A preparation method of flame retardant PC material

Through the use of combined PC resin and compound flame retardant, the problem of insufficient mechanical properties and flame retardant effect of existing flame retardant PC materials is solved, and the improvement of high flame retardancy and good mechanical properties is achieved, which is suitable for flame retardant PC. plastic sheets, and reduces cost and dispersion issues.

CN117247668BActive Publication Date: 2024-10-11AMMIKA (WUXI) NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311538197.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-17
Publication Date
2024-10-11
Estimated Expiration
2043-11-17

AI Technical Summary

Technical Problem

Existing flame-retardant PC materials have deficiencies in mechanical properties and flame-retardant effects, making it difficult to meet current usage requirements, and the dispersion and cost issues of flame retardants in the existing technology have not been effectively solved.

Method used

Using a compounding method of combined PC resin, silicone flame retardant and sulfonate flame retardant, through high-speed mixing and twin-screw extrusion granulation process, a flame-retardant product with high flame retardant performance and good mechanical properties is prepared. PC material.

Benefits of technology

The stability and mechanical properties of flame-retardant PC materials have been improved, and the problems of uneven dispersion and high cost of a single flame retardant have been solved. The prepared materials are suitable for use in flame-retardant PC plastic sheets and have better flame-retardant effects. and value for money.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a method for preparing a flame-retardant PC material, which adopts a material mixing injection molding mode to obtain a flame-retardant PC board with good flame-retardant properties, good mechanical properties and high comprehensive performance while ensuring that the materials are dry. The matrix is ​​a PC combination type PC resin that is a combination of PC resin, silicon PC and bromine-based flame-retardant PC. The matrix itself has certain flame-retardant properties. In addition, the compound use of two different flame retardants not only solves the problem of uneven dispersion of a single flame retardant, but also has a more excellent flame retardant effect. The prepared flame-retardant PC material has high stability, simple and efficient operation. The anti-dripping agent is a PC anti-dripping agent, which has the advantages of good compatibility, easy operation, no cohesion and wrinkling at room temperature, and can improve the impact strength of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardant engineering plastic preparation, and in particular to a method for preparing a flame retardant PC material. Background Art

[0002] PC board generally refers to PC sun board and PC endurance board, PC corrugated tile and PC lighting tile and PC synthetic resin tile. Sun board is a hollow multi-layer or double-layer structure, and endurance board is a solid board. PC board is also called polycarbonate board, which is resistant to weak acid. It is made of polycarbonate as the main component and adopts co-extrusion technology. PC is a thermoplastic engineering plastic with excellent comprehensive performance. It has excellent light transmittance, impact toughness, electrical insulation, weather resistance and other characteristics. It is widely used in aerospace, electrical lighting, light-transmitting building materials and other industries. PC sun board (also known as polycarbonate hollow board, glass capron board, PC hollow board) with good lighting effect is made of polycarbonate resin. It has the characteristics of high transparency, light weight, impact resistance, sound insulation, heat insulation, flame retardancy, anti-aging, etc. It is a kind of plastic board with extremely excellent comprehensive performance, energy saving and environmental protection. It is a plastic building material commonly used internationally.

[0003] With the continuous development of the plastics industry, the demand for polycarbonate products continues to increase, requiring them to have good mechanical properties and good low-thickness stable flame retardancy. Polycarbonate itself has certain flame retardancy, and can reach UL94 V-2 level (3.2mm) without modification, but it is still difficult to meet the current flame retardancy requirements. For this reason, it is necessary to prepare a flame-retardant PC to meet the use requirements. In the prior art, the patent document with patent announcement number CN115850940B discloses a flame-retardant PC plastic, which improves the ultrasonic welding strength of PC by adding silicon PC to the formula, solves the problem of low welding strength and low CTI in flame-retardant PC materials, and has high welding strength while having high CTI. The application publication number CN111171542A is a high CTI flame-retardant polycarbonate alloy material and its preparation method and use, which improves the CTI of the material by changing the crystallinity and crystal structure of the syndactylene added to PC. However, the degree of improvement of the CTI of this alloy is limited; there is no introduction to the content of improving the welding strength of the material. The application publication number is CN11419673A, a high CTI halogen-free flame-retardant polycarbonate material and its preparation process. The special microcapsule flame retardant with the capsule core covered by the capsule wall is used to improve the CTI value of the flame-retardant PC. The yield and cost of the homemade flame retardant are not disclosed in detail, and it is not cost-effective; there is no introduction to improving the welding strength of the material. Moreover, in the above research, the mechanical properties of the flame-retardant PC are not taken into account. It does not have a good reference and reference significance for the demand for flame retardant enhancement based on the existing basic mechanical requirements.

