mixture was allowed to stand for solid-liquid separation. The liquid after removing toluene by vacuum distillation contained a large amount of dinitroether.

[0086] Further experimental results show that an instantaneous GPa impact force can be generated between the grinding balls during the planetary ball milling process. This intensity of impact force can induce the decomposition of silver nitrite. High rotation speed results in a fast reaction but wastes too much silver nitrite. In addition, long ball milling time has little effect on the degree of reaction completion.

[0087] 3. Add dilute hydrochloric acid to the liquid containing a large amount of dinitro ether, and add micron-sized iron powder in batches while stirring at a speed of 30 r / min to 50 r / min. Maintain the reaction system temperature at 30℃. The molar amount of HCl in the hydrochloric acid is 8.5 times the molar amount of nitro in the dinitro ether, and the molar amount of iron powder is 1.0 times the molar amount of HCl. The iron powder is added every 15 ± 2 min, with each addition being 4% of the total amount of iron powder. After the reaction is completed, separate the oil and liquid. The oil phase is fractionated by a distillation column to obtain a linear aliphatic diamine curing agent.

[0088] Further experimental results show that stirring facilitates the contact between iron powder and hydrochloric acid, leading to the generation of hydrogen gas. High stirring speed causes the generated hydrogen gas to evaporate from the reaction system under mechanical stirring. Excess hydrogen gas is necessary to ensure that the nitro group is epoxidized to an amine group.

[0089] III. The low-temperature vibration-resistant epoxy resin of Example 2 is obtained by reacting the linear aliphatic epoxy resin adhesive containing oxygen atoms in the main chain with the linear aliphatic diamine curing agent.

[0090] IV. Performance testing of the low-temperature vibration-resistant epoxy resin in Example 2:

[0091] For comparison, bisphenol A type epoxy resin was cured using the same curing process to obtain bisphenol A type epoxy resin. The tensile strength test results of the two at room temperature, low temperature, and after vibration at low temperature are shown in Table 2 below:

[0092] Table 2. Tensile strength test results at room temperature and low temperature

[0093]

[0094] As shown in Table 2, the tensile strength of the low-temperature vibration-resistant epoxy resin in Example 2 at room temperature is slightly lower than that of the bisphenol A type epoxy resin currently used as an insulating rod for electrostatic dischargers. This is mainly because the molecular chain lacks more rigid aromatic groups. However, the tensile strength test results at liquid nitrogen temperature show a significant difference between the two. Firstly, the low temperature environment makes molecular chain segment movement difficult, leading to a significant increase in tensile strength. In particular, the tensile strength of the samples in this invention is generally more than 10% higher than that at room temperature, with an average value of 35.6 MPa. This is because the epoxy resin main chain lacks aromatic groups and has good mobility at low temperatures. However, the bisphenol A type epoxy resin, due to the inability of the rigid aromatic groups on the main chain to spin, experiences shrinkage at low temperatures, forming many microscopic defects or cracks. This results in a large deviation in the test data, with the highest tensile strength at 18 MPa and the lowest at only 7.8 MPa, making the average value significantly lower than the room temperature tensile strength.

[0095] Most importantly, regarding the low-temperature tensile strength after vibration, the low-temperature vibration-resistant epoxy resin of Example 2 exhibits a uniformly distributed tensile strength distribution after vibration, which is slightly higher than its room temperature tensile strength. In contrast, the bisphenol A type epoxy resin currently used as an insulating rod for electrostatic dischargers shows a significant deviation in low-temperature tensile strength after vibration, with the highest tensile strength reaching 14.4 MPa and the lowest only 4.3 MPa, resulting in an average value far lower than its room temperature tensile strength. These data indicate that the linear aliphatic epoxy resin with oxygen atoms in its main chain of Example 2 possesses excellent low-temperature resistance and vibration resistance.

[0096] The embodiments described above are merely illustrative of implementation methods of this disclosure, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of this patent disclosure. It should be noted that those skilled in the art can make various modifications, equivalent substitutions, and improvements without departing from the concept of this disclosure, and these all fall within the protection scope of this disclosure. Therefore, the protection scope of this patent disclosure should be determined by the appended claims.

