An apparatus and method for growing a regular cross-section single-crystal silicon rod by superimposed magnetic fields
The device and method for growing monocrystalline silicon rods with regular cross-sections by superimposing magnetic fields have solved the problems of energy consumption and impurity contamination in the traditional Czochralski method, and achieved efficient growth of monocrystalline silicon rods with regular cross-sections, thereby improving the quality and performance of silicon wafers for photovoltaic modules.
Patent Information
- Application Number
- CN202311215189.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-19
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-19
AI Technical Summary
Traditional Czochralski method produces cylindrical monocrystalline silicon rods. When cutting them into square silicon wafers, a large amount of edge material needs to be removed, resulting in high energy consumption and impurity contamination, which affects the efficiency of photovoltaic cells.
The device for growing regular cross-section monocrystalline silicon rods using magnetic field superposition creates a specific temperature field and magnetic field by setting up a rectangular melting zone and superconducting coils inside the furnace, controlling the flow of melt, and directly growing regular cross-section monocrystalline silicon rods.
It reduces the energy consumption of edge material remelting and regeneration, reduces impurity pollution, improves the utilization rate and quality of monocrystalline silicon, and meets the needs of photovoltaic modules.
Smart Images

Figure CN117265643B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of Czochralski crystal growth technology, and in particular to an apparatus and method for growing a regular cross-section single crystal silicon rod by superimposed magnetic field. Background Technology
[0002] To maximize power generation per unit area, solar cell modules typically use square silicon wafers. However, traditional Czochralski (CZ) growth methods produce cylindrical monocrystalline silicon rods. Therefore, creating square wafers requires complex cutting and processing. During the process of forming square monocrystalline silicon rods, a significant amount of edge material is removed. This edge material must be remelted for further crystal growth, resulting in substantial energy consumption and hindering energy conservation and emission reduction. Furthermore, the repeated remelting of the edge material introduces impurities into the molten silicon, causing pollution and ultimately reducing the power generation efficiency of the photovoltaic cells. Summary of the Invention
[0003] To address the aforementioned problems, one objective of this invention is to provide an apparatus for growing monocrystalline silicon rods with regular cross-sections using a superimposed magnetic field, thereby directly producing quasi-rectangular monocrystalline silicon rods, reducing energy consumption caused by the remelting and regrowing of edge material, and minimizing impurity contamination caused by edge material remelting. A second objective of this invention is to provide a method for growing monocrystalline silicon rods with regular cross-sections, thereby improving the utilization rate of the monocrystalline silicon cross-section, reducing cutting and processing losses, and improving the quality and performance of the monocrystalline silicon.
[0004] The first aspect of this invention provides an apparatus for growing single-crystal silicon with a regular cross-section using a superimposed magnetic field, the technical solution of which is:
[0005] A device for growing a regular cross-section single-crystal silicon rod using a superimposed magnetic field, comprising a furnace body and:
[0006] A melting zone, located within the furnace body, is configured to contain melt and seed crystals for growing single-crystal silicon; wherein at least a portion of the melting zone has a rectangular shape so that the melt surface of the melt located within the melting zone is rectangular, thereby establishing a temperature field with a first degree of matching to the contour of the melt surface.
[0007] A pulling mechanism, located above the molten zone, is used to connect the seed crystal, thereby driving the single crystal silicon to gradually move away from the molten zone in a direction perpendicular to the molten surface;
[0008] Two superconducting coils are disposed on opposite sides of the furnace exterior to form a magnetic field region, thereby applying a magnetic field to the molten zone; wherein,
[0009] The two superconducting coils are arranged along the length of the molten zone to change the ratio of the flow intensity of the melt on the molten surface in the length direction to that in the width direction, thereby forming a temperature field with a second degree of matching with the contour of the molten surface.
[0010] The second matching degree is greater than the first matching degree.
[0011] As one of the preferred options, the furnace body is provided with:
[0012] A graphite heater is fitted around the outer periphery of the molten zone to heat the silicon raw material within the molten zone to form the melt.
[0013] A water-cooled screen is located above the molten zone to control the temperature around the molten zone;
[0014] The insulation layer is connected to the water-cooled screen and is located on the outer periphery of the graphite heater;
[0015] The camera is located on the top wall of the furnace body;
[0016] A quartz inner crucible, wherein the inner edge contour of the quartz inner crucible forms the melting zone;
[0017] The graphite outer crucible is fitted onto the outer circumferential surface of the quartz inner crucible, and the two crucibles are matched in shape and outline.
[0018] As one preferred embodiment, the device further includes:
[0019] The first lifting mechanism is connected to the bottom of the melting zone;
[0020] The second lifting mechanism is connected to the bottom of the superconducting coil;
[0021] The first lifting mechanism and the second lifting mechanism have the same lifting rate to ensure that the melting zone is located in the central region of the magnetic field.
[0022] As one preferred embodiment, the melting zone includes a first region and a second region, wherein the first region is located above the second region;
[0023] The first region has a rectangular shape to form the melt surface;
[0024] The second region has an arc-shaped outline to connect with the first lifting mechanism.