[0004] In view of this, we disclose a method for preparing a flame retardant PC material. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention aims to provide a method for preparing a flame retardant PC material, which further improves the flame retardant effect of the flame retardant PC while ensuring the existing mechanical properties of the flame retardant PC, and the mechanical properties of the flame retardant PC board of the present invention are slightly improved.

[0006] To achieve the above object, the present invention proposes the following technical solutions:

[0007] A flame retardant PC material, comprising the following raw material components by weight:

[0008] 100 parts of combined PC resin;

[0009] Flame retardant A 25-30 parts;

[0010] Flame retardant B 20-35 parts;

[0011] Anti-dripping agent 1-5 parts.

[0012] On the basis of the above scheme and as a preferred scheme of the above scheme, the combined PC resin includes PC resin, silicon PC and bromine-based flame retardant PC, and the ratio of the three is PC resin: silicon PC: flame retardant PC is (50-60): (30-40): 10, the PC resin is any one of aromatic polycarbonate, aliphatic polycarbonate, aromatic-aliphatic polycarbonate, and the silicon PC is polysiloxane copolymer polycarbonate.

[0013] On the basis of the above scheme and as a preferred scheme of the above scheme, the PC resin is bisphenol A polycarbonate, and the melt flow rate of the PC resin is 5-25g / 10min, and the test conditions are: temperature 300°C, load 1.2Kg.

[0014] On the basis of the above scheme and as a preferred scheme of the above scheme, the bromine-based flame-retardant PC is tetrabromobisphenol A type PC.

[0015] On the basis of the above scheme and as a preferred scheme of the above scheme, the flame retardant A is an organosilicon flame retardant, and the flame retardant B is a sulfonate flame retardant.

[0016] On the basis of the above scheme and as a preferred scheme of the above scheme, the organosilicon flame retardant is polyborosiloxane, and the sulfonate flame retardant is potassium diphenyl sulfone sulfonate.

[0017] On the basis of the above scheme and as a preferred scheme of the above scheme, the method for preparing the flame retardant PC material comprises the following steps:

[0018] S1. Material pretreatment and preparation

[0019] After drying the polymer resin at 110-120°C for 3 hours, prepare the materials according to the raw material ratio of the flame retardant PC material;

[0020] S2. Material mixing

[0021] The materials prepared according to the above ratios are stirred and mixed at high speed for 5 minutes, and then kept at 80-120°C for 0.5 hours, and then stirred and mixed at the same stirring speed for 5 minutes to obtain a premix, wherein the high-speed stirring speed is 100-200 rpm;

[0022] S3, extrusion granulation

[0023] The premix is ​​melt-blended and extruded through a twin-screw extruder, pulled, granulated, and dried to prepare flame-retardant PC resin pellets;

[0024] S4, injection molding

[0025] The resin pellets obtained by extrusion are dried at 110-120° C., and a standard sample with a thickness of 2 mm is injection molded by an injection molding machine to obtain a flame retardant PC material.

[0026] On the basis of the above scheme and as a preferred scheme of the above scheme, the temperature of each temperature control zone of the twin-screw extruder in step S3 is:

[0027] Zone 1 240-250°C, Zone 2 260-270°C, Zone 3 260-270°C, Zone 4 260-270°C, Zone 5 250-260°C, Zone 6 240-250°C, Zone 7 230-240°C, Zone 8 220-230°C, Die head 220-230°C, vacuum controlled at -0.07MPa.

[0028] On the basis of the above scheme and as a preferred scheme of the above scheme, the injection temperature of step S4 is 220-280°C.