Claims

1. A low-temperature vibration-resistant epoxy resin, characterized in that, include: Linear aliphatic epoxy resin adhesive with oxygen atoms in the main chain and linear aliphatic diamine curing agent; The molecular structure of the epoxy resin adhesive is: ; The molecular formula of the curing agent is: ; The method for synthesizing the epoxy resin adhesive is as follows: dissolve disodium ethylene glycol in ethylene glycol to obtain a solution with a mass concentration of 10-20%. Under stirring, add 3-bromo-1-propanol dropwise to the solution at a rate of 240-360 min, with the total molar amount added being 2.2 times the molar amount of disodium ethylene glycol. The stirring speed is 30-60 r / min, and the temperature of the reaction system is controlled at 80±1℃. After the reaction is completed, ethylene glycol is separated to obtain a diol. A suspension polymerization method was used. Epichlorohydrin and diethyl ether were prepared into a solution. The diol was then added dropwise to the solution, with the total molar amount of the added diol being 1.1 times the molar amount of the epichlorohydrin. Simultaneously, a 50-70% sodium hydroxide aqueous solution was added dropwise at the same rate and molar amount as the diol. The stirring speed was 120-210 r / min. After the reaction was completed, small molecule organic matter in the reaction product was removed to obtain the epoxy resin adhesive.

2. The method for synthesizing the low-temperature vibration-resistant epoxy resin according to claim 1, characterized in that, The method includes synthesizing linear aliphatic epoxy resin adhesives with oxygen atoms in the main chain, wherein the synthesis method includes: A diol is generated by chain extension reaction of 3-bromo-1-propanol and disodium ethylene glycol, and the epoxy resin is generated by reaction of the diol with epichlorohydrin. The reaction process is as follows: dissolve the disodium ethylene glycol in ethylene glycol to obtain a solution with a mass concentration of 10-20%; under stirring, add 3-bromo-1-propanol dropwise to the solution over a time of 240-360 min, with the total molar amount added being 2.2 times the molar amount of disodium ethylene glycol; the stirring speed is 30-60 r / min; the temperature of the reaction system is controlled at 80±1℃; after the reaction is completed, ethylene glycol is separated to obtain the diol. A suspension polymerization method was used. Epichlorohydrin and diethyl ether were prepared into a solution. The diol was added dropwise to the solution, and the total molar amount of the added diol was 1.1 times the molar amount of the epichlorohydrin. At the same time, a 50-70% sodium hydroxide aqueous solution was added dropwise at the same rate and molar amount as the diol. The stirring speed was 120-210 r / min. After the reaction was completed, small molecule organic matter in the reaction product was removed to obtain the epoxy resin adhesive. It also includes the preparation of a linear aliphatic diamine curing agent, the preparation method comprising: Iodine is used to replace the hydroxyl group in a diol to generate an iodinated ether. The iodinated ether reacts with silver nitrite to generate a dinitro ether. The dinitro ether is then reacted with hydrochloric acid and iron powder to generate the diamine curing agent.

3. The method for synthesizing low-temperature vibration-resistant epoxy resin according to claim 2, characterized in that: The diol is produced by heating 3-bromo-1-propanol and disodium ethylene glycol. Under heating, nitrogen protection, and stirring, a solid mixture of red phosphorus and iodine in a molar ratio of 1:3 is added to the diol, wherein the molar amount of iodine is 1.2 times that of the diol. The system temperature is 60-80°C, the stirring speed is 60-120 r / min, and the reaction time is more than 4 hours to obtain the iodoether.

4. The method for synthesizing the low-temperature vibration-resistant epoxy resin according to claim 3, characterized in that: Silver nitrite, in a molar amount of 3.2 to 4.5 times that of the iodide, is mixed with the iodide and toluene and ball-milled. The volume of the toluene is twice that of the iodide. The ball-milling time is 200 to 300 minutes. After removing the toluene, a liquid containing dinitro ether is obtained. Under a stirring speed of 30-50 r / min, dilute hydrochloric acid is added to a liquid containing dinitro ether, and iron powder is added in portions. The reaction system temperature is 20-30℃. The molar amount of HCl in the dilute hydrochloric acid is 6.5-8.5 times the molar amount of nitro in the dinitro ether, and the molar amount of iron powder is 0.8-1.0 times the molar amount of HCl. The iron powder is added every 15±2 min, with each addition being 2-4% of the total amount of iron powder. After the reaction is completed, the oil is separated, and the oil phase is fractionated to obtain the curing agent.

5. The application of the low-temperature vibration-resistant epoxy resin according to claim 1 in the insulating rod material of rocket or missile electrostatic dischargers.

Citation Information

Patent Citations

  • Soybean oil-based aliphatic epoxy resin and preparation method thereof

    CN102875497A

  • Epoxy resin flexible curing agent and synthetic method thereof

    CN104844784A