[0025] As one preferred embodiment, the size of the first region is larger than the size of the seed crystal.
[0026] As one preferred embodiment, the projection surface of the superconducting coil coincides with the projection surface of the molten zone along the length direction of the molten surface.
[0027] A second aspect of the present invention also provides a method for growing a single-crystal silicon rod with a regular cross-section, which relies on the apparatus for growing a single-crystal silicon rod with a regular cross-section by superimposing a magnetic field as provided in the first aspect of the present invention, the method comprising:
[0028] The melt and seed crystal are received in the molten zone, and the melt forms a rectangular melt surface in the molten zone, thereby establishing a temperature field with a first degree of matching with the contour of the melt surface.
[0029] By applying a magnetic field parallel to the length direction of the molten zone to the molten zone using two superconducting coils, the ratio of the flow intensity of the melt on the molten surface in the length direction to that in the width direction is changed, thereby forming a temperature field with a second degree of matching with the contour of the molten surface; wherein, the second degree of matching is greater than the first degree of matching.
[0030] The melt and the seed crystal react under the temperature field corresponding to the second degree of matching to grow single-crystal silicon;
[0031] The growing single-crystal silicon is lifted in a direction perpendicular to the melt surface using a lifting mechanism to obtain a single-crystal silicon rod with a regular cross-section.
[0032] As one preferred embodiment, the method of applying a magnetic field parallel to the length direction of the molten zone using two superconducting coils to change the ratio of the flow intensity of the melt on the molten surface in the length direction to that in the width direction, thereby forming a temperature field with a second degree of matching with the contour of the molten surface, includes:
[0033] Adjusting the current intensity of the two superconducting coils, a magnetic field of target intensity is applied to the molten zone to change the ratio of the flow intensity of the melt in the length direction to the flow intensity in the width direction on the surface of the melt.
[0034] As one preferred embodiment, the method of using a lifting mechanism to lift the growing single-crystal silicon in a direction perpendicular to the melt surface to obtain a single-crystal silicon rod with a regular cross-section includes:
[0035] Adjust the lifting rate of the lifting mechanism, the temperature of the molten zone, and the current intensity of the two superconducting coils;
[0036] Under the influence of the temperature and the current intensity, the growing monocrystalline silicon is vertically lifted at the lifting rate using a lifting mechanism to obtain a monocrystalline silicon rod with a uniform cross-section along the direction perpendicular to the melt surface.
[0037] As one preferred embodiment, the method further includes:
[0038] The height of the melting zone is adjusted using the first lifting mechanism;
[0039] The height of the two superconducting coils is adjusted synchronously using a second lifting mechanism.
[0040] Compared with the prior art, this application has the following advantages:
[0041] This invention provides an apparatus for growing monocrystalline silicon with a regular cross-section using a magnetic field superposition method. The apparatus includes a furnace body and: a molten zone within the furnace body for accommodating a melt and a seed crystal to grow monocrystalline silicon; wherein at least a portion of the molten zone has a rectangular shape to make the melt surface of the melt within the molten zone rectangular, thereby establishing a temperature field with a first degree of matching to the contour of the melt surface; a lifting mechanism located above the molten zone for connecting the seed crystal to drive the monocrystalline silicon gradually away from the molten zone in a direction perpendicular to the melt surface; and two superconducting coils disposed on opposite sides outside the furnace body to form a magnetic field region to apply a magnetic field to the molten zone; wherein the two superconducting coils are arranged along the length of the molten zone to change the ratio of the flow intensity of the melt on the melt surface in the length direction to the width direction, thereby forming a temperature field with a second degree of matching to the contour of the melt surface; wherein the second degree of matching is greater than the first degree of matching.
[0042] By adopting the technical solution of this application, the shape of the melt filling the molten zone is adapted to the shape of the molten zone, so that the surface of the melt exhibits a specific shape. By designing the molten zone as rectangular, a temperature field with a first degree of matching with the contour of the molten zone is formed. By applying a magnetic field parallel to the length direction of the molten zone into the molten zone, under the combined action of thermal buoyancy, Lorentz force, and surface tension, the ratio of the flow intensity of the melt on the surface of the melt in the length direction to the width direction will change, so that the convective motion of the melt also exhibits the same contour as the molten zone. The distribution of the temperature field in the melt is also affected by the convective motion of the melt. Therefore, by the role of convective motion in forming the temperature field, a temperature field with a high degree of matching with the contour of the molten zone is formed, which changes the solid-liquid interface morphology and crystal quality, thereby better forming a single crystal silicon rod with a regular rectangular cross section. It can be directly applied to photovoltaic modules without cutting a large amount of edge material, reducing the energy consumption caused by the remelting and regrowing of edge material, and reducing the impurity pollution caused by the remelting of edge material. This is of great significance for energy conservation and emission reduction and the improvement of silicon wafer quality.
