3D printing material, printing method and preparation method
By combining the first crystalline polymer and the second crystalline polymer in the 3D printing material and controlling their melting state, the problem of warping and heat resistance of the crystalline polymer material in 3D printing is solved, and the excellent material is achieved. Resistance to warping and heat.
Patent Information
- Application Number
- CN202311546780.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-20
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-11-20
AI Technical Summary
The volume shrinkage and internal stress of crystalline polymer materials due to the formation of crystal structures during the 3D printing process make printed parts prone to warping. Increasing crystallinity can improve heat resistance, but it is difficult to balance warpage resistance and heat resistance. .
A 3D printing material is used, which is composed of a first crystalline polymer and a second crystalline polymer. By controlling the temperature, the first crystalline polymer melts while the second crystalline polymer remains in a crystalline state, forming a product with excellent warpage resistance. and heat-resistant prints.
It achieves the reduction of material fluidity and warpage rate after cooling during the printing process, improves the heat resistance and anti-warping performance of printed parts, and ensures the stability and shape integrity of printed parts at high temperatures.
Smart Images

Figure CN117264394B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of 3D printing technology, and in particular to a 3D printing material, a printing method and a preparation method. Background Art
[0002] Material-Extrusion Based 3D printing (ME-3DP) is one of the most mainstream forms of polymer material additive manufacturing technology, among which Fused Filament Fabrication (FFF) is one of the mainstream technical forms. Its principle is to melt the polymer material at high temperature to obtain melt fluidity, and extrude the melt layer by layer in a certain metered manner to form a shape. At present, amorphous polymer printing materials have been widely used in FFF printing technology. For crystalline polymer materials, during the cooling and cooling process after FFF printing melt extrusion, the formation of polymer crystal structure causes a large degree of volume shrinkage of the printed part, and generates large internal stress, causing the printed part to warp. Therefore, highly crystalline polymers have a greater risk of printing warping, and the forming mechanism is more complicated, that is, the higher the crystallinity, the stronger the crystallization ability, and the faster the crystallization rate of crystalline polymer materials, the greater the risk and degree of printing warping. But on the other hand, polymer crystallization is one of the most effective ways to improve the heat resistance of polymer printed parts. Therefore, for crystalline polymer printing materials, how to make them have both excellent printing anti-warping properties and high crystallinity during the printing process to achieve high heat resistance is a common technical problem.
[0003] Therefore, it is necessary to provide a 3D printing material and printing method that can both ensure good anti-warping performance of the printed parts and improve the heat resistance of the printed parts. Summary of the invention
[0004] The main purpose of this specification is to provide a 3D printing material, printing method and preparation method with better heat resistance and printing warping resistance.
[0005] In a first aspect, the present specification provides a 3D printing material, comprising: a first crystalline polymer, an upper limit temperature of a crystalline melting temperature range of which is a first upper limit temperature; and a second crystalline polymer, a lower limit temperature of a crystalline melting temperature range of which is a second lower limit temperature, and an upper limit temperature of a crystalline melting temperature range of which is a second upper limit temperature, and the second lower limit temperature is higher than the first upper limit temperature; wherein, when the 3D printing material is heated to a target printing temperature: the first crystalline polymer melts, the 3D printing material is in a molten fluid state, at least a portion of the second crystalline polymer remains in a crystalline state, and the target printing temperature is between the first upper limit temperature and the second upper limit temperature.
[0006] In some embodiments, the target printing temperature is between the first upper temperature limit and the second lower temperature limit.
[0007] In some embodiments, under preset conditions, the target part printed by the 3D printing material has a warpage rate of 0-10% after cooling, wherein the length of the target part is 150 mm, the width is 9.6 mm, and the height is 20 mm, and the preset conditions include: the printing material is a wire of the 3D printing material, the diameter specification of the wire is 1.75 mm±0.05 mm, the printing nozzle diameter is 0.4 mm, the slicing parameters during printing are line width 0.4 mm, layer height 0.2 mm, wall layer number 13, printing speed 100 mm / s, and printing temperature 190-230 o C, the bottom plate temperature is 30-60 o C.
[0008] In some embodiments, the warpage rate is 0-5%.
[0009] In some embodiments, the second crystalline polymer is prepared from the same type of polymer with different optical activities.
[0010] In some embodiments, the first crystalline polymer comprises homogeneous crystals composed of a high molecular weight polymer; and
[0011] The second crystalline polymer includes a stereocomplex crystal composed of the high molecular weight polymer.
[0012] In some embodiments, the first crystalline polymer comprises homogeneous crystals of polylactic acid; and the second crystalline polymer comprises stereocomplex crystals of polylactic acid.
[0013] In some embodiments, the crystalline melting temperature of the first crystalline polymer is in the range of 150-180 o C; and the crystalline melting temperature range of the second crystalline polymer is 200-250 o C.
[0014] In some embodiments, the second crystalline polymer has a crystallinity of 5% to 80%.
[0015] In some embodiments, the second crystalline polymer has a crystallinity of 10% to 50%.
[0016] In a second aspect, the present specification provides a method for printing 3D printing materials, comprising: inputting 3D printing materials into a print head of a 3D printer, wherein the 3D printing materials include any of the 3D printing materials described above; and heating the 3D printing materials to a target printing temperature, and curing the 3D printing materials after extruding them from the print head to complete printing.
[0017] In a third aspect, the present specification also provides a method for preparing a 3D printing material, comprising: obtaining left-handed polylactic acid and right-handed polylactic acid; mixing the left-handed polylactic acid and the right-handed polylactic acid in a preset ratio to obtain a blended composite material, wherein the blended composite material includes stereocomposite crystals of polylactic acid and homogeneous crystals of polylactic acid, the homogeneous crystals include the left-handed polylactic acid or the right-handed polylactic acid, and the stereocomposite crystals in the blended composite material have a crystallinity of 5%-80%; and obtaining the 3D printing material after extruding the blended composite material.
