A high-strength anticorrosive coating and preparation method thereof

Aqueous epoxy resins were prepared by modifying graphene oxide with diazonium hydroxymethyltetramethylimide and by chemical modification, which solved the problem of graphene stacking and agglomeration in the resin, improved the anti-corrosion performance and strength of the coating, and made it suitable for a variety of industrial applications.

CN117285853BActive Publication Date: 2024-11-15SHAANXI XINHONGYU ANTICORROSION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311079113.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-25
Publication Date
2024-11-15
Estimated Expiration
2043-08-25

AI Technical Summary

Technical Problem

In existing coatings, graphene nanosheets tend to aggregate and cluster in the resin, failing to disperse evenly. This weakens the physical barrier effect and reduces the anti-corrosion performance after the coating is damaged.

Method used

A waterborne epoxy resin was prepared by modifying graphene oxide with diazoxylpyromellitic methyl methacrylate and by chemical modification. Combined with fillers, toughening agents and diluents, a high-strength anti-corrosion coating was formed. The nitrogen hydroxyl groups chelate with the metal surface to form a protective film, which prevents graphene from stacking and disperses it uniformly in the resin.

Benefits of technology

It achieves uniform dispersion of graphene in resin, enhances the anti-corrosion performance and strength of coatings, and retains good anti-corrosion ability even after coating damage, making it suitable for a variety of industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of anti-corrosion coatings, relates to a high-strength anti-corrosion coating and a preparation method thereof, and discloses a high-strength anti-corrosion coating. The coating comprises, by weight, 12 to 18 parts of dinitrohydroxybenzene tetracarboximide-modified graphene oxide, 80 to 110 parts of water-based epoxy resin prepared by a chemical modification method, 40 to 55 parts of a curing agent, 10 to 15 parts of a toughening agent, 6 to 10 parts of a diluent, and 30 to 40 parts of a filler. The coating of the invention improves the coating performance by introducing dinitrohydroxybenzene tetracarboximide-modified graphene oxide. The nitrogen hydroxyl group in the structure of dinitrohydroxybenzene tetracarboximide can chelate with metal atoms on the surface of a workpiece to form a monomolecular protective film on the metal surface, thereby actively slowing down the corrosion process of the workpiece. The dinitrohydroxybenzene tetracarboximide itself has the characteristics of an inhibitor, can effectively prevent the stacking and agglomeration of graphene oxide, so that the modified graphene oxide can be fully and evenly dispersed in the resin to form a physical barrier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of anti-corrosion coatings, and specifically relates to a high-strength anti-corrosion coating and a preparation method thereof. Background Art

[0002] Metal materials have always played a vital role in the development of human civilization. In modern society, metal materials such as steel play an important role in many industrial fields such as oil and gas transportation, marine development, and chemical production due to their unique high strength, high ductility, high electrical and thermal conductivity. However, in actual applications, metal corrosion is a difficult problem that needs to be solved during the use of metal materials.

[0003] Due to its wide applicability, simple construction, low cost and many other advantages, coating anti-corrosion technology has become the most widely used metal anti-corrosion method. For example, the Chinese invention authorization patent with announcement number CN113698847B, the patent document with publication date September 6, 2019, discloses a bottom-to-top integrated high-performance graphene heavy-duty anti-corrosion coating and its preparation method and molding process. The above technical scheme has higher substrate adhesion, toughness, barrier properties, salt spray resistance, moisture and heat resistance and acid resistance than similar material coatings.

[0004] However, the coating prepared by the above scheme also has shortcomings. First, the above technical scheme directly disperses it by physical means such as stirring or ultrasound. The physical method is used to disperse graphene. Graphene nanomaterials have high surface energy. Physical dispersion makes it easy for graphene nanosheet materials to stack and agglomerate in the resin, and it is impossible to evenly disperse in the resin to form a physical barrier. Second, if the physically dispersed coating is damaged in actual application, the physical barrier property of the coating will be destroyed, and the overall anti-corrosion performance of the coating will be greatly weakened. Summary of the invention

[0005] In order to solve the defects in the above technical solution that the graphene nanosheet material is easy to stack and agglomerate in the resin and cannot be evenly dispersed in the resin to form a physical barrier; and if damage occurs in actual application, the physical barrier property of the coating will be destroyed and the overall anti-corrosion performance of the coating will be greatly weakened; the purpose of the present invention is to provide a high-strength anti-corrosion coating and a preparation method.