[0043] The method for growing a regular cross-section monocrystalline silicon rod provided in this embodiment of the invention has the same advantages over the prior art as the above-described device for growing a regular cross-section monocrystalline silicon rod by superimposing a magnetic field, and will not be repeated here. Attached Figure Description
[0044] To more clearly illustrate the technical solution of this application, the drawings used in the description of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0045] Figure 1 This is a schematic diagram of the overall structure of the device for growing a regular cross-section single crystal silicon rod by superimposed magnetic field according to an embodiment of this application;
[0046] Figure 2 This is a top cross-sectional view of the apparatus for growing a regular cross-section single crystal silicon rod by superimposed magnetic field according to an embodiment of this application;
[0047] Figure 3 This is a schematic diagram illustrating the flow principle of the melt according to another embodiment of this application;
[0048] Figure 4 This is a schematic diagram of the melting point isotherm distribution on the melt surface according to another embodiment of this application.
[0049] Explanation of reference numerals in the attached figures:
[0050] 100. Furnace body; 1. Graphite outer crucible; 2. Quartz inner crucible; 3. Superconducting coil; 4. Water-cooled screen; 5. Camera; 6. Insulation layer; 7. First lifting mechanism; 8. Second lifting mechanism; 9. Graphite heater; 10. Lifting mechanism; 11. Melting zone; 12. Monocrystalline silicon. Detailed Implementation
[0051] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0052] It should be noted that the basic principle of Czochralski growing single-crystal silicon rods is to bring a rotating seed crystal into contact with the polycrystalline silicon melt in the crucible. At the solid-liquid interface, the melt is arranged according to the crystal orientation of the seed crystal and solidifies to grow single-crystal silicon 12. The crystal is then pulled up, and as the pulling process continues, the melt gradually forms a single-crystal silicon rod with a larger size.
[0053] In Czochralski crystal growth, the cross-sectional shape of single-crystal silicon is primarily determined by the shape of the crystallization plane, which in turn is related to the temperature field distribution across the melt surface during crystallization. To obtain single-crystal silicon rods of specific shapes, some researchers have modified the crucible shape to adjust the temperature field. However, simply changing the crucible shape often results in single-crystal silicon rods that deviate significantly from the designed shape, failing to achieve a regular, specific shape.
[0054] Through extensive creative design experiments and professional thermodynamics and kinetics knowledge, the inventors discovered that the shape of the crystallization surface is affected by a variety of factors. The distribution of the temperature field on the melt surface is influenced by the convective motion of the melt; different convection patterns will result in different temperature field distributions, thus affecting the shape of the crystallization surface. The flow of the melt within the furnace body 100 is also affected by various factors such as inertia, melt properties, stress, and temperature gradient, leading to nonlinearity and complexity in the flow pattern.
[0055] Therefore, simply changing the shape of the crucible to adjust the temperature field cannot control the heat transfer path. The heat conduction path length is different in different regions, and the temperature distribution in different parts is uneven, causing the actual temperature field distribution to deviate from the expected shape of the crystal surface. In particular, when the expected shape of the crystal surface is a regular cross section, the prepared single crystal silicon 12 cross section often appears asymmetrical or uneven.
[0056] Meanwhile, in the process of controlling the growth of monocrystalline silicon 12, it can only control the pulling speed of the pulling mechanism 10 and the heating temperature of the heater. The process parameters that can be adjusted are limited and constrained. At the same time, the control time and control accuracy need to be improved. Otherwise, it cannot respond to changes in the cross-sectional size of monocrystalline silicon 12 and cannot achieve accurate shape, which can easily lead to unqualified monocrystalline silicon rods.
[0057] Furthermore, simply changing the crucible shape to prepare single-crystal silicon rods of a specific shape would require adapting the crucible's shape and size to prepare single-crystal silicon rods with other cross-sectional shapes. This would also necessitate simultaneous changes to the structure and parameters of other components such as the heating system and the lifting mechanism 10, increasing costs and difficulty, and extending the growth process, thus limiting the application scenarios of single-crystal silicon rods.
[0058] In view of this, embodiments of the present invention provide an apparatus for growing a regular cross-section monocrystalline silicon 12 by superimposing a magnetic field. Figure 1 An exemplary apparatus for growing a regular cross-section single-crystal silicon rod by superimposing a magnetic field according to some embodiments of the present disclosure is shown. Figure 2The diagram shows a top cross-sectional view of the apparatus, which includes a furnace body 100 and a melting zone 11 disposed within the furnace body 100 and configured to accommodate melt and a seed crystal for growing single-crystal silicon 12. At least a portion of the melting zone 11 has a rectangular shape to ensure that the melt surface of the melt within the melting zone 11 is rectangular, thereby establishing a temperature field with a first degree of matching to the contour of the melt surface. A lifting mechanism 10, located above the melting zone 11, connects the seed crystal to drive the single-crystal silicon 12 towards... The direction perpendicular to the melt surface gradually moves away from the molten zone 11; two superconducting coils 3 are disposed on opposite sides outside the furnace body 100 to form a magnetic field region to apply a magnetic field to the molten zone 11; wherein, the two superconducting coils 3 are disposed along the length direction of the molten zone 11 to change the ratio of the flow intensity of the melt on the melt surface in the length direction to the flow intensity in the width direction, thereby creating a temperature field with a second degree of matching with the contour of the melt surface; wherein, the second degree of matching is greater than the first degree of matching.