[0018] It can be seen from the above technical solution that the 3D printing material provided in this specification introduces a crystalline polymer (second crystalline polymer) with a higher melting point on the basis of a material containing only a single crystalline polymer (first crystalline polymer), so that the obtained 3D printing material has excellent printing anti-warping and heat resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of this specification, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this specification. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 A schematic diagram of the crystallization melting temperature range of 3D printing materials according to some embodiments of this specification is shown;
[0021] Figure 2 A schematic diagram of the crystallization melting temperature range of 3D printing materials according to some embodiments of this specification is shown;
[0022] Figure 3 A schematic diagram of the crystallization melting temperature range of 3D printing materials according to some embodiments of this specification is shown;
[0023] Figure 4 A schematic diagram of the crystallization melting temperature range of 3D printing materials according to some embodiments of this specification is shown;
[0024] Figure 5 A schematic diagram showing a target printing model used in some embodiments of the present specification is shown;
[0025] Figure 6 A photo of the finished product after printing the 3D printing material in Example 1 is shown;
[0026] Figure 7 A photo of the finished product after printing the 3D printing material in Example 2 is shown;
[0027] Figure 8 A photo of the finished product after printing with the 3D printing material in Comparative Example 1 is shown;
[0028] Fig. 9 A photo of the finished product after printing with the 3D printing material in Comparative Example 2 is shown. DETAILED DESCRIPTION
[0029] The following description provides specific application scenarios and requirements of this specification, with the purpose of enabling those skilled in the art to make and use the contents of this specification. Various local modifications to the disclosed embodiments will be apparent to those skilled in the art, and the general principles defined herein may be applied to other embodiments and applications without departing from the spirit and scope of this specification. Therefore, this specification is not limited to the embodiments shown, but to the widest scope consistent with the claims.
[0030] In order to facilitate the understanding of this specification, the specification will be described more fully below with reference to the relevant drawings. The preferred embodiments of this specification are given in the drawings. However, this specification can be implemented in many different forms without departing from the core spirit of this specification and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of this specification more thorough and comprehensive.
[0031] The terms used herein are only used for the purpose of describing specific example embodiments and are not restrictive. For example, unless the context clearly indicates otherwise, as used herein, the singular forms "a", "an" and "the" may also include plural forms. When used in this specification, the terms "include", "comprise" and / or "contain" mean that the associated integers, steps, operations, elements and / or components exist, but do not exclude the existence of one or more other features, integers, steps, operations, elements, components and / or groups or that other features, integers, steps, operations, elements, components and / or groups may be added in the system / method.
[0032] In the present application, "X includes at least one of A, B, or C" means that X includes at least A, or X includes at least B, or X includes at least C. That is, X may include only any combination of A, B, and C, or may include any combination of A, B, and C and other possible contents / elements at the same time. The any combination of A, B, and C may be A, B, C, AB, AC, BC, or ABC.
[0033] In view of the following description, these and other features of this specification, as well as the operation and function of the relevant elements of the structure, and the economy of the combination and manufacture of the parts can be significantly improved. The description also includes all figures and text in the drawings referenced in this specification, all of which form a part of this specification. However, it should be clearly understood that the drawings are only for the purpose of illustration and description and are not intended to limit the scope of this specification. It should also be understood that the drawings are not drawn to scale. At the same time, for the convenience of description, the terms that may appear in this specification are first explained as follows.
[0034] A crystalline polymer refers to a copolymer having at least one component that is crystallizable and has a sufficient sequence length to generate crystals. In a crystalline polymer, the region where the molecules are regularly arranged is the crystalline region, and the region where the molecules are disorderly arranged is the amorphous region. The percentage of the crystalline region is called the crystallinity. For ease of description, the crystalline polymer is used in this specification to represent a crystalline polymer having both crystalline and amorphous regions. It should be noted that the first crystalline polymer and the second crystalline polymer in this specification are both crystalline polymers, and the first crystalline polymer and the second crystalline polymer contain different types of crystals.
[0035] The polymer molecules with side chains or end groups may be the reason why they cannot be completely crystallized. Due to the incomplete crystallization, the crystalline polymers have a clear melting point (T m ), the melting of crystalline polymers is completed within a relatively large temperature range. For ease of description, the crystal melting temperature range is used in this specification to represent the temperature range corresponding to the complete melting of crystalline polymers.
[0036] The lower melting point is the temperature at which the crystals in a crystalline polymer begin to melt. At this temperature, the molecular structure of the material begins to change, from the original ordered arrangement to a disordered arrangement, causing the material to change from a solid state to a liquid state, thus becoming fluid and plastic.
[0037] In the first aspect, the present specification provides a 3D printing material. The material includes at least two forms of crystalline polymers: a first crystalline polymer and a second crystalline polymer. The crystalline melting temperature range of the first crystalline polymer is between the first lower limit temperature T1 and the first upper limit temperature T2; the crystalline melting temperature range of the second crystalline polymer is between the second lower limit temperature and the second upper limit temperature. The second lower limit temperature is higher than the first upper limit temperature. In other words, the 3D printing material is formed by mixing two crystalline polymers with different crystalline melting temperature ranges, and the crystalline melting temperature ranges corresponding to the first crystalline polymer and the second crystalline polymer contained in the above 3D printing material do not intersect. In this way, when the 3D printing material is heated to a target printing temperature between the first upper limit temperature and the second upper limit temperature, the first crystalline polymer melts, and at least part of the second crystalline polymer remains in a crystalline state. In this way, at the target temperature, the 3D printing material is both in a molten fluid state and can flow, and at the same time, when cooling, because part of the material is still in a crystalline state, its shrinkage deformation is smaller than that of a 3D printing material that is completely amorphous at the printing temperature.
