Biochar concrete and preparation method thereof
By adding ore powder and modified plant fiber compound to biochar concrete, the problem of deterioration of density and mechanical properties caused by high amount of biochar is solved, and the increase of biochar dosage and the enhancement of carbon emission reduction ability is achieved. .
Patent Information
- Application Number
- CN202311358919.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-10-19
AI Technical Summary
At high dosage, existing biochar concrete has reduced density and weakened crack barrier effect, resulting in a decrease in mechanical properties, reduced carbon emissions and limited carbon storage capacity.
By adding ore powder and modified plant fiber compound to the concrete, fill the pore structure of biochar, improve the adhesion and dispersion of biochar, reduce the agglomeration effect, and improve the density and mechanical properties of concrete, thereby increasing the biochar, thereby increasing the biochar. The amount of carbon is 3%-5% of the cement used.
It effectively improves the carbon emission reduction ability and carbon storage capacity of biochar concrete, while maintaining or improving the mechanical properties of concrete, avoiding the reduction of density and crack barrier effects caused by high amounts of biochar.
Smart Images

Figure BDA0004502726880000051 
Figure BDA0004502726880000081
Abstract
Description
Technical Field
[0001] The present application relates to the field of concrete, and in particular to a biochar concrete and a preparation method thereof. Background Art
[0002] Cement and its composite materials are the most commonly used hydraulic construction materials, important resources and commodities that affect economic development, and are still irreplaceable basic construction materials. It is estimated that the cement industry accounts for about 5-7% of all man-made carbon dioxide emissions. Therefore, while improving the strength of cement, using new materials to reduce or partially replace the use of cement is of great significance to my country's construction and environmental protection fields.
[0003] Although adding plant fibers such as raw rice husks or straw to cement can reduce the amount of cement used to a certain extent, it will not increase the strength of the cement. This is because plant fibers such as straw have a higher silicon content, but the silicon is amorphous and non-crystalline. In particular, 80-98% of the silicon in rice straw is in an amorphous form and cannot be hydrated with the minerals in cement to form a stable product.
[0004] Carbon sequestration is also a key technology to mitigate global warming. Biochar is also a form of carbon, but the current research on the sequestration and application of biochar is mainly concentrated in the field of soil improvement. Carbon sequestration in concrete means adding biochar to cement-based materials in a certain proportion. Since the life of concrete can reach 100 years, these carbons will form carbon sinks for a long time and no longer exchange carbon with carbon sources. This can basically achieve permanent sequestration, reduce the amount of cement used, and can seal part of the carbon, so it can effectively reduce carbon emissions; and, after high-temperature pyrolysis of plant fibers, it is found that the amorphous silicon in the plant fibers gradually changes to a crystalline state. Compared with the direct addition of crop raw materials, the addition of biochar formed by pyrolysis is more stable, which enhances the mechanical properties of concrete to a certain extent.
[0005] However, the amount of biochar added to concrete should not be too much. The reference "Study on Basic Mechanical Properties and Carbon Resistance of Hickory and Cattail Shell Biochar Concrete" mentioned that the amount of biochar added to concrete should not exceed 2% of the cement mass. This is because biochar itself has a porous structure. When biochar is added to the concrete mixture as a filler, when the amount of biochar added is too much, the number of primary pores introduced by biochar increases, which reduces the density of the concrete and causes strength loss; and biochar is prone to agglomeration effect. As the amount of biochar added increases and the agglomeration effect occurs, the crack barrier effect of fine particles is weakened, and the splitting tensile strength of concrete decreases, resulting in a decrease in toughness. Therefore, the current ability of adding biochar to concrete to reduce carbon emissions and store carbon is still limited. Summary of the invention
[0006] In order to ensure the mechanical properties of concrete while improving the carbon emission reduction and carbon sequestration capabilities of biochar concrete, the present application provides a biochar concrete.
[0007] The biochar concrete provided in this application adopts the following technical solution:
[0008] A biochar concrete comprises the following components and their weight parts:
[0009] Composite cement admixture 530-560 parts, fine aggregate 608-614 parts, coarse aggregate 1129-1140 parts, water 210-220 parts;
[0010] The composite cement admixture comprises a composite admixture of cement: biochar powder: mineral powder: fiber in a mass ratio of 1: (0.032-0.056): (0.12-0.16): (0.064-0.084);
[0011] The particle size of the mineral powder is L1, the pore size of the biochar powder is L2, both L1 and L2 are micrometer-sized, and L2 is smaller than L1;
[0012] The fiber composite admixture comprises plant fiber, modified plant fiber and acrylic adhesive, wherein the modified plant fiber is obtained by subjecting the plant fiber to surface modification treatment.