[0059] Specifically, the melting zone 11 is a container for loading polycrystalline silicon raw materials and heating the silicon to melt it into a molten material. For example, the melting zone 11 can be formed by a combination of a quartz inner crucible 2 and a graphite outer crucible 1 nested together. The quartz inner crucible 2 is located on the inner side, and its inner edge outline forms the melting zone 11, directly contacting the molten material. Its outer edge outline is closely attached to the inner edge outline of the outer graphite inner crucible, and the overall shapes of the two are matched. The graphite outer crucible 1 can hold the quartz inner crucible 2 and the molten material and its seed crystal located within it. The melting zone 11 is usually equipped with a heater, such as a graphite heater 9, which is fitted onto the outer peripheral wall of the graphite outer crucible 1 to heat and control the temperature of the molten material inside the quartz inner crucible 2.
[0060] It needs to be explained that within the molten zone 11, the melt and the seed crystal react to grow single-crystal silicon 12, forming a crystallization surface and a melt surface within this reaction system. The crystallization surface refers to the area within the molten zone 11 where the melt and the seed crystal meet, where crystallization or dissolution occurs. Alternatively, it can be understood as the boundary between the melt and the already formed solid crystal during crystal growth; its shape determines the final appearance and cross-sectional shape of the single-crystal silicon rod. The melt surface refers to the plane within the molten zone 11 where the melt and the seed crystal meet; its shape determines the flow state and surface tension between the melt and the single crystal.
[0061] The rectangular shape of at least a portion of the melting zone 11 can be understood as the upper middle part of the crucible being a cuboid, or the overall shape of the crucible being a cuboid, thus forming a reaction region with a rectangular cross-sectional profile. This reaction region can serve as the area where the seed crystal and the melt come into contact, and the melt surface of the melt within this region is rectangular. It should be understood that the rectangular portion should be larger than the area occupied by the seed crystal when it is inside the melt, ensuring that the melt surface is always within this region, maintaining the rectangular shape of the melt surface.
[0062] In this embodiment, the lifting mechanism 10 can be understood as a device for controlling the rotation and lifting of the seed crystal and the single crystal. It is typically composed of a motor, a drive shaft, a lifting platform, etc., to control and synchronize the rotation speed and lifting speed. In this embodiment, the lifting mechanism 10 drives the single crystal silicon 12 to be lifted vertically upward without rotation, and the seed crystal is rectangular.
[0063] The cross-sectional shape of the single-crystal silicon 12 is directly determined by the shape of the crystallization plane, which in turn is related to the temperature field distribution on the melt surface during crystallization. When the melting point isotherm on the melt surface is circular, a single-crystal silicon rod with a circular cross-section is grown; when the melting point isotherm is quasi-rectangular, a single-crystal silicon rod with a quasi-rectangular cross-section is grown. Within the rectangular region of the molten zone 11, a quasi-rectangular temperature field can be initially formed, causing the crystal to grow along a quasi-rectangular melting point isotherm, thus giving the crystal a tendency to grow towards a rectangular shape.
[0064] The temperature field distribution on the melt surface is mainly influenced by the convective motion of the melt. Different convection patterns result in different temperature field distributions, thus affecting the shape of the crystal surface. Furthermore, silicon melt is conductive, and moving silicon melt is affected by the Lorentz force in a magnetic field, causing its flow pattern to change.
[0065] In this embodiment, two symmetrically arranged superconducting coils 3 can be energized to generate a magnetic field, and the intensity and direction of the magnetic field can be adjusted by setting the current intensity and direction. Therefore, the convective motion of the silicon melt can be controlled by the magnetic field, so that the convective motion affects the formation of the temperature field in the melt zone, and establishes a temperature field with a second degree of matching with the contour of the melt surface, thereby controlling the temperature field distribution on the melt surface, further forming a quasi-rectangular temperature field, so that the crystal grows along the quasi-rectangular melting point isotherm, and thus the crystallization surface is quasi-rectangular, growing a quasi-rectangular single crystal silicon rod.
[0066] Thus, it can be understood that the first matching degree and the second matching degree characterize the similarity between the temperature field and the contour of the melt surface. In this embodiment, the first matching degree means that the temperature field and the contour of the melt surface are relatively similar, presenting a rectangular temperature field, while the second matching degree means that the temperature field and the contour of the melt surface are at the same height, presenting a quasi-rectangular temperature field.