[0038] The first crystalline polymer and the second crystalline polymer can be polylactic acid material, nylon, photosensitive resin, etc., or any mixture or combination of these materials. For example, the first crystalline polymer and the second crystalline polymer can be the same type of polymer with different crystal structures, such as homogeneous crystals of polylactic acid and stereocrystals of polylactic acid. The first crystalline polymer and the second crystalline polymer can also be different types of polymers.
[0039] Figure 1 FIG. 2 shows a schematic diagram of the crystallization melting temperature range of 3D printing materials according to some embodiments of this specification. Figure 1 As shown in the figure, on the temperature coordinate axis, point O represents the first lower limit temperature, point A represents the first upper limit temperature, and the temperature range between OA is the crystal melting temperature range of the first crystalline polymer; point B represents the second lower limit temperature, point C represents the second upper limit temperature, and the temperature range between BC is the crystal melting temperature range of the second crystalline polymer. For example, if the temperature corresponding to point A is 100 o C, the first lower limit temperature O of the crystalline melting temperature range corresponding to the first crystalline polymer may be lower than 100 o A temperature of 99°C, such as o C. 90 o C. 80 o C or 70 o C and other temperature values; at the same time, the crystallization melting temperature range [B, C] of the second crystalline polymer can be higher than point A. For example, if the temperature corresponding to point A is 180 oIf C, then the first lower limit temperature O of the crystallization melting temperature range corresponding to the first crystalline polymer can be a certain temperature lower than 180 o °C, such as 120 o °C, 130 o °C, 140 o °C or 150 o °C and other temperature values; at the same time, the crystallization melting temperature range [B, C] of the second crystalline polymer can be higher than point A, for example, [B, C]=[200 o °C - 250 o °C].
[0040] According to the positions of each point on the temperature axis, the order of temperatures from low to high is: O < A < B < C. When the 3D printing material is heated to the first lower limit temperature O, the first crystalline polymer begins to melt; when heated continuously to point A, the first crystalline polymer is completely melted; when heated continuously to point B, the crystals of the second crystalline polymer begin to melt; when the temperature is further increased to point C, the second crystalline polymer is completely melted.
[0041] Based on this, in this specification, the melting states of the first crystalline polymer and the second crystalline polymer contained in the 3D printing material can be adjusted by controlling the temperature, so as to adjust the overall melting state of the 3D printing material. When the temperature is between point A and point C, the first crystalline polymer in the 3D printing material is completely melted, and a part of the second crystalline polymer is in a molten state. At this time, although there is still part of the second crystalline polymer in the crystal state in the 3D printing material, the 3D printing material as a whole can present a molten fluid state. In this case, since the 3D printing material as a whole presents a molten fluid state, normal printing operations can be completed; and because there is still part of the second crystalline polymer in the crystal state in the 3D printing material, it still shows a solid state. These crystals are widely distributed at various positions of the molten fluid of the 3D printing material and can play a role similar to that of "physical cross-linking points" or "composite filler particles". While improving the heat resistance of the 3D printing material, it can also effectively prevent the 3D printing material from warping and deforming due to thermal expansion and contraction during the cooling and solidification process after printing, making the 3D printing material have excellent warping resistance. The 3D printing material provided in this specification has both excellent printing warping resistance and heat resistance.
[0042] Therefore, this specification introduces a crystalline polymer (second crystalline polymer) with a higher melting point on the basis of a material containing only a single crystalline polymer (first crystalline polymer), and the obtained 3D printing material has good heat resistance and printing anti-warping properties. The printing operation temperature (i.e., the target printing temperature) of the 3D printing material provided in this specification is between the first upper limit temperature and the second upper limit temperature. In addition, the 3D printing material provided in this specification can have a variety of forms. For example, according to actual needs, it can be a wire-type 3D printing material, or a particle-type 3D printing material, and of course, it can also be a 3D printing material with other physical properties.
[0043] According to the above statements, for the above-mentioned 3D printing material, the target printing temperature for 3D printing should be between the first upper limit temperature and the second lower limit temperature. Figure 2 The case where the temperature of the 3D printing material is controlled between point A and point B according to some embodiments of this specification is shown. At this time, the first crystalline polymer in the 3D printing material is completely melted, and the second crystalline polymer has not yet begun to melt, and the 3D printing material as a whole can present a molten fluid state. When the 3D printing material as a whole presents a molten fluid state, normal printing operations can be completed; and because the second crystalline polymer in the 3D printing material is in a crystalline state, these crystals are widely distributed in various positions of the molten fluid of the 3D printing material, which can play a role similar to "physical cross-linking points" or "composite filling particles". While improving the heat resistance of the 3D printing material, it can also effectively avoid the 3D printing material from warping and deformation due to internal stress formed by thermal expansion and contraction during the cooling and solidification process after printing, so that the 3D printing material has excellent anti-warping properties. Therefore, the printing operation temperature (i.e., the target printing temperature) of the 3D printing material provided in this specification can be further between the first upper limit temperature A and the second lower limit temperature B.