[0013] By adopting the above technical solution, after biochar is added to concrete, due to the porous structure of the biochar particles, a part of the volume of the cement matrix is occupied by the voids in the biochar in the form of pores, and the concrete is mixed with mineral powder, and the particle size of the added mineral powder is smaller than the pore size of the biochar powder. During the concrete mixing and molding process, the mineral powder can fill and support the pores of the biochar powder to reduce the number of primary pores introduced by the biochar, thereby reducing the formation of more capillary networks in the gel mechanism of the concrete, which causes the density of the concrete to decrease and the degree of mechanical properties to decrease.
[0014] At the same time, the surface of the plant fiber itself is distributed with hydroxyl groups. After pyrolysis carbonization treatment, cellulose, hemicellulose, protein, fat, etc. in the biomass form many oxygen-containing functional groups, thereby forming a large number of functional groups such as carboxyl and carbonyl on the surface and inside of the biochar. The hydroxyl group and the carboxyl group have good affinity, which can greatly increase the adhesion between the plant fiber and the biochar powder, so that the biochar particles can adhere to and combine with the modified plant fiber. Acrylic glue allows the plant fiber and the modified plant fiber to be bonded and mixed with each other. After surface modification, the modified plant fiber is obtained, the surface of the modified plant fiber becomes rough, and the interface bonding performance of the modified plant fiber is improved, which is more conducive to the dispersion of the plant fiber and the modified plant fiber in the concrete, so that the biochar that is adhered and combined with the plant fiber is not easy to agglomerate in the concrete, and has a better dispersion effect, thereby reducing the crack barrier effect of fine particles in the concrete caused by the high amount of biochar, and the splitting tensile strength of the concrete is reduced, resulting in a decrease in toughness.
[0015] From the above, it can be concluded that the addition of mineral powder and fiber composite admixtures can reduce the impact of high biochar content on the density of concrete and the weakening of the crack barrier effect, thereby reducing the impact of increased biochar content on the mechanical properties of concrete to a certain extent. Therefore, the content of biochar in concrete can be increased to about 3%-5% of the amount of cement used, so as to improve the carbon emission reduction and carbon sequestration capabilities of biochar concrete to a certain extent.
[0016] Optionally, the preparation process of the modified plant fiber comprises the following steps:
[0017] In an alkaline solution, the colloid on the surface of the plant fiber is removed by sodium sulfate and sodium pyrophosphate, then it is acid-washed and washed with water, and finally processed into filaments, dried, and taken out for use;
[0018] A silane coupling agent is added to the alcohol solution in a certain proportion, and the pH value of the solution is adjusted to 4.0-4.5. The treated plant fiber is placed in the solution and soaked for 1-2 hours. The plant fiber is taken out and dried continuously to obtain the modified plant fiber.
[0019] By adopting the above technical solution, the colloid on the surface of the plant fiber can be removed and the hydrogen bonds can be broken, thereby improving the roughness of the surface of the plant fiber.
[0020] Optionally, the mass ratio of the plant fiber, modified plant fiber and acrylic adhesive is 1:(2.4-2.8):(1.2-1.4).
[0021] By adopting the above technical solution and the above input ratio, the plant fibers can be fully adhered and combined with the biochar, and it is more conducive to the dispersion of the plant fibers and modified plant fibers in concrete.
[0022] Optionally, the preparation process of the fiber composite admixture comprises the following steps:
[0023] First, the plant fiber and one third of the acrylic adhesive are homogenized and stirred at a stirring speed of 100-130 r / min for 4-6 min, and then the modified plant fiber and the remaining acrylic adhesive are added and the homogenization stirring is continued for 15-18 min to obtain a fiber composite admixture.
[0024] Optionally, the fineness of the biochar is 200-220 mesh.
[0025] By adopting the above technical solution, the biochar of the above fineness can better fill and support the pores formed during the solidification process of the cement substrate, so as to improve the density of the concrete to a certain extent.