[0067] More specifically, please see Figure 3 and Figure 4 , Figure 3 This is a schematic diagram of melt flow at the melt surface. Figure 4 This is a schematic diagram of the melting point isotherm distribution on the surface of the melt. When the superconducting coil 3 is arranged along the length of the molten region 11, the direction of the magnetic field applied to the molten region 11 is parallel to the length of the molten region 11. In the device provided by this invention, when the device is as follows... Figure 1 When placed as shown, the length direction of the crucible is the X-axis direction. When a transverse superconducting magnetic field along the positive X-axis is applied to the melt, under the combined action of thermal buoyancy, Lorentz force, and surface tension, the melt flow intensity on the melt surface parallel to the X-axis will decrease, while the melt flow intensity parallel to the Y-axis will increase, ultimately forming as shown. Figure 3 The flow pattern shown Figure 3 The thicker the arrow, the stronger the flow intensity. Therefore, for melts parallel to the X-axis, the flow intensity is weaker, and convective heat transfer is weaker, causing the melting point isotherm on the melt surface to shift towards the crucible wall in the X-axis direction. For melts parallel to the Y-axis, the flow intensity is stronger, and convective heat transfer is stronger, causing the melting point isotherm on the melt surface to shift away from the crucible wall in the Y-axis direction. In summary, when a transverse superconducting magnetic field along the positive X-axis is applied to the melt, the melting point isotherm will be "stretched" in the direction parallel to the magnetic field and "shortened" in the direction perpendicular to the magnetic field, ultimately forming a shape like... Figure 4 The crystal plane shown is a "quasi-rectangular" shape.
[0068] As a specific explanation of this embodiment, the direction of the magnetic field affects the trajectory of charged particles in the melt, forming a specific convection pattern. If the direction of the magnetic field is the same as the width direction of the rectangle, the melting point isotherm on the melt surface will be "stretched" along the width direction, causing the temperature field distribution on the melt surface to deviate from the expected rectangular shape. This results in the crystallization surface shape deviating from the expected shape, and the final single-crystal silicon rod exhibiting irregular cross-sectional characteristics. Therefore, in order to achieve a rectangular cross-section single-crystal silicon rod, in this embodiment, the direction of the magnetic field should be parallel to the length direction of the melt zone 11, so that the melt flows in the direction of the magnetic field. This causes the convection motion in the melt to affect the rectangular temperature field, forming a quasi-rectangular temperature field through a specific convection pattern, thereby forming a regular "quasi-rectangular" melting point isotherm. This ensures that the crystallization surface maintains the same contour as the crucible and the crystal, thus obtaining the desired regular-shaped single-crystal silicon rod.
[0069] Thus, the molten zone 11 of the present invention makes the temperature field distribution in the melt form an approximately rectangular shape, thereby avoiding temperature fluctuations and eddy currents caused by mismatched contours; the magnetic field parallel to the length direction of the molten zone 11 controls the convection mode of the melt, making the temperature field distribution in the melt closer to the expected quasi-rectangular contour; under the superposition effect of the convection mode formed by the melt participating in the further establishment of the temperature field, the heat transfer path can be better controlled, the uniformity and stability of the temperature field can be effectively controlled, the fluctuation and deformation of the crystallization surface can be reduced, the expected shape of the crystallization surface can be formed, and the crystallization quality and efficiency can be improved.
[0070] In summary, the monocrystalline silicon rods prepared by the device provided by this invention have a regular quasi-rectangular cross-section, which meets the finished product requirements of photovoltaic modules. This avoids the edge skin generated by cutting silicon wafers. Compared with the phenomenon in the prior art where the area of the edge skin (circular area minus the area of the inscribed square of the circle) accounts for as high as 36.34%, this invention significantly improves the utilization rate of the monocrystalline silicon 12 cross-section, reduces cutting and processing losses, and enhances the quality and performance of monocrystalline silicon 12.
[0071] It can be seen that this invention innovatively introduces a mode in which the shape of the crystal surface is influenced by both the melting zone 11 and the magnetic field. The melting zone 11 can still be equipped with some functional components from existing Czochralski crystal growth apparatuses to form a new apparatus. In this embodiment of the invention, some functional components may include a water-cooled screen 4 disposed above the melting zone 11 to prevent the outer wall of the crucible from overheating and being damaged or affecting the ambient temperature. The water-cooled screen 4 can abut against the outer wall of the crucible to form an effective heat insulation layer, and is also connected to the cooling system to realize the circulation and regulation of the internal cooling water. The crucible mentioned can be a combination of the above-mentioned graphite outer crucible 1 and quartz inner crucible 2, which has the characteristics of high temperature resistance, corrosion resistance, and non-contamination of the melt. A heat insulation layer 6 can be provided between the furnace body 100 and the graphite heater 9, and below the water-cooled screen 4. A CCD camera 5 is arranged in an opening in the furnace wall above the furnace body 100, with its viewing angle facing the inside of the crucible, for online monitoring of the shape of the crystal surface.
[0072] It should be noted that the device is usually equipped with a control system and a measurement system. The control system can control and adjust the device as a whole. It is connected to components such as the crucible, graphite heater 9, seed crystal, pulling mechanism 10, water-cooled screen 4, and measurement system to realize real-time feedback and adjustment of various parameters. The measurement system is generally composed of photoelectric sensors, weighing sensors, temperature sensors, etc., which can measure and monitor the performance parameters of the single crystal silicon rod such as diameter, length, temperature, and weight, to realize real-time measurement and monitoring of various parameters, so as to achieve real-time feedback of the single crystal growth process and provide data support for the control system.