[0044] The 3D printing material can measure the printing warpage performance by the deformation generated during the printing process. The smaller the warpage of the 3D printed product after printing, the better the anti-warpage performance of the 3D printing material. The warpage performance can be measured by the warpage rate. The warpage rate can be measured in the following way: under the preset target external environment, the 3D printing material of the target size is printed on the target base plate into a target part of a rectangular block of target size (L×W×H) by the target process flow, wherein the side of the target part contacting the target base plate is the bottom surface, and its length is L, width is W, and height is H; after the rectangular part is cooled, the height of the four corners of the bottom surface of the rectangular part away from the target base plate is measured (that is, the distance between the four corners and the highest point of the target base plate), and the average value h is calculated; then the warpage rate warp of the 3D material is defined as: the h value is divided by the height H of the target part, that is, the following formula is used for calculation:
[0045]
[0046] Obviously, when L, W, and H are constant, the smaller the average height h of the four corners of the bottom surface of the cuboid from the ground after cooling, the smaller the deformation of the part during cooling, and the smaller the warping rate. In this specification, the printing warping performance can be measured by the deformation generated by the 3D printing material during the printing process. The smaller the warping degree of the 3D printed product after printing, the better the anti-warping performance of the 3D printing material.
[0047] It is understandable that for the same material, under different standard sizes and different external cooling environments, the cooling speed and uniformity of the material are different, so the warpage may also be different.
[0048] Figure 5 A schematic diagram of a target printing model used in some embodiments of this specification is shown. The target size of the target part in the target printing model may be L = 150 mm, W = 9.6 mm, H = 20 mm. In this case, the following formula is used for calculation:
[0049]
[0050] According to some embodiments of the present application, the preset target external environment may include: the printing material is PLA wire, the wire diameter specification is 1.75 mm ± 0.05 mm, the printing nozzle diameter is 0.4 mm, the slicing parameters during printing are line width 0.4 mm, layer height 0.2 mm, wall layer number (shell) 13, and printing speed 100 mm / s. In addition, the printing temperature in this embodiment is matched according to the material type and extrusion characteristics, for example, the printing temperature of PLA material is 190-230 o C, the bottom plate temperature is 30-60 o C.
[0051] For example, if the target part (printed part) is 150 mm long and 20 mm high, and the average warpage height h of the four corners after cooling is 1 mm, the warp rate is calculated to be 5%.
[0052] For example, in some embodiments, under the above-mentioned preset printing conditions (i.e., the target part has a length of 150 mm, a width of 9.6 mm, and a height of 20 mm, the preset conditions include: the printing material is a wire of a 3D printing material, the diameter specification of the wire is 1.75 mm±0.05 mm, the printing nozzle diameter is 0.4 mm, the slicing parameters during printing are a line width of 0.4 mm, a layer height of 0.2 mm, a wall layer number of 13, a printing speed of 100 mm / s, and a printing temperature of 190-230o C, the bottom plate temperature is 30-60 o C, the printing air cooling intensity is 100%), the warpage rate of the target part printed by the 3D printing material after cooling is 0-10%, that is, the warpage rate of the target part after cooling can be any percentage between 0% and 10%, for example, it can be 0%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, etc. Furthermore, the warpage rate of the target part in the present application is maintained between 0% and 5%, that is, the warpage rate can be any percentage between 0% and 5%, for example, it can be 0%, 0.2%, 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, etc.
[0053] In some embodiments, the second crystalline polymer is prepared from the same type of polymer with different optical activities.
[0054] High molecular polymers are formed by the polymerization of monomer molecules. When the monomer molecules of the polymer show different optical activities, the corresponding crystal types formed may be different. Accordingly, the same type of polymer may include multiple different crystal forms. In the same type of polymer, the physical properties corresponding to different crystal forms are also different.
[0055] In this specification, the second crystalline polymer in the 3D printing material can be obtained by transforming other crystal forms in the same type of polymer, that is, the first crystalline polymer and the second crystalline polymer in the 3D printing material can be derived from the same type of polymer. Since the first crystalline polymer and the second crystalline polymer are the same type of polymer, the same type of polymers have good compatibility.
[0056] In some embodiments, the first crystalline polymer includes a homogeneous crystal composed of the high molecular weight polymer; and the second crystalline polymer includes a stereocomplex crystal composed of the high molecular weight polymer.
[0057] When the crystal type of the polymer includes homogeneous crystals and stereocomposite crystals, the crystalline polymer corresponding to the homogeneous crystals can be used as the first crystalline polymer of the 3D printing material, and the crystalline polymer corresponding to the stereocomposite crystals can be used as the second crystalline polymer of the 3D printing material. Generally speaking, in the same type of polymer, the melting point of the stereocomposite crystal is higher than the melting point of the homogeneous crystal, and therefore, the second lower limit temperature of the second crystalline polymer is higher than the first upper limit temperature of the first crystalline polymer.
[0058] For example, the first crystalline polymer may include homogeneous crystals of polylactic acid; and the second crystalline polymer may include stereocomposite crystals of the polylactic acid. Of course, it can be understood by those skilled in the art that the first crystalline polymer and the second crystalline polymer may also include stereocomposite crystals of other materials. For the purpose of demonstration only, this application takes polylactic acid as an example for illustration.
[0059] Polylactic acid (PLA) is an aliphatic polymer compound and a new type of biodegradable polymer material. The polymerized monomer lactic acid of polylactic acid has stereoisomerism, and there are two optical isomers, L-lactic acid and D-lactic acid. Therefore, polylactic acid also has three isomers, namely, left-handed poly L-lactic acid (PLLA), right-handed poly D-lactic acid (PDLA) and racemic poly DL-lactic acid (PDLLA). Among them, PLLA and PDLA are both crystalline polymers, while PDLLA is a non-crystalline polymer that is not crystalline and is in an amorphous state. The crystallization properties of polylactic acid have an important influence on its mechanical properties. The polylactic acid molecular chains in the crystal region are arranged regularly and tightly, so that the crystallization of polylactic acid is beneficial to improving the mechanical properties and heat resistance.