[0026] Optionally, the biochar is at least one of highland barley straw ash, corn straw, wheat straw, rice straw, cotton straw and soybean straw.
[0027] Optionally, the biochar is prepared by:
[0028] First, the cleaned biochar raw material is crushed and dried, and then pyrolyzed in an oxygen-limited environment at 280-320°C. The pyrolysis process takes about 1-3 hours, and it is completely carbonized to form biochar particles. Finally, it is naturally cooled to room temperature, ground into fine particles and sieved to obtain biochar.
[0029] By adopting the above technical solution, the pores of the biochar formed by pyrolysis and carbonization at the above temperature are mainly macropores and mesopores, so as to reduce the possibility that the biochar is formed with too many micropores and the mineral powder is difficult to fill and support the pores of the biochar.
[0030] Optionally, the fineness of the mineral powder is 1350-1500 mesh.
[0031] By adopting the above technical scheme, the macropore radius of biochar is usually ≥20μm, the mesopore radius is usually 0.15-20μm, and the particle size of the mineral powder with a fineness of 1350-1500 mesh is usually around 9-10μm. It can fill and support the macropores and part of the mesopores of biochar without easily causing agglomeration effect due to excessive fineness and small particle size.
[0032] Optionally, the mineral powder is at least one of zeolite powder, montmorillonite powder, wollastonite and talc powder.
[0033] In a second aspect, the present application provides a method for preparing biochar concrete using the following technical solution:
[0034] A method for preparing biochar concrete comprises the following steps:
[0035] The biochar powder, mineral powder and fiber admixture are mixed and stirred in proportion until the mixture is uniform, and then one-fourth of the water and one-half of the cement are added according to the proportion required, and the mixture is stirred for the first time until the mixture is uniform;
[0036] Coarse aggregate and fine aggregate, as well as the remaining water and cement, are added and stirred for a second time until the mixture is uniform. The uniformly stirred concrete mixture is placed in a precast mold and vibrated and cured to obtain concrete.
[0037] By adopting the above technical solution, by adding the components in batches
[0038] Stirring is performed so that the biochar powder adheres to and combines with the mineral powder and fiber composite admixture first, and then is stirred and mixed with the coarse aggregate and the fine aggregate, so that the mineral powder can better fill and support the porous structure of the biochar powder, and the biochar is dispersed in the concrete.
[0039] Optionally, the stirring speeds of the first stirring and the second stirring are both 8-12 r / min, the stirring time of the first stirring is 2-5 min, and the stirring time of the second stirring is 5-7 min.
[0040] In summary, the present application includes at least one of the following beneficial technical effects:
[0041] 1. By adding mineral powder and fiber composite admixtures, the effect of high biochar content on the density of concrete and the weakening of crack barrier effect can be reduced, thereby reducing the impact of increased biochar content on the mechanical properties of concrete to a certain extent. Therefore, the content of biochar in concrete can be relatively increased to enhance the carbon emission reduction and carbon sequestration capabilities of biochar concrete; 2. Biochar with a fineness of 200-220 mesh can better fill and support the pores formed during the solidification process of the cement matrix, thereby improving the density of concrete to a certain extent. DETAILED DESCRIPTION
[0042] 1. Implementation
[0043] Embodiment 1:
[0044] Preparation of modified plants:
[0045] The corn stalk fiber was boiled for 2 hours in a solution with an alkali concentration of 30 g / L, a Na2SO4 concentration of 1 g / L, and a sodium pyrophosphate concentration of 0.5 g / L to remove the colloid on the surface of the corn stalk fiber, then acid-washed and washed with water, and finally processed into filaments, dried at 70°C for 5 hours, and taken out for use;
[0046] Add 0.6% KH-550 silane coupling agent to 95% ethanol aqueous solution at a ratio of 6:4, mix thoroughly for 1 hour, adjust the pH to 4 with acetic acid, soak the treated corn stalk fiber in the solution for 1.5 hours, take out the corn stalk fiber and dry it in a constant temperature oven at 70°C;
[0047] The diameter of corn straw fiber is 40-50μm.
[0048] Preparation of fiber composite admixture:
[0049] Prepare 10g corn straw fiber, 26g of the modified plant fiber prepared above and 13g of acrylic glue, that is, the mass ratio of corn straw fiber, modified plant fiber and acrylic glue is 1:2.6:1.3;
[0050] First, 10 g corn straw fiber and 4 g acrylic glue were added into a stirring kettle for homogenization stirring at a stirring speed of 120 r / min for 5 min.