[0006] The purpose of the present invention can be achieved by the following technical scheme: a high-strength anti-corrosion coating comprises: 12 to 18 parts of dinitrohydroxybenzene tetracarboximide modified graphene oxide, 80 to 110 parts of water-based epoxy resin prepared by chemical modification, 40 to 55 parts of curing agent, 10 to 15 parts of toughening agent, 6 to 10 parts of diluent, and 30 to 40 parts of filler.

[0007] Furthermore, the toughening agent includes at least one of epoxy oil and dimer fatty acid.

[0008] Furthermore, the diluent includes at least one of phthalic acid and xylene.

[0009] Furthermore, the filler comprises calcined kaolin, glass powder, talc powder and quartz powder in a mass ratio of 1:4:4:2; and the particle size of the filler is 120-200 μm.

[0010] The dinitrohydroxypyromellitamide modified graphene oxide is prepared and synthesized from graphene oxide and dinitrohydroxypyromellitamide.

[0011] The dinitrohydroxypyromellitimide modified graphene oxide is prepared by the following method: dispersing the prepared graphene oxide in deionized water, then adding the precipitated dinitrohydroxypyromellitimide, and ultrasonically treating until the two are dispersed in the deionized water; heating the dispersed mixed solution to 80 degrees Celsius under magnetic stirring for 8 hours, centrifuging to obtain a precipitate, washing the obtained precipitate with deionized water, and finally drying to prepare the dinitrohydroxypyromellitimide modified graphene oxide.

[0012] The weight ratio of graphene oxide to dinitrohydroxybenzene tetracarboximide is 1:2-1:3.

[0013] The water-based epoxy resin prepared by the chemical modification method is prepared by the following method: epoxy resin and acrylic acid are placed in a reaction container as raw materials, and then a catalyst is added, and the temperature is raised under nitrogen protection, and stirring is started when all the raw materials are melted; when the temperature of the reaction system reaches 110 degrees Celsius, the reaction is prepared by heat preservation and the acid value is measured, and the reaction endpoint is reached when the acid value is lower than 5, and the water-based epoxy resin prepared by the chemical modification method is obtained.

[0014] Furthermore, the catalyst is triphenylphosphine.

[0015] The graphene oxide is prepared by the following method: adding graphite powder and NaNO3 into a reaction container, slowly adding concentrated sulfuric acid, mechanically stirring and reacting for 0.5 hours, placing in an ice bath, slowly adding potassium permanganate powder, and reacting for 1 hour; after the reaction is completed, removing the ice bath, and then reacting at 30 degrees Celsius for 24 hours; slowly adding deionized water within 0.5 hours; then adding hydrogen peroxide, stopping the reaction after reacting for 1 hour, using centrifugal separation to obtain a precipitate, and washing the precipitate with deionized water, and finally freeze-drying the obtained product to prepare graphene oxide.

[0016] Furthermore, the graphene oxide is prepared from graphite powder, NaNo3, concentrated sulfuric acid, deionized water and hydrogen peroxide as raw materials in a weight ratio of 3:1:50:50:25.

[0017] Furthermore, the concentration of the concentrated sulfuric acid is 70%; the concentration of the hydrogen peroxide is 30%.

[0018] The dinitrohydroxypyromellitimide is prepared by the following method: hydroxylamine hydrochloric acid and triethylamine are put into a reaction container, ethanol solution is added, and stirred until both are completely dissolved in the ethanol solution, and then pyromellitic anhydride is added for reflux reaction for 8 hours. After the reaction is completed, deionized water is added to precipitate dinitrohydroxypyromellitimide solid.

[0019] Furthermore, the dinitrohydroxypyromellitic imide is prepared from hydroxylamine hydrochloric acid, triethylamine and pyromellitic anhydride as raw materials in a weight ratio of 1:2:1.

[0020] Furthermore, the weight ratio of the ethanol to deionized water is 1:1.

[0021] The preparation method of the high-strength anti-corrosion coating is as follows: adding a water-based epoxy resin prepared by a chemical modification method and the prepared dihydrogen hydroxybenzene tetracarboximide-modified graphene oxide into a reaction container, mechanically stirring for 0.5 hours, and after the modified graphene oxide is evenly dispersed, adding a filler, stirring evenly, adding a toughening agent and a diluent, and mixing evenly; finally, adding a curing agent, and continuing to stir, and the preparation and synthesis of the high-strength anti-corrosion coating is completed after sufficient mixing.