[0073] It should be noted again that the graphite heater 9, water-cooled screen 4, insulation layer 6, crucible, control system and measurement system in the device of the present invention are all devices with known functions. For clarity and brevity, some descriptions of known functions and structures have been omitted in the description of the corresponding devices. For other details, please refer to the prior art with the functions described in the present invention.
[0074] In order to further improve the matching degree between the temperature field and the contour of the melt surface and form a more accurate quasi-rectangular temperature field distribution, the shapes of the seed crystal, the crucible, the graphite heater 9 and the water-cooled screen 4 mentioned in the embodiments of the present invention are all rectangular.
[0075] It needs to be explained that, to ensure isomorphic growth, traditional devices mainly employ two control methods during crystal growth. One method involves changing the pulling speed; increasing the pulling speed causes the crystal cross-section to shrink proportionally while decreasing it causes it to expand proportionally. Therefore, this method cannot adjust the aspect ratio of the crystal plane. The other method involves changing the heater power and circumferential power distribution, i.e., adjusting the aspect ratio of the crystal cross-section by changing the ratio of heating power in the length and width directions. However, this adjustment method has a significant delay and cannot guarantee high-quality isomorphic crystal growth.
[0076] In conjunction with the above embodiments, the strength and direction of the magnetic field depend on the equipment parameters such as the external magnetic source, electrodes, and current, while the magnitude of the temperature field depends on process parameters such as the heating method and heating power. In this embodiment, two superconducting coils 3 are used to apply transverse superconducting magnetic fields of different intensities to the melt, controlling the flow and heat transfer of the silicon melt. The greater the magnetic field strength, the greater the aspect ratio of the quasi-rectangular cross-section; the smaller the magnetic field strength, the smaller the aspect ratio of the quasi-rectangular cross-section, thereby controlling the shape of the crystal surface. Therefore, when it is necessary to prepare monocrystalline silicon rods of different shapes to adapt to different types of photovoltaic modules, it is only necessary to adjust the current intensity of the two superconducting coils 3 and apply a magnetic field of the target intensity to the molten zone 11. The shape of the target crystal surface can be quickly and flexibly switched to achieve isomorphic growth of monocrystalline silicon 12 without requiring major modifications to the furnace body 100 and other matching components, saving costs and resources and improving efficiency. Thus, the method of adjusting the aspect ratio of the crystal cross-section by changing the magnetic field strength has a fast response and high adjustment accuracy, which is of great significance for ensuring isomorphic crystal growth.
[0077] Here, "aspect ratio" refers to the ratio of the length to the width of a quasi-rectangular crystal face. For example, an aspect ratio of 1 results in a square.
[0078] In conjunction with the above embodiments, in another embodiment achieving isomorphic growth of single-crystal silicon 12, the control system can adjust the lifting rate of the lifting mechanism 10, the power of the graphite heater 9, and the current of the superconducting coil 3 in real time based on the shape of the crystal surface detected by the CCD camera 5 above the furnace body 100, thereby ensuring that the crystal grows isomorphically with the same quasi-rectangular cross-section. In this embodiment, by adjusting the current of the superconducting coil 3, the aspect ratio of the quasi-rectangular cross-section can be quickly changed, responding promptly to changes in the cross-sectional shape of the single-crystal silicon 12, achieving more precise isomorphic growth, and contributing to obtaining more uniform and high-quality single-crystal silicon rods.
[0079] Among them, "equal shape" can be understood as the shape and size of each cross section of a single crystal silicon rod being consistent in the direction perpendicular to the melt surface.
[0080] In a further technical solution, the device further includes a first lifting mechanism 7 connected to the bottom of the molten zone 11; and a second lifting mechanism 8 connected to the bottom of the superconducting coil 3. The first lifting mechanism 7 and the second lifting mechanism 8 operate at the same lifting rate to ensure that the molten zone 11 is located in the central region of the magnetic field. In this embodiment, both the crucible and the seed crystal move vertically, while the superconducting coil 3 moves synchronously in the vertical direction, thereby ensuring that the melt within the molten zone 11 is always within the magnetic field. In some embodiments, the heights of the first lifting mechanism 7 and the second lifting mechanism 8 can be kept level by controlling their lifting rates.
[0081] In some embodiments, the side-view projection area of the superconducting coil 3 covers the side-view projection area of the molten region 11 to ensure that the melt is subjected to the magnetic field. In some embodiments, the side-view projection surface of the superconducting coil 3 coincides with the side-view projection surface of the molten region 11, that is, the side-view surface of the superconducting coil 3 is rectangular, the side-view surface of the molten region 11 is rectangular, and the side-view surface shapes and sizes of the two are the same. In this embodiment, material of the superconducting coil 3 is saved, and magnetic field energy is prevented from leaking to other areas (areas outside the molten region 11).