[0051] Then, 26 g of modified plant fiber and the remaining acrylic adhesive were added, and the mixture was stirred homogenously at a stirring speed of 120 r / min for 18 min to obtain a fiber composite admixture.
[0052] The diameter of corn straw fiber is 40-50μm.
[0053] Biochar preparation:
[0054] First, the cleaned highland barley straw is crushed to obtain highland barley straw ash, dried, and then pyrolyzed in an oxygen-limited environment at 300°C for about 2 hours to completely carbonize it to generate biochar particles. Finally, it is naturally cooled to room temperature, ground into fine particles and sieved to obtain biochar;
[0055] The biochar with a fineness of 210 mesh was obtained by sieving.
[0056] Concrete preparation:
[0057] Prepare 420g of cement, 20g of biochar powder, 60g of zeolite powder, and 30g of fiber composite admixture, that is, the mass ratio of cement, biochar powder, mineral powder, and fiber composite admixture is 1:0.048:0.14:0.072, wherein the strength of cement is 42.5, and the fineness of zeolite powder is 1400 mesh;
[0058] Then prepare 210g water, 608g fine aggregate, and 1129g coarse aggregate, wherein the fine aggregate is river sand with a particle size of 0-4.75mm, and the coarse aggregate is crushed stone with a particle size of 4.75-31.5mm;
[0059] 20g of biochar powder, 60g of zeolite powder and 30g of fiber composite admixture are put into a mixing drum and mixed until uniformly mixed. Then, 84g of ethanol and 210g of cement are added for the first mixing at a stirring speed of 10r / min and a stirring time of 4min. Then, 608g of fine sand, 1129g of gravel, and the remaining water and cement are added for the second mixing at a stirring speed of 10r / min and a stirring time of 6min. The uniformly mixed concrete mixture is loaded into a prefabricated mold, vibrated and compacted, and a concrete specimen is obtained after curing.
[0060] Embodiment 2-3:
[0061] A biochar concrete, the differences from Example 1 are shown in Table 1.
[0062] Table 1:
[0063]
[0064] Embodiment 4:
[0065] A biochar concrete, which is different from Example 2 in that the mass ratio of cement, biochar powder, mineral powder and fiber composite admixture is 1:0032:0.12:0.064.
[0066] Embodiment 5:
[0067] A biochar concrete, which is different from Example 2 in that the mass ratio of cement, biochar powder, mineral powder and fiber composite admixture is 1:0056:0.16:0.084.
[0068] Embodiment 6:
[0069] A biochar concrete, which is different from Example 2 in that the mass ratio of plant fiber, modified plant fiber and acrylic adhesive is 1:2.4:1.2.
[0070] Embodiment 7:
[0071] A biochar concrete, which is different from Example 2 in that the mass ratio of plant fiber, modified plant fiber and acrylic adhesive is 1:2.8:1.4.
[0072] Embodiment 8:
[0073] A biochar concrete, which is different from Example 2 in that: during the preparation of the biochar, pyrolysis is carried out in an oxygen-limited environment at 280°C.
[0074] Embodiment 9:
[0075] A biochar concrete, which is different from Example 2 in that: during the preparation of the biochar, pyrolysis is carried out in an oxygen-limited environment at 320°C.
[0076] Embodiment 10:
[0077] A biochar concrete, which is different from Example 2 in that: the fineness of the biochar is 200 mesh.
[0078] Embodiment 11:
[0079] A biochar concrete, which is different from Example 2 in that: the fineness of the biochar is 220 mesh.
[0080] Embodiment 12:
[0081] A biochar concrete, which is different from Example 2 in that: the fineness of the zeolite powder is 1350 mesh.
[0082] Embodiment 13:
[0083] A biochar concrete, which is different from Example 2 in that: the fineness of the zeolite powder is 1500 mesh.
[0084] 2. Comparison
[0085] Comparative Example 1:
[0086] The difference from Example 2 is that the composite cement admixture only includes cement and biochar powder, and the mass ratio of cement to biochar powder is 1:0.02.
[0087] Comparative Example 2:
[0088] The difference from Example 2 is that the zeolite powder in the composite cement admixture is replaced by cement in an equal amount.