[0029] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0030] The present invention discloses a method for preparing a flame-retardant PC material, which adopts a material mixing injection molding mode, and obtains a flame-retardant PC board with good flame-retardant performance, good mechanical properties and high comprehensive performance while ensuring that the materials are dry. The matrix adopts a combined PC resin, which itself has certain flame-retardant properties, and the compound use of two different flame retardants not only solves the problem of uneven dispersion of a single flame retardant, but also has a more excellent flame-retardant effect. The prepared flame-retardant PC material has high stability, simple and efficient operation, and is very suitable for flame-retardant PC plastic plates / sheets and other applications.

[0031] It should be appreciated that all combinations of the foregoing concepts, as well as additional concepts described in greater detail below, may be considered part of the present subject matter disclosure to the extent such concepts are not mutually inconsistent.

[0032] The foregoing and other aspects, embodiments and features of the present invention will be more fully understood from the following description. Other additional aspects of the present invention, such as the features and / or beneficial effects of the exemplary embodiments, will be apparent from the following description or will be learned from the practice of the specific embodiments according to the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meanings understood by people with general skills in the field to which the present invention belongs.

[0034] The words "first", "second" and similar words used in the patent application specification and claims of the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, unless the context clearly indicates otherwise, the singular form of "a", "an" or "the" and other similar words do not indicate a quantitative limitation, but indicate the existence of at least one. "Include" or "comprise" and other similar words mean that the elements or objects appearing before "include" or "comprise" cover the features, wholes, steps, operations, elements and / or components listed after "include" or "comprise", and do not exclude the existence or addition of one or more other features, wholes, steps, operations, elements, components and / or their collections. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0035] At present, the commonly used PC flame retardant systems include bromine, phosphate, sulfonate, silicone, etc. Bromine flame retardants have good compatibility with PC and good flame retardant effect, but they are easy to decompose at high temperatures, and the screw and mold are easily corroded to produce black spots, which affects the surface quality of the extruded sheet. In addition, bromine flame retardants produce a large amount of smoke and toxic and harmful gases when burned, which is very harmful and limits their application. For this reason, we directly use synthetic bromine flame retardant PC. Different bromine flame retardant PCs can be obtained according to the selection of raw materials. The bromine flame retardant PC of the present invention is preferably tetrabromobisphenol A type PC, and the preparation process is as follows:

[0036] First, 0.08 mol of sodium hydroxide, 0.06 mol of tetrabromobisphenol A, 3.90 mol of water and 0.0018 mol of p-tert-butylphenol were added to a 250 mL four-necked round-bottom flask, and the mixture was stirred at 20-25° C. for 0.5 h to obtain bisphenol sodium salt; the temperature was raised to 30° C., 0.10 mol of a 12 wt% sodium hydroxide aqueous solution was dripped into the four-necked flask of bisphenol sodium salt, and then a dichloromethane solution containing 0.08 mol of phosgene was dissolved therein.

[0037] Secondly, after the reaction titration is completed, the reaction is kept at 30°C for 15 minutes, and then the temperature is raised to 35°C, and a dichloromethane solution containing 0.0015 mol of tetrabutylammonium hydroxide is added to the flask. After stirring for 5 minutes, the temperature is quickly raised to 40°C and reacted for 0.5 hours. After the reaction is completed, the temperature is cooled to room temperature, and the organic phase is separated and separated to obtain brominated flame-retardant PC.

[0038] The direct preparation and use of bromine-based flame-retardant PC can reduce the possibility of flame retardant environmental pollution and solve the problem of flame retardant easy to seep out and then fail in the flame retardant system of the present invention. Secondly, in the flame retardant system, the use of phosphate-based flame retardants has a certain effect on the mechanical properties of PC; although sulfonate-based flame retardants have significant flame retardant effects, they are difficult to disperse in the PC system; silicon-based flame retardants have good processing performance and have little effect on mechanical properties, but when added alone, the amount added is large and the cost is high. The simultaneous addition of the three will affect the stability of the flame retardant effect, and due to the poor dispersion effect, there is a certain problem of decreased mechanical properties. For this reason, we adopted the compound use of flame retardant A and flame retardant B. After trying the combination of phosphate-based flame retardants, sulfonate-based flame retardants, and silicon-based flame retardants and the comparison of the simultaneous addition of the three, we selected the flame retardant A as an organosilicon flame retardant and the flame retardant B as a sulfonate flame retardant to achieve the optimization of the compounding effect. The flame retardant A of the present invention is purchased from FS-15 silicone flame retardant of Dongguan Dingxin Plastic Raw Materials Co., Ltd.; the flame retardant B is purchased from FK-1 sulfonate flame retardant of Dongguan Dingxin Plastic Raw Materials Co., Ltd.