[0082] The side-view projection surface can be understood as the side where the viewpoint is located along the length of the molten zone 11.
[0083] Furthermore, the rectangular side view of the molten zone 11 can be understood as the molten zone 11 being divided into a first region and a second region. When the first region and the second region have the same shape, the molten zone 11 is a cuboid; when the first region and the second region have different shapes, they are combined to form a... Figure 1 The cavity is shown. The first region is located above the second region. The first region is rectangular and its size is larger than the seed crystal, ensuring that the crystal always reacts within the first region during growth, maintaining a roughly rectangular temperature field. The second region is arc-shaped to facilitate the installation of the first lifting mechanism 7, improving the overall strength of the device.
[0084] This invention also proposes a method for growing a single-crystal silicon rod with a regular cross-section, which relies on the device described above for growing a single-crystal silicon rod with a superimposed magnetic field. The method includes the following steps:
[0085] S1. The melt zone 11 is used to receive the melt and the seed crystal, so that the melt forms a rectangular melt surface in the melt zone 11, thereby establishing a temperature field with a first degree of matching with the contour of the melt surface.
[0086] S2. Using two superconducting coils 3, a magnetic field parallel to the length direction of the molten zone 11 is applied to the molten zone 11, changing the ratio of the flow intensity of the melt on the molten surface in the length direction to that in the width direction, thereby forming a temperature field with a second matching degree to the contour of the molten surface; wherein, the second matching degree is greater than the first matching degree.
[0087] S3. The melt and the seed crystal react in the temperature field and the convection mode to grow single crystal silicon 12.
[0088] S4. Using the lifting mechanism 10, the growing single crystal silicon 12 is lifted in a direction perpendicular to the melt surface to obtain a single crystal silicon rod with a regular cross-section.
[0089] Further, step S2 includes:
[0090] S21. Adjust the current intensity of the two superconducting coils 3 and apply a magnetic field of target intensity to the molten zone 11 to change the ratio of the flow intensity of the melt in the length direction to the flow intensity in the width direction on the surface of the melt.
[0091] Further, step S4 includes:
[0092] S41. Adjust the lifting rate of the lifting mechanism 10, the temperature of the melting zone 11, and the current intensity of the two superconducting coils 3;
[0093] S42. Under the influence of the temperature and the current intensity, the growing monocrystalline silicon 12 is vertically lifted by the lifting mechanism 10 at the lifting rate to obtain a monocrystalline silicon rod with a uniform cross-section in the direction perpendicular to the melt surface.
[0094] Furthermore, the method further includes the following steps:
[0095] S5. Adjust the height of the melting zone 11 using the first lifting mechanism 7;
[0096] S6. The height of the two superconducting coils 3 is adjusted synchronously using the second lifting mechanism 8.
[0097] It should be noted that, for the sake of simplicity, the method embodiments are all described as a series of actions. However, those skilled in the art should understand that the embodiments of this application are not limited to the described order of actions, because according to the embodiments of this application, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also understand that the embodiments described in the specification are all preferred embodiments, and the actions involved are not necessarily required by the embodiments of this application.
[0098] As the method embodiments are basically similar to the device embodiments, the description is relatively simple, and relevant parts can be found in the description of the method embodiments.
[0099] It should be noted that the various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.
[0100] It should also be noted that, in this document, the terms "upper," "lower," "left," "right," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the invention. Furthermore, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations, nor should they be construed as indicating or implying relative importance. Moreover, the term "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, such that a process, method, article, or terminal device that comprises a list of elements includes not only those elements, but also other elements not expressly listed, or elements inherent to such a process, method, article, or terminal device.
[0101] The foregoing has provided a detailed description of the apparatus and method for growing a regular cross-section single-crystal silicon rod using magnetic field superposition. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the embodiments above are merely for the purpose of helping to understand this application, and the content of this specification should not be construed as a limitation of this application. Furthermore, those skilled in the art will recognize that various modifications and variations in the specific implementation methods and application scope based on this application are possible. It is neither necessary nor possible to exhaustively list all implementation methods here, but obvious variations or modifications derived therefrom are still within the protection scope of this application.
Claims
1. A device for growing a regular cross-section single-crystal silicon rod using a superimposed magnetic field, characterized in that, Including the furnace body and: A melting zone, located within the furnace body, is configured to contain melt and seed crystals for growing single-crystal silicon; wherein at least a portion of the melting zone has a rectangular shape so that the melt surface of the melt located within the melting zone is rectangular, thereby establishing a temperature field with a first degree of matching to the contour of the melt surface. A pulling mechanism, located above the molten zone, is used to connect the seed crystal, thereby driving the single crystal silicon to gradually move away from the molten zone in a direction perpendicular to the molten surface; Two superconducting coils are disposed on opposite sides of the furnace exterior to form a magnetic field region, thereby applying a magnetic field to the molten zone; wherein, The two superconducting coils are arranged along the length of the molten zone to form a transverse magnetic field parallel to the length of the molten zone. This weakens the melt flow intensity parallel to the length direction and strengthens the melt flow intensity parallel to the width direction on the surface of the melt. As a result, the melting point isotherm on the surface of the melt is elongated in the length direction and shortened in the width direction, forming a quasi-rectangular temperature field with a second degree of matching to the contour of the melt surface. Wherein, the second matching degree is greater than the first matching degree; the first matching degree and the second matching degree characterize the similarity between the contours of the temperature field and the melt surface, the first matching degree represents that the contours of the temperature field and the melt surface are relatively similar, and the second matching degree represents that the contours of the temperature field and the melt surface are at the same height.