[0089] Comparative Example 3:
[0090] The difference from Example 2 is that the fiber composite admixture in the composite cement admixture is replaced by cement in equal amount.
[0091] Comparative Example 4:
[0092] The difference from Example 2 is that the mass ratio of cement, biochar powder, mineral powder and fiber composite admixture is 1:0064:0.18:0.095.
[0093] Comparative Example 5:
[0094] The difference from Example 2 is that the modified plant fiber in the fiber composite admixture is replaced by plant fiber in equal amounts.
[0095] Comparative Example 6:
[0096] The difference from Example 2 is that the mass ratio of the plant fiber, the modified plant fiber and the acrylic adhesive is 1:2:1.
[0097] Comparative Example 7:
[0098] The difference from Example 2 is that the mass ratio of plant fiber, modified plant fiber and acrylic adhesive is 1:3:1.6.
[0099] Comparative Example 8:
[0100] The difference from Example 2 is that during the process of preparing biochar, pyrolysis is carried out in an oxygen-limited environment at 600°C.
[0101] Comparative Example 9:
[0102] The difference from Example 2 is that the fineness of the zeolite powder is 1600 mesh.
[0103] Comparative Example 10:
[0104] The difference from Example 2 is that the fineness of the zeolite powder is 1000 mesh.
[0105] Comparative Example 11:
[0106] The difference from Example 2 is that all the prepared cement, biochar powder, zeolite powder, fiber composite admixture, fine aggregate and coarse aggregate are directly put into the mixing drum for mixing and stirring at a stirring speed of 10 r / min and a stirring time of 10 min.
[0107] 3. Performance testing method:
[0108] 1) The compressive strength of the concrete specimens of Examples 1-13 and Comparative Examples 1-8 was tested with reference to the compressive strength test method in GB / T 50081-2019 Standard for Test Methods for Physical and Mechanical Properties of Concrete. The test results are shown in Table 2;
[0109] 2) The splitting tensile strength test method of the concrete specimens of Examples 1-13 and Comparative Examples 1-8 was tested with reference to the splitting tensile strength test method in GB / T 50081-2019 Standard for Test Methods for Physical and Mechanical Properties of Concrete. The test results are shown in Table 2;
[0110] 3) The flexural strength of the concrete specimens of Examples 1-13 and Comparative Examples 1-8 was tested with reference to the flexural strength test method in GB / T 50081-2019 Standard for Test Methods for Physical and Mechanical Properties of Concrete. The test results are shown in Table 2;
[0111] 4) The bulk density of the concrete specimens of Examples 1-13 and Comparative Examples 1-8 was tested with reference to the hardened concrete density test method in the "GB / T 50081-2019 Standard for Test Methods for Physical and Mechanical Properties of Concrete". The test results are shown in Table 2.
[0112] Table 2:
[0113]
[0114] 4. Results Analysis and Summary
[0115] Combining Examples 1-3 and Table 2, it can be seen that, in combination with Comparative Example 1, the composite cement admixture of Comparative Example 1 only includes cement and biochar powder, and the mass ratio of cement to biochar powder is 1:0.02, that is, the amount of biochar powder added is 2% of the amount of cement used, which is the limit value of the amount of biochar powder added provided in the current literature. It can be seen from Table 2 that the compressive strength, splitting tensile strength, flexural strength and bulk density of the concrete of Examples 1-3 are similar to those of Comparative Example 1, which indicates that the mechanical properties of the concrete of Examples 1-3 are almost not lost compared to ordinary concrete.
[0116] Moreover, the weight portions of the composite cement admixture, fine aggregate, coarse aggregate and water in Examples 1-3 are all different. As can be seen from Table 2, the compressive strength, splitting tensile strength, flexural strength and bulk density of the concrete prepared by the weight of the composite cement admixture, fine aggregate, coarse aggregate and water in Example 2 are all higher than those in Example 1 and Example 3. As can be seen from the above, the mechanical properties of the biochar concrete formed by mixing and curing 546 parts of composite cement admixture, 611 parts of fine aggregate, 1134 parts of coarse aggregate and 215 parts of water are relatively better.