[0060] Under different external environments, different types of crystal forms can be transformed into each other. The crystal formed by pure PLLA or pure PDLA alone is a homogeneous crystal (HC). Stereocomposite crystal (SC) is a special crystal form of polylactic acid, which can be formed in a blended system of PLLA and PDLA. Compared with homogeneous crystals, stereocomposite crystals have better heat resistance and chemical stability. In this specification, the first crystalline polymer of the 3D printing material may be a crystalline polymer corresponding to the homogeneous crystal formed by pure PLLA alone, and the second crystalline polymer may be a crystalline polymer corresponding to the stereocomposite crystal formed by PLLA and PDLA; or the first crystalline polymer of the 3D printing material may be a crystalline polymer corresponding to the homogeneous crystal formed by pure PDLA alone, and the second crystalline polymer may be a crystalline polymer corresponding to the stereocomposite crystal formed by PLLA and PDLA.
[0061] In some embodiments, the crystalline melting temperature range of the first crystalline polymer may be 150-180 o C; and the crystalline melting temperature range of the second crystalline polymer may be 200-250o C.
[0062] Figure 3 FIG. 2 shows a schematic diagram of the crystallization melting temperature range of 3D printing materials according to some embodiments of this specification. Figure 3 As shown in the figure, in the 3D printing material with polylactic acid as the raw material, the temperature corresponding to point A (the first upper limit temperature) is 180 o C, the temperature corresponding to point B (the second lower limit temperature) is 200 o C, the temperature corresponding to point C (the second upper limit temperature) is 250 o C.
[0063] For 3D printing materials, when at 150 o C, the first crystalline polymer (containing polylactic acid homogeneous crystals) begins to melt; continue heating to 180 o C, the first crystalline polymer is completely melted; continue heating to 200 o C, the crystals of the second crystalline polymer (including stereocomplex crystals of polylactic acid) began to melt; and then the temperature continued to rise to 250 o C, the second crystalline polymer is completely melted.
[0064] In this manual, the target printing temperature can be controlled at 180 o C and 250 o C, for example, the target printing temperature can be 180 o C. 185 o C. 190 o C. 195 o C. 200 o C. 205 o C. 210 o C. 215 o C. 220 o C. 225 o C. 230 o C. 235 o C. 240 o C. 245 o C, or 250 oC, or any temperature between any two of the above temperature values. At such a temperature, the homogeneous crystals of polylactic acid in the 3D printing material are completely melted, and part of the second crystalline polymer (including the stereocomposite crystals of polylactic acid) is in a molten state. At this time, although part of the second crystalline polymer (including the stereocomposite crystals of polylactic acid) in the 3D printing material is in a crystalline state, the 3D printing material as a whole can present a molten fluid state. In this case, when the 3D printing material as a whole presents a molten fluid state, normal printing operations can be completed; and since part of the second crystalline polymer (including the stereocomposite crystals of polylactic acid) in the 3D printing material is in a crystalline state, it still appears in a solid state. These crystals are widely distributed in various positions of the molten fluid of the 3D printing material, which can play a role similar to "physical cross-linking points" or "composite filling particles". While improving the heat resistance of the 3D printing material, it can also effectively reduce the warping deformation phenomenon caused by thermal expansion and contraction and crystallization during the cooling and solidification process of the 3D printing material after printing, so that the 3D printing material has excellent anti-warping properties.
[0065] Figure 4 FIG. 2 shows a schematic diagram of the crystallization melting temperature range of 3D printing materials according to some embodiments of this specification. Figure 4 As shown, the target printing temperature can be further controlled at 180 o C and 200 o C, for example, the target printing temperature can be 180 o C. 182 o C. 185 o C. 188 o C. 190 o C. 193 o C. 195 o C. 197 o C, or 200 o C, or any temperature between any two of the above temperature values. At this time, the homogeneous crystals of polylactic acid in the 3D printing material are completely melted, and the stereocomposite crystals of polylactic acid have not yet begun to melt, and the 3D printing material as a whole can present a molten fluid state. When the 3D printing material as a whole presents a molten fluid state, normal printing operations can be completed; and because the stereocomposite crystals of polylactic acid in the 3D printing material are completely in a crystalline state, these crystals are widely distributed in various positions of the molten fluid of the 3D printing material, which can play a role similar to "physical cross-linking points" or "composite filling particles". While improving the heat resistance of the 3D printing material, it can also effectively reduce the warping deformation phenomenon caused by thermal expansion and contraction and crystallization during the cooling and solidification process of the 3D printing material after printing, so that the 3D printing material has excellent anti-warping properties.
[0066] In some embodiments, the second crystalline polymer has a crystallinity of 5% to 80%. In 3D printing materials using polylactic acid as a raw material, the second crystalline polymer has a crystallinity of 5% to 80%, that is, the stereocomplex crystals of polylactic acid account for 5% to 80% of the 3D printing material. If the crystallinity of the second crystalline polymer is too low, the heat resistance of the printed part cannot be effectively improved; if the crystallinity of the second polymer is too high, the material will not be fully melted at the printing temperature, the melt viscosity will be too high, and the wire cannot be extruded for printing. Specifically, the crystallinity of the second crystalline polymer can be any percentage value of 5%, 10%, 20%, 30%, 40%, 50%, 60%, 79%, or 80%, or any percentage example between any two of the above percentage values.
[0067] In some embodiments, the crystallinity of the second crystalline polymer may be 10% to 50%. Experiments have shown that when the crystallinity of the second crystalline polymer is between 10% and 50%, for example, when the crystallinity of the second crystalline polymer is 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc., the printing material has a moderate degree of melting during the printing process, has better printing processing performance, and the printed product can exhibit better heat resistance.