[0039] In the present invention, the combined PC resin includes PC resin, silicon PC and bromine-based flame retardant PC, and the ratio of PC resin: silicon PC: flame retardant PC is (50-60): (30-40): 10, the PC resin is an aromatic polycarbonate, and the present invention is preferably bisphenol A polycarbonate, and the PC resin melt flow rate is 5-25g / 10min, and the test conditions are: temperature 300°C, load 1.2Kg. The PC resin of the present invention is purchased from the standard grade PC plastic raw material of Guangzhou Hongcheng Plastic Co., Ltd., with the brand name LXW-1. Furthermore, the silicon PC is a polysiloxane copolymer polycarbonate, selected from the polysiloxane copolymer polycarbonate produced by Gansu Polyyin D-0013 (containing 20% ​​silicon).

[0040] Furthermore, the anti-drip agent of the present invention is a high-transmittance PC anti-drip agent, model HG-200, purchased from Guangdong Nao New Material Technology Co., Ltd. The use of PC anti-drip agent has the advantages of easy operation, no cohesion and wrinkling at room temperature, and can improve the impact strength of the material. Moreover, the PC anti-drip agent has good compatibility with PC resin.

[0041] Performance Testing

[0042] The mechanical properties test includes three aspects: tensile strength, tensile modulus and notched impact strength. The tensile strength and tensile modulus are tested in accordance with GB / T 1040.2-2006. According to relevant test requirements and regulations, the sample size is uniformly controlled to 185 mm×20 mm×2 mm; further, the test speed in the tensile strength test is 50 mm / min, and the test speed in the tensile elastic modulus test is 1 mm / min.

[0043] The notched impact strength was tested in accordance with GB / T 1843-2008. According to the relevant test requirements and regulations, the sample size was 80 mm × 10 mm × 2 mm.

[0044] A flame retardant test was conducted on a standard sample with a thickness of 2 mm. Specifically, the 60 s vertical burning test was conducted in accordance with HB 5469. The size of the vertical burning sample was 368 mm × 76 mm × 2 mm.

[0045] The light transmittance of the sample is also an important indicator. The light transmittance and haze of the material are tested in accordance with GB / T 2410-2008, and the sample size is 50 mm×50 mm×2 mm.

[0046] Examples 1-3

[0047] The components shown in Table 1 were weighed by weight percentage: PC resin, silicon PC, brominated flame retardant PC, flame retardant A, flame retardant B, anti-dripping agent and other raw materials were weighed according to the proportions shown in Table 1 Examples 1-3. After the polymer resin was dried at 110°C for 3 hours, the materials prepared according to the above ratios were stirred and mixed at high speed for 5 minutes, and then kept at 100°C for 0.5 hours, and then stirred and mixed at the same stirring rate for 5 minutes to obtain a premix; wherein the high-speed stirring rate was 200rpm.

[0048] The premix is ​​melt-blended and extruded through a twin-screw extruder, towed, granulated, and dried to prepare flame-retardant PC resin pellets; the temperature of each temperature control zone of the twin-screw extruder is:

[0049] Zone 1 240-250°C, Zone 2 260-270°C, Zone 3 260-270°C, Zone 4 260-270°C, Zone 5 250-260°C, Zone 6 240-250°C, Zone 7 230-240°C, Zone 8 220-230°C, Die head 220-230°C, vacuum controlled at -0.07MPa.

[0050] The resin pellets obtained by extrusion are dried at 110-120°C, and a standard sample with a thickness of 2 mm is injection molded by an injection molding machine to obtain a flame retardant PC material, wherein the injection molding temperature is 220-280°C.