[0117] In combination with Example 2, Examples 4-5, Comparative Example 1 and Table 2, it can be seen that the mass ratios of cement, biochar powder, mineral powder and fiber composite admixture in the composite cement admixture of Examples 4-5 are different from those in Example 2. It can be seen from Table 2 that the compressive strength, splitting tensile strength, flexural strength and bulk density of Examples 4-5 are not much different from those of Example 2 and Comparative Example 1.
[0118] In addition, in combination with Comparative Examples 2-4, the zeolite powder in the composite cement admixture in Comparative Example 2 is replaced by cement in an equal amount, the fiber composite admixture in the composite cement admixture in Comparative Example 3 is replaced by cement in an equal amount, and the mass ratio of cement, biochar powder, mineral powder and fiber composite admixture in Comparative Example 4 is outside the scope of the present application. It can be seen from Table 2 that the compressive strength, splitting tensile strength, flexural strength and bulk density of Comparative Examples 2-4 are significantly lower than those of Examples 2 and 4-5.
[0119] From the above, it can be concluded that the compound use of cement, biochar powder, mineral powder and fiber composite admixtures can guarantee the mechanical properties of biochar concrete to a certain extent, and the mass ratio of cement, biochar powder, mineral powder and fiber composite admixture in the composite cement admixture is in the range of 1: (0.022-0.046): (0.12-0.18): (0.014-0.034), which can better guarantee the mechanical properties of concrete with a higher amount of biochar.
[0120] Combining Example 2, Examples 6-7 and Table 2, it can be seen that the mass ratios of plant fiber, modified plant fiber and acrylic adhesive in the fiber composite admixture are different from those in Example 2. As can be seen from Table 2, the compressive strength, splitting tensile strength, flexural strength and bulk density of the concrete prepared in Examples 6-7 are lower than those in Example 2.
[0121] In combination with Comparative Examples 5-7, it can be seen that the modified plant fibers in the fiber composite admixture of Comparative Example 5 are replaced by plant fibers in equal amounts, while the mass ratios of plant fibers, modified plant fibers and acrylic adhesive in Comparative Examples 6-7 are all outside the scope of the present application. It can be seen from Table 2 that the compressive strength, splitting tensile strength, flexural strength and volume density of the concrete prepared in Comparative Examples 5-7 are significantly lower than those in Example 2 and Example 6-7.
[0122] From the above, it can be concluded that the compounding and incorporation of plant fiber, modified plant fiber and acrylic adhesive according to the mass ratio range of this application can better guarantee the mechanical properties of biochar concrete, and when the mass ratio of plant fiber, modified plant fiber and acrylic adhesive is 1:2.6:1.3, the mechanical properties of concrete with a higher amount of biochar can be better guaranteed.
[0123] Combining Example 2, Examples 8-9 and Table 2, it can be seen that the pyrolysis temperature in the biochar preparation process of Examples 8-9 is different from that of Example 2. It can be seen from Table 2 that the compressive strength, splitting tensile strength, flexural strength and bulk density of the concrete of Examples 8-9 are all lower than those of Example 2. And combined with Comparative Example 8, the pyrolysis temperature in the biochar preparation process of Comparative Example 8 is outside the pyrolysis temperature range of the present application. It can be seen from Table 2 that the compressive strength, splitting tensile strength, flexural strength and bulk density of the concrete of Comparative Example 8 are significantly lower than those of Examples 2 and Examples 8-9.
[0124] From the above, it can be concluded that the pyrolysis temperature in the biochar preparation process is within 280-320°C, which can better guarantee the mechanical properties of concrete with a higher biochar content; and the pyrolysis temperature of 300°C can better guarantee the mechanical properties of concrete with a higher biochar content.
[0125] Combining Example 2, Example 12-13 and Table 2, it can be seen that the fineness of the mineral powder in Example 12-13 is different from that in Example 2. It can be seen from Table 2 that the compressive strength, splitting tensile strength, flexural strength and bulk density of the concrete prepared in Example 12-13 are similar to those in Example 2. Combining Comparative Examples 9-10, the fineness of the mineral powder in Comparative Examples 9-10 is outside the fineness range of the mineral powder in this application. It can be seen from Table 2 that the compressive strength, splitting tensile strength, flexural strength and bulk density of the concrete in Comparative Examples 9-10 are significantly lower than those in Example 2 and Example 12-13. It can be obtained from the above that the fineness of the mineral powder in the composite cement admixture is between 1350-1500 mesh, which can provide a better guarantee for the mechanical properties of concrete with a higher biochar content.