[0068] According to some embodiments of the present application, the differential scanning calorimetry (DSC) method is used in this specification to test the crystallinity of 3D printing materials. The specific test method is as follows:
[0069] (1) Take 3D printing wire as the test object and take 3-8 mg of wire sample;
[0070] (2) Using a differential scanning calorimeter (DSC), the temperature rise curve of the sample from low temperature to a completely molten state was measured in a nitrogen atmosphere at a heating rate of 10 o C / min;
[0071] (3) Obtain the melting enthalpy value △H of the second crystalline polymer from the DSC first heating curve m , then the crystallinity of the second crystalline polymer in the 3D printing filament is defined as follows:
[0072]
[0073] In the formula, is the theoretical melting enthalpy of complete crystallization of the second crystalline polymer.
[0074] In the second aspect, the present specification provides a method for printing 3D printing materials. The method may include: inputting 3D printing materials into the print head of a 3D printer, wherein the 3D printing materials include any of the 3D printing materials described above; and heating the 3D printing materials to a target printing temperature, and curing after extruding from the print head to complete printing. The 3D printing materials provided in this specification can be applied to various 3D printing processes to prepare 3D printed products of various forms, and the printing temperature is controlled at the target printing temperature described above during the printing process. The original form of the 3D printing material can be selected or adjusted according to user needs. For example, the 3D printing material provided in this specification can be a melt extrusion 3D printing material, which mainly includes two forms: ① wire material, suitable for wire melting manufacturing; ② granular material, suitable for large-size additive manufacturing. At present, the 3D printing materials provided in this specification can also be in other forms, which are not described one by one here.
[0075] In a third aspect, the specification also provides a method for preparing a 3D printing material. The method may include: obtaining L-polylactic acid and D-polylactic acid; mixing the L-polylactic acid and the D-polylactic acid in a preset ratio to obtain a blended composite material, wherein the blended composite material includes stereocomposite crystals of polylactic acid and homogeneous crystals of polylactic acid, the homogeneous crystals include the L-polylactic acid or the D-polylactic acid, and the stereocomposite crystals in the blended composite material have a crystallinity of 5%-80%; and extruding the blended composite material to obtain the 3D printing material.
[0076] In this specification, pure left-handed polylactic acid and pure right-handed polylactic acid can be mixed to form stereocomposite crystals of polylactic acid in the blending system. Left-handed polylactic acid and right-handed polylactic acid can be co-crystallized in a ratio of 1:1 to form stereocomposite crystals of polylactic acid. During the preparation process, the addition ratio of left-handed polylactic acid and right-handed polylactic acid can be regulated. When the addition ratio of left-handed polylactic acid to right-handed polylactic acid is not equal to 1, the excess one will form a corresponding homogeneous crystal, and the corresponding blended composite material contains both homogeneous crystals and stereocomposite crystals of polylactic acid, that is, the 3D printing material provided in this specification. Therefore, in order to obtain a 3D printing material containing both homogeneous crystals and stereocomposite crystals of polylactic acid, the preset ratio between left-handed polylactic acid and right-handed polylactic acid can be controlled within a certain range deviating from 1:1. For example, the preset ratio can be 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1 or other ratios.
[0077] In this specification, after the L-polylactic acid and the D-polylactic acid are mixed, the temperature can be controlled at 150-250 oC range to ensure co-crystallization between L-polylactic acid and D-polylactic acid, thereby forming a stereocomposite crystal of polylactic acid.
[0078] The following are specific preparation examples involved in the above content of the present disclosure. It should be clear that the following examples are only for illustrating the 3D printing materials, the printing methods of 3D printing materials and the preparation methods of 3D printing materials disclosed above, and the specific implementation methods and parameters used are only one or a concentrated method in accordance with the many processes and methods described above. Those skilled in the art can use other parameters according to the content introduced in this specification to prepare the 3D printing materials according to the above method without deviating from the core spirit disclosed in the application. For example, the following examples use polylactic acid as a raw material to prepare 3D printing materials. Those skilled in the art can fully understand that the above-mentioned 3D printing materials, the printing methods of 3D printing materials and the preparation methods of 3D printing materials can also apply other raw materials, as long as they comply with the core spirit disclosed in this specification. It is only limited to the length that the present disclosure does not specifically describe the embodiments of other raw materials.
[0079] As mentioned above, the performance tests of the examples and comparative examples in this specification were carried out using the same method.
[0080] 1. Warpage test conditions:
[0081] (1) Target printing model size, rectangular parallelepiped: length L = 150 mm, width W = 9.6 mm, height H = 20 mm;
[0082] (2) Printing material wire diameter specification: 1.75 mm ± 0.05 mm, printing nozzle diameter 0.4 mm;
[0083] (3) Slicing parameters: line width 0.4 mm, layer height 0.2 mm, number of wall layers (shell) 13;
[0084] (4) Printing speed: 100 mm / s;
[0085] (5) The printing temperature should be matched according to the material type and extrusion characteristics. For example, the printing temperature of PLA material is 190-230 o C, the bottom plate temperature is 30-60 o C;
[0086] (6) Printing air cooling intensity is 100%;
[0087] In the warpage test of the same type of printing materials, the same printer, base material and slicing parameters are used for comparison. After printing, measure the height of the four corners of the printed part away from the printing base, and then calculate the average value h; divide the h value by the total height of the printed part (20 mm) to define the warpage Warp, which is calculated using the following formula:
[0088]
[0089] 2. Heat resistance test: GB / T 1633-2000 thermoplastics Vicat softening temperature (VST) is used for determination. 120 Method, using a force of 10 N and a heating rate of 120 o C / h.