[0022] Furthermore, the curing agent is a polyamide curing agent.

[0023] The present invention has the beneficial effects:

[0024] (1) The present invention improves the coating performance by introducing dinitrohydroxybenzene tetracarboximide to modify graphene oxide. The nitrogen hydroxyl group in the structure of dinitrohydroxybenzene tetracarboximide can chelate with the metal atoms on the surface of the workpiece to form a monomolecular protective film on the metal surface, which can effectively prevent corrosive media such as H2O and O2 from contacting the substrate, thereby actively slowing down the corrosion process of the workpiece;

[0025] (2) Diazohydroxybenzene tetracarboximide can be used to modify graphene oxide. It has the characteristics of an inhibitor and can effectively prevent the stacking and agglomeration of graphene oxide, so that the modified graphene oxide can be fully and evenly dispersed in the resin to form a physical barrier. DETAILED DESCRIPTION

[0026] Now describe in detail various exemplary embodiments of the present invention, this detailed description should not be considered as limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing a particular embodiment, and are not used to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper limit and the lower limit of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the range.

[0027] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0028] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0029] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0030] The "parts" indicated in the following examples are all parts by weight.

[0031] Example 1

[0032] A high-strength anti-corrosion coating is composed of the following components by weight: 12 parts of dinitrohydroxybenzene tetracarboximide-modified graphene oxide, 100 parts of water-based epoxy resin prepared by a chemical modification method, 50 parts of a curing agent, 10 parts of a toughening agent, 6 parts of a diluent, and 30 parts of a filler.

[0033] The toughening agent is dimer fatty acid, the diluent is phthalic acid; the filler comprises calcined kaolin, glass powder, talcum powder and quartz powder in a mass ratio of 1:4:4:2.

[0034] The particle size of the filler used was 120-160 μm.

[0035] Preparation of graphene oxide: First, add 6g of graphite powder and 2g of NaNO3 into a reaction container, slowly add 70% concentrated sulfuric acid totaling 100g, react under mechanical stirring at 30 degrees Celsius for 0.5h, place in an ice bath with a temperature of 0 degrees Celsius, slowly add 3g of potassium permanganate powder, and react for 1h; after the reaction is completed, remove the ice bath, and then react at 30 degrees Celsius for 24h; slowly add deionized water totaling 100g within 0.5h; then add 30% hydrogen peroxide totaling 50g within 3min, and stop the reaction after 1h; use centrifugal separation to obtain a precipitate, wash the precipitate with deionized water, and finally freeze-dry the product to obtain graphene oxide.

[0036] Preparation of dinitrohydroxybenzene tetracarboximide: 5 g of hydroxylamine hydrochloride and 10 g of triethylamine are put into a reaction container, 100 g of ethanol solution is added, and stirred until both are completely dissolved in the ethanol solution, then 5 g of pyromellitic anhydride is added and refluxed for 8 hours. After the reaction is completed, 100 g of deionized water is added to precipitate dinitrohydroxybenzene tetracarboximide solid.

[0037] Among them, the weight ratio of hydroxylamine hydrochloric acid: triethylamine: pyromellitic anhydride is 1:2:1; the weight ratio of ethanol and deionized water is 1:1.

[0038]

[0039] The above formula is a schematic diagram for the synthesis of dinitrohydroxybenzene tetracarboximide.

[0040] Preparation of hydroxy-diazobenzene tetracarboximide-modified graphene oxide: 3 g of the graphene oxide prepared above was dispersed in deionized water, and then 6 g of the precipitated dihydrogen-hydroxybenzene tetracarboximide was added, and ultrasonic treatment was performed until both were dispersed in deionized water; the dispersed mixed solution was heated to 80 degrees Celsius under magnetic stirring for 8 hours, centrifuged to obtain a precipitate, and the obtained product was washed with deionized water, and finally dried to obtain dihydrogen-hydroxybenzene tetracarboximide-modified graphene oxide;

[0041] Wherein, the weight ratio of graphene oxide to dinitrohydroxybenzene tetracarboximide is 1:2.