[0126] Combining Example 2, Comparative Example 11 and Table 2, it can be seen that the concrete preparation process of Comparative Example 11 is different from that of Example 2. From Table 2, it can be seen that the compressive strength, splitting tensile strength, flexural strength and bulk density of the concrete prepared in Comparative Example 11 are significantly lower than those in Example 2. As can be seen from the above, in the present application, the components are added in batches for stirring, so that the biochar powder can be first adhered and combined with the mineral powder and the fiber composite admixture, so as to better guarantee the mechanical properties of the concrete with a higher biochar content.
[0127] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, all equivalent changes made according to the products, methods, and principles of the present application should be included in the protection scope of the present application.
Claims
1. A biochar concrete, characterized in that: Includes the following components and their contents: Composite cement admixture 530-560 parts, fine aggregate 608-614 parts, coarse aggregate 1129-1140 parts, water 210-220 parts; The composite cement admixture comprises a composite admixture of cement: biochar powder: mineral powder: fiber in a mass ratio of 1: (0.032-0.056): (0.12-0.16): (0.064-0.084); The particle size of the mineral powder is L1, the pore size of the biochar powder is L2, both L1 and L2 are micrometer-sized, and L2 is smaller than L1; The fiber composite admixture comprises plant fiber, modified plant fiber and acrylic glue; The preparation process of the modified plant fiber comprises the following steps: In an alkaline solution, the colloid on the surface of the plant fiber is removed by sodium sulfate and sodium pyrophosphate, then it is acid-washed and washed with water, and finally processed into filaments, dried, and taken out for use; A silane coupling agent is added to the alcohol solution in a certain proportion, and the pH value of the solution is adjusted to 4.0-4.
5. The treated plant fiber is placed in the solution and soaked for 1-2 hours. The plant fiber is taken out and dried continuously to obtain the modified plant fiber.
2. The biochar concrete according to claim 1, characterized in that: The mass ratio of the plant fiber, the modified plant fiber and the acrylic adhesive is 1:(2.4-2.8):(1.2-1.4).
3. The biochar concrete according to claim 1, characterized in that: The preparation process of the fiber composite admixture comprises the following steps: First, the plant fiber and one third of the acrylic adhesive are homogenized and stirred at a stirring speed of 100-130 r / min for 4-6 min, and then the modified plant fiber and the remaining acrylic adhesive are added and the homogenization stirring is continued for 15-18 min to obtain a fiber composite admixture.
4. The biochar concrete according to claim 1, characterized in that: The fineness of the biochar is 200-220 meshes.
5. The biochar concrete according to claim 4, characterized in that: The preparation steps of the biochar are: First, the cleaned biochar raw material is crushed and dried, and then pyrolyzed in an oxygen-limited environment at 280-320°C for 1-3 hours to completely carbonize it into biochar particles. Finally, it is naturally cooled to room temperature, ground into fine particles and sieved to obtain biochar.
6. The biochar concrete according to claim 1, characterized in that: The fineness of the mineral powder is 1350-1500 mesh.
7. The biochar concrete according to claim 6, characterized in that: The mineral powder is at least one of zeolite powder, montmorillonite powder, wollastonite and talc powder.
8. A method for preparing biochar concrete according to any one of claims 1 to 7, characterized in that: The following steps are involved: The biochar powder, mineral powder and fiber admixture are mixed and stirred in proportion until the mixture is uniform, and then one-fourth of the water and one-half of the cement are added according to the proportion required, and the mixture is stirred for the first time until the mixture is uniform; Coarse aggregate and fine aggregate, as well as the remaining water and cement, are added and stirred for a second time until the mixture is uniform. The uniformly stirred concrete mixture is placed in a precast mold and vibrated and cured to obtain concrete.
9. The method for preparing biochar concrete according to claim 8, characterized in that: The stirring speeds of the first stirring and the second stirring are both 8-12 r / min, the stirring time of the first stirring is 2-5 min, and the stirring time of the second stirring is 5-7 min.
Citation Information
Patent Citations
High-hardness thermal-insulation plant fiber cement composite ribbon board and manufacturing method thereof
CN105060811A
Sulfate-erosion-resistant plant fiber concrete and preparation method thereof
CN116535151A