[0051] Comparative Example 1

[0052] Different from Example 1, the raw materials such as PC resin, silicon PC, bromine flame retardant PC, flame retardant A, flame retardant B, anti-dripping agent, etc. are weighed according to the proportions shown in Table 1 Example 1. After the polymer resin is dried at 110° C. for 3 hours, the materials prepared according to the above ratios are stirred and mixed at high speed for 5 minutes to obtain a premix, and then the premix is ​​directly melt-blended and extruded through a twin-screw extruder, towed, granulated, and dried to prepare flame-retardant PC resin pellets.

[0053] The resin pellets obtained by extrusion are dried at 110-120°C, and a standard sample with a thickness of 2 mm is injection molded by an injection molding machine to obtain a flame retardant PC material, wherein the injection molding temperature is 220-280°C.

[0054] Comparative Examples 2-8

[0055] The components shown in Table 1 are weighed by weight percentage: PC resin, silicon PC, brominated flame retardant PC, flame retardant A, flame retardant B, anti-dripping agent and other raw materials are weighed according to the proportions shown in Table 1 Comparative Examples 2-8. After the polymer resin is dried at 110°C for 3 hours, the materials prepared according to the above ratios are stirred and mixed at high speed for 5 minutes, and then kept at 100°C for 0.5 hours, and then stirred and mixed at the same stirring rate for 5 minutes to obtain a premix; wherein the high-speed stirring rate is 200rpm.

[0056] The premix is ​​melt-blended and extruded through a twin-screw extruder, towed, granulated, and dried to prepare flame-retardant PC resin pellets; the temperature of each temperature control zone of the twin-screw extruder is:

[0057] Zone 1 240-250°C, Zone 2 260-270°C, Zone 3 260-270°C, Zone 4 260-270°C, Zone 5 250-260°C, Zone 6 240-250°C, Zone 7 230-240°C, Zone 8 220-230°C, Die head 220-230°C, vacuum controlled at -0.07MPa.

[0058] The resin pellets obtained by extrusion are dried at 110-120°C, and a standard sample with a thickness of 2 mm is injection molded by an injection molding machine to obtain a flame retardant PC material, wherein the injection molding temperature is 220-280°C.

[0059] During the use of flame retardant A and flame retardant B, the maximum usage of flame retardant A relative to the PC matrix is ​​30 parts, at which time the flame retardant can play a flame retardant role and is stably dispersed in the PC matrix; the maximum usage of flame retardant B relative to the PC matrix is ​​35 parts, at which time the flame retardant can play a flame retardant role and is stably dispersed in the PC matrix. Therefore, when used alone, the ratio that can achieve the best flame retardant effect is selected as a comparative example. Furthermore, the synthesis process of bromine-based flame-retardant PC has too many steps, and the cost of using bromine-based flame-retardant PC alone for PC board preparation increases, so no relevant comparative tests are performed. See Table 1 for detailed comparison of relevant tests.

[0060] Table 1 Material ratio and test results analysis table

[0061]

[0062] From the analysis of the comparison results in Table 1 above, it can be seen that the present invention adopts the mode of "high-speed stirring-heat preservation-high-speed stirring" for material mixing, and then performs basic granulation, which can well ensure the dryness of the material during use and improve the mechanical properties to a certain extent. Furthermore, the compound use of flame retardant A and flame retardant B utilizes the large molecular weight and high degree of crosslinking of silicon-based flame retardants, and the hydroxyl functional groups in the molecules are combined with PC through hydrogen bonds to form a cross-linked network structure; the intermolecular force during the use of sulfonate flame retardants is also a boost on one hand. By using the compound flame retardant system, in the PC matrix, the interaction force of the PC molecular chains is enhanced, and the molecular chain rigidity is large, which is conducive to the increase of tensile strength and modulus.

[0063] Regarding flame retardancy, the combination of flame retardant A and flame retardant B, on the one hand, when flame retardant B is used alone, more dripping occurs during the combustion process, and the smoke is larger during the combustion process; with the auxiliary effect of flame retardant A, the smoke released during the combustion process is weakened, and the dripping is significantly reduced. This is due to the synergistic effect of the two flame retardants. During the combustion process, a dense and stable carbonized protective layer is formed, which has flame retardancy, smoke suppression, and anti-dripping properties. Flame retardant A and flame retardant B have little effect on the transparency of PC board.