2. The apparatus for growing a regular cross-section single-crystal silicon rod by superimposed magnetic field according to claim 1, characterized in that, The furnace body is equipped with: A graphite heater is fitted around the outer periphery of the molten zone to heat the silicon raw material within the molten zone to form the melt. A water-cooled screen is located above the molten zone to control the temperature around the molten zone; The insulation layer is connected to the water-cooled screen and is located on the outer periphery of the graphite heater; The camera is located on the top wall of the furnace body; A quartz inner crucible, wherein the inner edge contour of the quartz inner crucible forms the melting zone; The graphite outer crucible is fitted onto the outer circumferential surface of the quartz inner crucible, and the two crucibles are matched in shape and outline.
3. The apparatus for growing a regular cross-section single-crystal silicon rod by superimposed magnetic field according to claim 1, characterized in that, The device further includes: The first lifting mechanism is connected to the bottom of the melting zone; The second lifting mechanism is connected to the bottom of the superconducting coil; The first lifting mechanism and the second lifting mechanism have the same lifting rate to ensure that the melting zone is located in the central region of the magnetic field.
4. The apparatus for growing a regular cross-section single-crystal silicon rod by superimposed magnetic field according to claim 3, characterized in that, The melting zone includes a first region and a second region, with the first region located above the second region; The first region has a rectangular shape to form the melt surface; The second region has an arc-shaped outline to connect with the first lifting mechanism.
5. The apparatus for growing a regular cross-section single-crystal silicon rod by superimposed magnetic field according to claim 4, characterized in that, The size of the first region is larger than the size of the seed crystal.
6. The apparatus for growing a regular cross-section single-crystal silicon rod by superimposed magnetic field according to claim 1, characterized in that, Along the length of the melt surface, the projection surface of the superconducting coil coincides with the projection surface of the molten zone.
7. A method for growing a single-crystal silicon rod with a regular cross-section, characterized in that, The method is implemented using the apparatus for growing a regular cross-section single-crystal silicon rod by superimposed magnetic fields as described in any one of claims 1-6, and includes: The melt and seed crystal are received in the molten zone, and the melt forms a rectangular melt surface in the molten zone, thereby establishing a temperature field with a first degree of matching with the contour of the melt surface. By applying a magnetic field parallel to the length direction of the molten zone to the molten zone using two superconducting coils, the ratio of the flow intensity of the melt on the molten surface in the length direction to that in the width direction is changed, thereby forming a temperature field with a second degree of matching with the contour of the molten surface; wherein, the second degree of matching is greater than the first degree of matching. The melt and the seed crystal react under the temperature field corresponding to the second degree of matching to grow single-crystal silicon; The growing single-crystal silicon is lifted in a direction perpendicular to the melt surface using a lifting mechanism to obtain a single-crystal silicon rod with a regular cross-section.
8. The method for growing a single-crystal silicon rod with a regular cross-section according to claim 7, characterized in that, The step of applying a magnetic field parallel to the length direction of the molten zone to the molten zone using two superconducting coils, thereby changing the ratio of the flow intensity of the melt on the molten surface in the length direction to the flow intensity in the width direction, and thus forming a temperature field with a second degree of matching with the contour of the molten surface, includes: Adjusting the current intensity of the two superconducting coils, a magnetic field of target intensity is applied to the molten zone to change the ratio of the flow intensity of the melt in the length direction to the flow intensity in the width direction on the surface of the melt.
9. A method for growing a single-crystal silicon rod with a regular cross-section according to claim 7 or 8, characterized in that, The process of using a lifting mechanism to lift the growing single-crystal silicon in a direction perpendicular to the melt surface to obtain a single-crystal silicon rod with a regular cross-section includes: Adjust the lifting rate of the lifting mechanism, the temperature of the molten zone, and the current intensity of the two superconducting coils; Under the influence of the temperature and the current intensity, the growing monocrystalline silicon is vertically lifted at the lifting rate using a lifting mechanism to obtain a monocrystalline silicon rod with a uniform cross-section in the direction perpendicular to the melt surface.
10. The method for growing a single-crystal silicon rod with a regular cross-section according to claim 7, characterized in that, The method further includes: The height of the melting zone is adjusted using the first lifting mechanism; The height of the two superconducting coils is adjusted synchronously using a second lifting mechanism.
Citation Information
Patent Citations
Growth of crystals made of electrically conductive melts, comprises crystallizing the electrically conductive melts into a diamond- or zinc blend structure, and introducing a crystal seed oriented in drawing direction into the melt