[0090] 3. Crystallinity test conditions of the second crystalline polymer:
[0091] (1) Take 3D printing wire as the test object and take 3-8 mg of wire sample;
[0092] (2) Using a differential scanning calorimeter (DSC), the temperature rise curve of the sample from low temperature to a completely molten state was measured in a nitrogen atmosphere at a heating rate of 10 o C / min;
[0093] (3) Obtain the melting enthalpy value △H of the second crystalline polymer from the DSC first heating curve m , then the crystallinity of the second crystalline polymer in the 3D printing filament is defined as follows:
[0094]
[0095] In the formula, is the theoretical melting enthalpy of complete crystallization of the second crystalline polymer.
[0096] Example 1
[0097] The present embodiment provides a 3D printing material, which is prepared by the following method: mixing L-polylactic acid and D-polylactic acid in a molar ratio of 4:1, and controlling the processing temperature to be between 150°C and 250°C. o C, the obtained blended composite material is the SC-PLA printing material containing homogeneous crystals and stereocomposite crystals, that is, the 3D printing material.
[0098] In the preparation method of this embodiment, the raw material contains an excess of L-polylactic acid, and the first crystalline polymer of the corresponding 3D printing material includes an excess of L-polylactic acid. The second crystalline polymer in the 3D printing material is a stereocomplex crystal of polylactic acid. The above-mentioned crystallinity test method is used to control the primary temperature rise range to 30-250 o C, the heating rate is 10 oC / min, the melting enthalpy of the second crystalline polymer was 36.4 J / g. Since the theoretical melting enthalpy of the stereocomplex crystal of polylactic acid is It is 142 J / g, so the crystallinity of the second crystalline polymer is calculated to be 25.6%.
[0099] The SC-PLA printing material was subjected to an anti-warping printing test at a temperature of 210°C to obtain a printed product. Figure 6 The finished photo after printing is shown. Figure 6 The finished product size in the figure is the same as the target printing model size, both are rectangular: length L = 150 mm, width W = 9.6 mm, height H = 20 mm. Figure 6 As shown in the figure, the printed product has no warping as a whole, showing excellent anti-warping properties. Figure 6 The printed product shown has a warpage rate of 0.24% as measured by the above-mentioned warpage rate test method.
[0100] At the same time, the printed products were subjected to Vicat heat resistance test, using GB / T 1633-2000 thermoplastic Vicat softening temperature (VST) determination. 120 Method, using a force of 10 N and a heating rate of 120 o C / h, the Vicat heat resistance temperature of the printed product was measured to be 156.9 o C, has good heat resistance.
[0101] It can be seen that the SC-PLA printing material provided in this embodiment has both excellent printing anti-warping properties and print heat resistance.
[0102] Example 2
[0103] The present embodiment provides a 3D printing material, which is prepared by the following method: mixing L-polylactic acid and D-polylactic acid in a molar ratio of 7:3, and controlling the processing temperature to be between 150°C and 250°C. o C, the obtained blended composite material is the SC-PLA printing material containing homogeneous crystals and stereocomposite crystals, that is, the 3D printing material.
[0104] In the preparation method of this embodiment, the raw material contains an excess of L-polylactic acid, and the first crystalline polymer of the corresponding 3D printing material includes an excess of L-polylactic acid. The second crystalline polymer in the 3D printing material is a stereocomplex crystal of polylactic acid. The above-mentioned crystallinity test method is used to control the primary temperature rise range to 30-250 o C, the heating rate is 10 o C / min, the melting enthalpy of the second crystalline polymer was 53.2 J / g. Since the theoretical melting enthalpy of the stereocomplex crystal of polylactic acid is It is 142 J / g, so the crystallinity of the second crystalline polymer is calculated to be 37.5%.
[0105] The SC-PLA printing material was subjected to an anti-warping printing test at a temperature of 210°C to obtain a printed product. Figure 7 The finished photo after printing is shown. Figure 7 The finished product size in the figure is the same as the target printing model size, both are rectangular: length L = 150 mm, width W = 9.6 mm, height H = 20 mm. Figure 7 As shown in the figure, the printed product has no warping as a whole, showing excellent anti-warping properties. Figure 7 The printed product shown has a warpage rate of 3% as measured by the above-mentioned warpage rate test method.
[0106] At the same time, the printed products were subjected to Vicat heat resistance test, using GB / T 1633-2000 thermoplastic Vicat softening temperature (VST) determination. 120 Method, using a force of 10 N and a heating rate of 120 o C / h, the Vicat heat resistance temperature of the printed product was measured to be 166.3 o C, has good heat resistance.
[0107] It can be seen that the SC-PLA printing material provided in this embodiment has both excellent printing anti-warping properties and print heat resistance.
[0108] Comparative Example 1
[0109] In this comparative example, ordinary L-polylactic acid material was used to prepare 3D printing material according to the same material processing technology as Example 1.
[0110] The same anti-warping printing test method as in Example 1 was used for testing. Figure 8 The finished product after printing is shown in the figure. Figure 8 As shown, the printed product has excellent anti-warping properties, and the warping rate is 0.21% according to the test.
[0111] However, the Vicat softening temperature (VST) of thermoplastics in GB / T 1633-2000 is used for determination. 120 Method, using a force of 10 N and a heating rate of 120 o C / h, the Vicat heat resistance temperature of the printed parts is 61.7 o C, indicating that the heat resistance of the 3D printing material prepared in this comparative example is low.