[0064] Furthermore, the mixture of PC resin, silicon PC and bromine flame retardant PC can achieve a better matrix use effect and facilitate the use of compound flame retardants; in addition, the compound use of flame retardant A and flame retardant B reduces the cost to a certain extent, solves the problem of uneven dispersion of a single flame retardant, and has a more excellent flame retardant effect. The flame retardant PC material prepared by the present invention has high stability, simple operation and high efficiency.

[0065] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.

Claims

1. A flame retardant PC material, characterized in that: The raw materials include the following components by weight: 100 parts of combined PC resin; Flame retardant A 25-30 parts; Flame retardant B 20-35 parts; 1-5 parts of anti-dripping agent; The combined PC resin comprises PC resin, silicon PC and bromine flame retardant PC, and the ratio of PC resin: silicon PC: bromine flame retardant PC is (50-60): (30-40): 10, the PC resin is any one of aromatic polycarbonate, aliphatic polycarbonate and aromatic-aliphatic polycarbonate, and the silicon PC is polysiloxane copolymer polycarbonate; The flame retardant A is an organosilicon flame retardant, and the flame retardant B is a sulfonate flame retardant; The brominated flame retardant PC is tetrabromobisphenol A type PC, and the preparation process is as follows: First, 0.08 mol of sodium hydroxide, 0.06 mol of tetrabromobisphenol A, 3.90 mol of water and 0.0018 mol of p-tert-butylphenol were added to a 250 mL four-necked round-bottom flask, and the mixture was stirred at 20-25° C. for 0.5 h to obtain bisphenol sodium salt; the temperature was raised to 30° C., 0.10 mol of a 12 wt% sodium hydroxide aqueous solution was dripped into the four-necked flask containing the bisphenol sodium salt, and then a dichloromethane solution containing 0.08 mol of phosgene was dissolved therein; Secondly, after the reaction titration is completed, the reaction is carried out at 30°C for 15 minutes, and then the temperature is raised to 35°C, and a dichloromethane solution containing 0.0015 mol of tetrabutylammonium hydroxide is added to the flask. After stirring for 5 minutes, the temperature is quickly raised to 40°C and reacted for 0.5 hours. After the reaction is completed, the temperature is lowered to room temperature, and the organic phase is separated and separated to obtain brominated flame-retardant PC. The preparation method of the flame retardant PC material comprises the following steps: S1. Material pretreatment and preparation After drying the polymer resin at 110-120°C for 3 hours, prepare the materials according to the raw material ratio of the flame retardant PC material; S2. Material mixing The materials prepared according to the above ratios are stirred and mixed at high speed for 5 minutes, and then kept at 80-120°C for 0.5 hours, and then stirred and mixed at the same stirring speed for 5 minutes to obtain a premix, wherein the high-speed stirring speed is 100-200 rpm; S3, extrusion granulation The premix is ​​melt-blended and extruded through a twin-screw extruder, pulled, granulated, and dried to prepare flame-retardant PC resin pellets; S4, injection molding The resin pellets obtained by extrusion are dried at 110-120° C., and a standard sample with a thickness of 2 mm is injection molded by an injection molding machine to obtain a flame retardant PC material.

2. A flame retardant PC material according to claim 1, characterized in that: The PC resin is aromatic polycarbonate, and the PC resin has a melt flow rate of 5-25 g / 10 min. The test conditions are: temperature 300° C., load 1.2 kg.

3. The flame retardant PC material according to claim 1, characterized in that: The organosilicon flame retardant is polyborosiloxane, and the sulfonate flame retardant is potassium diphenyl sulfone sulfonate.

4. The flame retardant PC material according to claim 1, characterized in that: The temperature of each temperature control zone of the twin-screw extruder in step S3 is: Zone 1 240-250°C, Zone 2 260-270°C, Zone 3 260-270°C, Zone 4 260-270°C, Zone 5 250-260°C, Zone 6 240-250°C, Zone 7 230-240°C, Zone 8 220-230°C, Die head 220-230°C, vacuum controlled at -0.07MPa.

5. The flame retardant PC material according to claim 1, characterized in that: The injection molding temperature of step S4 is 220-280°C.