[0042] Preparation of water-based epoxy resin by chemical modification method: 100g epoxy resin and 70g acrylic acid are placed in a reaction container as raw materials, and then 5g triphenylphosphine catalyst is added. Under nitrogen protection, the temperature is raised, and stirring is started when all the raw materials are melted; when the temperature of the reaction system reaches 110 degrees Celsius, the reaction temperature is maintained and the acid value is measured. When the acid value is lower than 5, the reaction endpoint is reached, and the water-based epoxy resin prepared by the chemical modification method is obtained.

[0043] The acid value refers to the mass fraction of KOH consumed by the acid component in each gram of sample.

[0044] The weight ratio of waterborne epoxy resin to curing agent is 2:1, and the curing agent used is polyamide curing agent.

[0045] The preparation method of the high-strength anti-corrosion coating is as follows: 100 parts by weight of waterborne epoxy resin prepared by a chemical modification method and 12 parts by weight of prepared dihydroxylbenzene tetracarboximide modified graphene oxide are added into a reaction container, mechanically stirred for 0.5 hours, and after the modified graphene oxide is evenly dispersed, 30 parts by weight of filler are added, and after stirring evenly, 10 parts by weight of toughening agent and 6 parts by weight of diluent are added, and mixed evenly; finally, 50 parts by weight of curing agent are added, and stirring is continued, and after sufficient mixing, the preparation and synthesis of the high-strength anti-corrosion coating is completed.

[0046] Example 2

[0047] A high-strength anti-corrosion coating is composed of the following components by weight: 14 parts of dinitrohydroxybenzene tetracarboximide-modified graphene oxide, 80 parts of water-based epoxy resin prepared by a chemical modification method, 40 parts of a curing agent, 10 parts of a toughening agent, 8 parts of a diluent, and 30 parts of a filler.

[0048] The toughening agent is epoxy oil and dimer fatty acid, and the weight ratio of the two is 1:1; the diluent is xylene.

[0049] The particle size of the filler used was 160-180 μm.

[0050] The weight ratio of graphene oxide to dinitrohydroxybenzene tetracarboximide is 1:3.

[0051] The preparation methods of modified graphene oxide, waterborne epoxy resin and high-strength anti-corrosion coating are all the same as those in Example 1.

[0052] Example 3

[0053] A high-strength anti-corrosion coating is composed of the following components by weight: 16 parts of dinitrohydroxybenzene tetracarboximide-modified graphene oxide, 100 parts of water-based epoxy resin prepared by a chemical modification method, 50 parts of a curing agent, 12 parts of a toughening agent, 8 parts of a diluent, and 40 parts of a filler.

[0054] The toughening agent is epoxy oil and the diluent is xylene.

[0055] The particle size of the filler used was 140-180 μm.

[0056] The weight ratio of graphene oxide to dinitrohydroxybenzene tetracarboximide is 1:3.

[0057] The preparation methods of modified graphene oxide, waterborne epoxy resin and high-strength anti-corrosion coating are all the same as those in Example 1.

[0058] Example 4

[0059] A high-strength anti-corrosion coating is composed of the following components by weight: 18 parts of dinitrohydroxybenzene tetracarboximide-modified graphene oxide, 100 parts of water-based epoxy resin prepared by a chemical modification method, 50 parts of a curing agent, 15 parts of a toughening agent, 10 parts of a diluent, and 40 parts of a filler.

[0060] The toughening agent is epoxy oil; the diluent is phthalic acid and xylene, and the weight ratio of the two is 1:1.

[0061] The particle size of the filler used was 160-200 μm.

[0062] The weight ratio of graphene oxide to dinitrohydroxybenzene tetracarboximide is 1:2.

[0063] The preparation methods of modified graphene oxide, waterborne epoxy resin and high-strength anti-corrosion coating are all the same as those in Example 1.

[0064] The coatings prepared in Examples 1 to 4 were subjected to a performance test. The coatings were sprayed, brushed or dipped on the surface of a clean workpiece, and the coating thickness was 0.3 to 0.5 mm. After the coating was applied, the coating was cured in a blast oven at 40 degrees Celsius for 12 hours, and then the coatings were uniformly tested for performance. The test results are shown in Table 1. The test method was performed in accordance with the relevant standards of GB22 / T 3432-2023.