[0112] It can be seen that compared with the material in Example 1, the SC-PLA printing material provided in Comparative Example 1 cannot have both excellent printing anti-warping properties and print heat resistance.
[0113] Comparative Example 2
[0114] In this comparative example, ordinary L-polylactic acid material was used, 1% of a crystal nucleating agent was added, and a 3D printing material was prepared according to the same material processing process as in Example 1.
[0115] The same anti-warping printing test method as in Example 1 was used for testing. Fig. 9 The finished product after printing is shown in the figure. Fig. 9 As shown, the printed product exhibits significant warping, and the warping rate is 17.3% as measured, which exhibits poorer anti-warping properties compared to Example 1.
[0116] Under the same experimental conditions, the Vicat heat resistance temperature of the printed parts was tested to be 160.7 o C.
[0117] It can be seen from this that the SC-PLA printing material provided in Comparative Example 2 also cannot have both excellent printing anti-warping and print heat resistance.
[0118] In summary, after reading this detailed disclosure, it will be apparent to those skilled in the art that the foregoing detailed disclosure may be presented only by way of example and may not be limiting. Although not explicitly stated herein, it will be appreciated by those skilled in the art that this specification is intended to encompass various reasonable changes, improvements, and modifications to the embodiments. These changes, improvements, and modifications are intended to be proposed by this specification and are within the spirit and scope of the exemplary embodiments of this specification.
[0119] The above is a description of a specific embodiment of the present specification. Other embodiments are within the scope of the appended claims. In some cases, the actions or steps recorded in the claims can be performed in an order different from that in the embodiments and still achieve the desired results. In addition, the processes depicted in the accompanying drawings do not necessarily require the specific order or continuous order shown to achieve the desired results. In some embodiments, multitasking and parallel processing are also possible or may be advantageous.
[0120] In addition, certain terms in this specification have been used to describe embodiments of this specification. For example, "one embodiment", "an embodiment" and / or "some embodiments" mean that a particular feature, structure or characteristic described in conjunction with the embodiment may be included in at least one embodiment of this specification. Therefore, it can be emphasized and should be understood that two or more references to "an embodiment" or "one embodiment" or "an alternative embodiment" in various parts of this specification do not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics may be appropriately combined in one or more embodiments of this specification.
[0121] It should be understood that in the foregoing description of the embodiments of this specification, in order to help understand a feature and for the purpose of simplifying this specification, this specification sometimes combines various features in a single embodiment, drawing or its description. Alternatively, this specification also disperses various features in multiple embodiments of this specification. However, this does not mean that the combination of these features is necessary. When reading this specification, it is entirely possible for those skilled in the art to extract some of the features and understand them as separate embodiments. In other words, the embodiments in this specification can also be understood as the integration of multiple secondary embodiments. This is also true when the content of each secondary embodiment is less than all the features of a single aforementioned disclosed embodiment.
Claims
1. A method for printing a 3D printing wire, characterized in that: include: Input the 3D printing filament into the print head of the 3D printer; as well as The 3D printing wire is heated to a target printing temperature and solidified into a pre-printed part after being extruded from the print head to complete printing. Wherein, the 3D printing wire comprises: The homogeneous crystal of polylactic acid has an upper limit temperature of a crystal melting temperature range being a first upper limit temperature; and A stereocomposite crystal of polylactic acid, wherein the lower limit temperature of the crystal melting temperature range is a second lower limit temperature, and the upper limit temperature of the crystal melting temperature range is a second upper limit temperature, and the second lower limit temperature is higher than the first upper limit temperature; The target printing temperature is between the first upper limit temperature and the second upper limit temperature.
2. The wire material printing method according to claim 1, characterized in that: The target printing temperature is further between the first upper limit temperature and the second lower limit temperature.
3. The wire material printing method according to claim 1, characterized in that: When the 3D printing filament is heated to the target printing temperature: The homogeneous crystal melts and the 3D printing wire is in a fluid state. At least a portion of the stereocomposite crystals remain in a crystalline state, so that the 3D printing wire contains both the polylactic acid material in a fluid state and the stereocomposite crystals in a solid state.
4. The wire material printing method according to claim 1, characterized in that: Under the preset conditions, the target part printed by the 3D printing wire has a warpage rate of 0-10% after cooling, wherein the length of the target part is 150 mm, the width is 9.6 mm, and the height is 20 mm. The preset conditions include: the diameter specification of the wire is 1.75 mm±0.05 mm, the print nozzle diameter is 0.4 mm, the slicing parameters during printing are line width 0.4 mm, layer height 0.2 mm, wall layer number 13, printing speed 100 mm / s, and printing temperature 190-230 o C, the bottom plate temperature is 30-60 o C.
5. The wire material printing method according to claim 4, characterized in that: The warpage rate is 0~5%.
6. The wire material printing method according to claim 1, characterized in that: The stereocomplex crystals are prepared by using the same type of polymers with different optical activities.
7. The wire material printing method according to claim 1, characterized in that: The diameter specification of the wire is 1.75 mm±0.05 mm.
8. The wire material printing method according to claim 1, characterized in that: The crystallinity of the stereocomposite crystal is 5% to 80%.
9. The wire material printing method according to claim 8, characterized in that: The crystallinity of the stereocomposite crystal is 10% to 50%.
Citation Information
Patent Citations
Preparation method of high molecular weight polylactic acid material with high stereo-compound content
CN104804388A
Composite polylactic acid material for 3D printing and preparation method thereof
CN106046726A
Easy-to-dye polylactic acid material for 3D printing and dyeing process thereof
CN106280335A
All-stereo composite polylactic acid material with excellent melt stability and preparation method thereof
CN112920575A
Stereocomplex polylactic acid and preparation method thereof
CN113980443A