A method for preparing light-blocking masterbatch and PETG heat-shrinkable label film
By using a mixture of riboflavin and carotenoids with surface-coated polydopamine layer as light barrier masterbatch in dairy product packaging, a high-performance PETG heat shrinkable label film was prepared, which solved the rancidity of dairy products caused by photooxidation in the prior art in the prior art The problem has significantly improved the fresh preservation effect of dairy products.
Patent Information
- Application Number
- CN202311279368.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-10-07
AI Technical Summary
The heat shrinkable label film in existing dairy product packaging cannot effectively block light oxidation, resulting in the easy runny dairy product and affecting taste and quality.
A mixture of riboflavin and carotenoids coated with a polydopamine layer surface is used as the light-blocking masterbatch, and added it to the core layer of the PETG heat-shrinking label film. A high-performance light-blocking label film is prepared by a flat film method. Improve its ability to absorb visible and ultraviolet light.
It significantly improves the light-blocking and barrier properties of the label film, enhances the protective effect on dairy products, reduces rancidity caused by photooxidation, and extends the shelf life of dairy products.
Smart Images

Figure BDA0004477917520000041 
Figure BDA0004477917520000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat shrinkable label film preparation, and in particular relates to a preparation method of a light-blocking barrier masterbatch and a PETG heat shrinkable label film. Background Art
[0002] The main nutrients of milk are fatty acids, protein, lactose, vitamins, minerals, etc. The fat in milk generally exists in the form of fat globules or free fat. Under the action of oxidation, lipase is activated and the milk fat is decomposed by lipase to produce free fatty acids, which brings about the sour smell and rancid smell of fat decomposition, which seriously affects the normal taste of milk.
[0003] Most dairy products are packaged in bottles, and dairy product packaging has extremely high requirements for light blocking, because: photooxidation is the main cause of milk fat oxidation in milk. Milk can absorb part of visible light or ultraviolet light, causing milk fat to undergo photooxidation, which promotes the rancidity of dairy products. The degree of rancidity of milk is related to the wavelength, intensity and duration of light, as well as the dissolved oxygen content of the product. Riboflavin (one of the vitamins in milk) is the main photosensitizer in milk and can promote the photooxidation process of milk fat. Therefore, the wrapping sleeve label (i.e., heat shrink label film) used in dairy product packaging, if it has good light blocking performance, can provide a protective barrier for the dairy products in the bottle. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a light-blocking barrier masterbatch and a PETG heat-shrinkable label film.
[0005] A method for preparing a mixture of riboflavin and carotenoids with a surface coated with a polydopamine layer comprises the following steps:
[0006] Step 1, weigh a set mass of dopamine hydrochloride into deionized water, and stir until the dopamine hydrochloride is dissolved to prepare an aqueous solution of dopamine hydrochloride;
[0007] Step 2, adding 10% by mass sodium hydroxide solution to the aqueous solution of dopamine hydrochloride and stirring, and adjusting the pH of the aqueous solution of dopamine hydrochloride to a set value;
[0008] Step 3, weighing a set amount of riboflavin and carotenoids, adding them to the solution prepared in step 2, heating the solution to a set temperature and stirring for a certain period of time;
[0009] Step 4: Add a set amount of dilute hydrochloric acid to the reaction solution of step 3, adjust the pH of the reaction solution to a set value, filter by suction, rinse the filter layer with deionized water, and vacuum dry to obtain a riboflavin and carotenoid mixture coated with a polydopamine layer.
[0010] As a preference:
[0011] The addition ratio of dopamine hydrochloride in step 1 to the total addition ratio of riboflavin and carotenoids in step 3 is 1:5, and the addition ratio of riboflavin and carotenoids is 1:1;
[0012] Step 2: adjusting the pH value of the dopamine hydrochloride aqueous solution to 8;
[0013] In step 3, the solution is heated to 30° C. and stirred for 30 to 45 minutes;
[0014] In step 4, dilute hydrochloric acid is added to adjust the pH of the reaction solution to 7, and the solution is filtered by suction. The filter layer is rinsed with deionized water for 2 to 3 times, and vacuum dried at 75° C. for 4 to 6 hours in a vacuum dryer.
[0015] A light-blocking masterbatch comprising a mixture of riboflavin and carotenoids coated with a polydopamine layer on the surface, comprising the following components in parts by mass:
[0016] PETG powder 67-77 parts;
[0017] Nano-montmorillonite 5-10 parts;
[0018] 3.75-5 parts of rutile (R-type) titanium dioxide;
[0019] 3.75-5 parts of ZnO powder;
[0020] 7.5 to 10 parts of a mixture of riboflavin and carotenoids coated with a polydopamine layer;
[0021] 2 parts of antioxidant 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate);
[0022] 1 to 2 parts of phosphite antioxidant.
[0023] Preferably, the average wafer thickness of the nano-montmorillonite is less than 25 nm, the montmorillonite content in the nano-montmorillonite is greater than 95%; the density of the rutile titanium dioxide is 4.26 g / cm 3 , refractive index is 2.72; the purity of titanium dioxide in rutile titanium dioxide is ≥99%; the purity of ZnO in ZnO powder is ≥99%; the phosphite antioxidant is triphenyl phosphite or trimethyl phosphite.