[0065] Table 1 Coating performance test table

[0066]

[0067] After the test is completed, the surface coating of Example 1, Example 2, Example 3, and Example 4 is partially destroyed, but the surface of the workpiece is not destroyed. The above standard test is performed again. The performance indicators characterizing the corrosion resistance, oxygen permeability and water permeability are increased to a certain extent. The test results show that the destroyed coating still has strong corrosion resistance and is suitable for coping with various scenarios in practical applications.

[0068] Comparative Example 1

[0069] On the basis of Example 3, the dinitrohydroxypyromellitimide-modified graphene oxide in Example 3 was replaced with an equal amount of unmodified graphene oxide; the remaining operations were consistent with Example 3.

[0070] The coating prepared in Comparative Example 1 was subjected to the same performance test as the coating prepared in Example 3.

[0071] Comparative Example 2

[0072] On the basis of Example 3, the addition of dinitrohydroxypyromellitimide-modified graphene oxide was eliminated, and no other alternative raw materials were added.

[0073] The coating prepared in Comparative Example 2 was subjected to the same performance test as the coating prepared in Example 3.

[0074] Comparative Example 3

[0075] With reference to the Chinese invention patent with publication number CN113698847B, the coating composition disclosed therein was selected according to the optimal ingredients in the disclosed patent to prepare the coating of Comparative Example 3.

[0076] The coating prepared in Comparative Example 3 was subjected to the same performance test as the coating prepared in Example.

[0077] The performance tests of the coatings prepared in Comparative Example 1, Comparative Example 2, and Comparative Example 3 were carried out, and the coatings were sprayed, brushed, or dipped on the surface of a clean workpiece, with a coating thickness of 0.3-0.5 mm; after the coating was applied, the coating was cured in a blast oven at 40 degrees Celsius for 12 hours, and then the coatings were uniformly tested for performance; the test results are shown in Table 2; the test method was carried out in accordance with the relevant standards of GB22 / T 3432-2023.

[0078] Table 2 Comparative coating performance test table

[0079]

[0080] Result analysis: It can be seen from Table 1 that the coating prepared in this embodiment has a pencil hardness of at least 5H. The preferred embodiments, such as the formulas of Embodiment 2 and Embodiment 3, have a hardness of 6H and excellent compressive strength. The corrosion resistance is also excellent. The coating has high strength and can be more widely used in practice.

[0081] It can be seen from the test results in Table 2 that in Comparative Example 1, when the graphene oxide was not modified, its corrosion resistance was greatly reduced, and the coating had no defects after drying, but the 24h oxygen permeability value was too high to measure the data; its water permeability also increased significantly, and compared with the embodiments of the present invention, it obviously did not have excellent corrosion resistance.

[0082] Comparative Example 2 is a comparative example without adding graphene oxide. The test results show that the corrosion resistance of Comparative Example 2 is weak, and the oxygen permeability and water permeability are too large, and the specific values ​​cannot be obtained. The test results of Comparative Example 2 show that the modified graphene oxide added by the present invention significantly improves the anti-corrosion and strength performance of the coating.

[0083] Comparative Example 3 is a technical solution disclosed in the authorized patent. The coating strength of Comparative Example 3 is relatively weak and its practical application range is relatively narrow. The coating strength prepared by the technical solution of the present invention is more than 70% greater than that of the prior art, and has a wider application prospect than Comparative Example 3.

[0084] In summary, the high-strength anti-corrosion coating of the present invention introduces dinitrohydroxybenzene tetracarboximide to modify graphene oxide. The nitrogen hydroxyl group in the structure of dinitrohydroxybenzene tetracarboximide can chelate with the atoms on the metal surface to form a monomolecular protective film on the metal surface, which can effectively prevent corrosive media such as H2O and O2 from contacting the substrate, thereby actively slowing down the corrosion process of the metal; and dinitrohydroxybenzene tetracarboximide itself has the characteristics of an inhibitor, which can effectively prevent the stacking and agglomeration of graphene oxide, so that the modified graphene oxide can be fully and evenly dispersed in the resin to form a physical barrier; and it chelates with the metal atoms on the surface of the workpiece, even if the coating is destroyed, it has a strong anti-corrosion ability, and the two-dimensional structure of graphene is dispersed in the coating, which greatly enhances the strength of the coating, and the pencil hardness and compressive strength are both excellent.

[0085] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A high-strength anti-corrosion coating, characterized in that: The composition is as follows, by weight: 12 to 18 parts of dinitrohydroxypyromellitimide-modified graphene oxide, 80 to 110 parts of waterborne epoxy resin prepared by chemical modification, 40 to 55 parts of curing agent, 10 to 15 parts of toughening agent, 6 to 10 parts of diluent, and 30 to 40 parts of filler; The toughening agent includes at least one of epoxy oil and dimer fatty acid; The diluent includes: at least one of phthalic acid and xylene; The filler includes calcined kaolin, glass powder, talcum powder, and quartz powder, and the particle size of the filler is 120-200 μm; The dinitrohydroxypyromellitic imide is prepared by the following method: hydroxylamine hydrochloride and triethylamine are placed in a reaction container, an ethanol solution is added, and the mixture is stirred until the two are completely dissolved in the ethanol solution, and then pyromellitic anhydride is added for reflux reaction for 8 hours. After the reaction is completed, deionized water is added to precipitate the dinitrohydroxypyromellitic imide solid; the weight ratio of the ethanol to the deionized water is 1:1; The dinitrohydroxypyromellitimide modified graphene oxide is prepared by the following method: dispersing graphene oxide in deionized water, then adding dinitrohydroxypyromellitimide, and ultrasonically treating until the two are dispersed in the deionized water; heating the dispersed mixed solution to 80 degrees Celsius under magnetic stirring for 8 hours, centrifuging to obtain a precipitate, washing the obtained precipitate with deionized water, and finally drying to obtain the dinitrohydroxypyromellitimide modified graphene oxide; The weight ratio of graphene oxide to dinitrohydroxybenzene tetracarboximide is 1:2-1:

3.

2. The high-strength anti-corrosion coating as claimed in claim 1, characterized in that: The dinitrohydroxypyromellitimide modified graphene oxide is present in an amount of 14 to 16 parts by weight.

3. The high-strength anti-corrosion coating as claimed in claim 1, characterized in that: The filler is a mixed filler consisting of calcined kaolin, glass powder, talcum powder and quartz powder in a mass ratio of 1:4:4:

2.

4. The high-strength anti-corrosion coating as claimed in claim 1, characterized in that: The particle size of the filler is 140-180 μm.

5. The high-strength anti-corrosion coating as claimed in claim 1, characterized in that: The waterborne epoxy resin prepared by the chemical modification method is prepared by the following method: epoxy resin and acrylic acid are placed as raw materials in a reaction container, a catalyst is added, and the temperature is raised under nitrogen protection. When all the raw materials are melted, stirring is started; when the temperature of the reaction system reaches 110 degrees Celsius, the reaction temperature is maintained and the acid value is measured. When the acid value is lower than 5, the reaction reaches the end point, and the waterborne epoxy resin prepared by the chemical modification method is obtained; The catalyst is triphenylphosphine.

6. The high-strength anti-corrosion coating as claimed in claim 1, characterized in that: The graphene oxide is prepared by the following method: graphite powder and NaNO3 are added into a reaction container, concentrated sulfuric acid is slowly added, and after mechanical stirring for reaction for 0.5 hours, potassium permanganate powder is slowly added under ice bath conditions, and the reaction continues for 1 hour; after the reaction is completed, the ice bath is removed and the reaction is continued for 24 hours; deionized water is added dropwise for 0.5 hours; then hydrogen peroxide is added dropwise, the reaction is continued for 1 hour, and then the reaction is stopped, and the obtained product is freeze-dried to prepare graphene oxide.

7. The method for preparing the high-strength anticorrosive coating according to any one of claims 1 to 6, characterized in that: The preparation method of the high-strength anti-corrosion coating is as follows: adding a water-based epoxy resin prepared by a chemical modification method and the prepared dihydrogen hydroxybenzene tetracarboximide-modified graphene oxide into a reaction container, mechanically stirring for 0.5 hours, and after the modified graphene oxide is evenly dispersed, adding a filler, stirring evenly, adding a toughening agent and a diluent, and mixing evenly; finally, adding a curing agent, and continuing to stir, and the preparation and synthesis of the high-strength anti-corrosion coating is completed after sufficient mixing; the curing agent is a polyamide curing agent.