[0024] A method for preparing a light-blocking PETG heat-shrinkable label film by using a light-blocking masterbatch, wherein the heat-shrinkable label film is prepared by a flat film method, and the heat-shrinkable label film comprises a surface layer A, a core layer and a surface layer B from top to bottom, and the thickness ratio of the surface layer A, the core layer and the surface layer B is 10-15:70-80:10-15; the preparation method comprises the following steps:
[0025] Step 1, grinding the PETG powder at low temperature; weighing nano-montmorillonite, rutile titanium dioxide, ZnO powder, a mixture of riboflavin and carotenoids coated with a polydopamine layer, antioxidant 1010 and phosphite antioxidant according to set weight proportions, adding them together with the ground PETG powder into a high-speed mixer, and mixing them evenly;
[0026] Step 2, adding the material obtained in step 1 into a twin-screw extruder for granulation to prepare a light-blocking masterbatch;
[0027] Step 3, in terms of mass fraction, the extrusion raw materials of the extruders corresponding to the surface layer A and the surface layer B are prepared according to the following chemical components: 98% of PETG raw materials and 2% of open and smooth masterbatch; the extrusion raw materials of the extruder corresponding to the core layer are prepared according to the following chemical components: 90-94% of PETG raw materials and 6-10% of light-blocking masterbatch;
[0028] Step 4, conveying the extrusion raw materials corresponding to the surface layer A and the surface layer B to the extruder A for plasticization, and conveying the extrusion raw materials corresponding to the core layer to the extruder B for plasticization; respectively metering the extrusion raw materials corresponding to the surface layer A and the surface layer B after extrusion plasticization and the extrusion raw materials corresponding to the core layer by a metering pump, and then filtering through a filter, entering the convection flow channel of the distributor before the die through a melt pipe to merge into one, casting through the die head onto the casting cold roller, casting through the casting cold roller, transversely stretching the casting in the transverse stretching zone, shaping the film in the process of forming in the rear section of the transverse stretching, pulling the stretched film, and then winding the pulled film through a winder, inspecting and packaging the wound film to obtain a light-blocking PETG heat shrinkable label film.
[0029] Preferably, the particle size of the PETG powder after cryogenic grinding in step 1 is 125 mesh.
[0030] Preferably, in step 4: the plasticizing temperature of extruder A and extruder B is 245-270°C, the temperature of the die head is 265-270°C; the casting cold roller is equipped with cooling water, and the inlet temperature of the casting cold roller cooling water is 28°C.
[0031] Preferably, in step 4, the transverse stretching zone is provided with a preheating zone, a stretching zone, a shaping zone and a cooling zone; the temperature of the preheating zone is 90-115°C, the temperature of the stretching zone is 85-95°C, the temperature of the shaping zone is 70-82°C, and the temperature of the cooling zone is 40-45°C.
[0032] Preferably, the transverse stretching ratio of the transverse stretching zone in step 4 is 1:5.2.
[0033] The beneficial effects of the present invention are:
[0034] The present invention forms a layer of polydopamine PDA by polymerizing the surface of the mixture of riboflavin and carotenoids, which can improve the light-blocking performance of riboflavin and carotenoids and reduce the damage to the effective structure during the molding process.
[0035] The present invention develops a light-blocking barrier masterbatch comprising a mixture of riboflavin and carotenoids coated with a polydopamine layer on the surface, and adds the light-blocking barrier masterbatch into the core layer material formula of PETG heat shrinkable label film in a certain proportion, which can improve the light-blocking barrier performance of the label film, thereby enhancing its protective effect and effect on the packaged dairy products.
[0036] The light-blocking barrier masterbatch prepared by the present invention uses a mixture of riboflavin and carotenoids with a surface-coated polydopamine layer as a light-absorbing substance, and the light-absorbing substance can absorb or shield visible light and ultraviolet light in a wavelength range that has a greater impact on milk; and the light-blocking barrier masterbatch and montmorillonite with good barrier function are jointly prepared into a PETG heat shrinkable label film with high light-blocking property. DETAILED DESCRIPTION
[0037] The present invention is further described below in conjunction with embodiments. The description of the following embodiments is only used to help understand the present invention. It should be noted that for ordinary persons in the art, without departing from the principle of the present invention, the present invention can also be modified in some ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0038] Example 1
[0039] A method for preparing a mixture of riboflavin and carotenoids with a surface coated with a polydopamine layer comprises the following steps:
[0040] (1) Weigh 10 g of dopamine hydrochloride and add it to 300 ml of deionized water, stirring until the dopamine hydrochloride is dissolved to prepare an aqueous solution of dopamine hydrochloride; after the dopamine hydrochloride is dissolved in water, the hydrochloric acid is converted into chloride ions and hydrogen ions to obtain a dopamine monomer solution; the dopamine hydrochloride (DA, 98%) used in this example was purchased from Aladdin Reagent (Shanghai) Co., Ltd.;
[0041] (2) adding a 10% by mass sodium hydroxide solution to the aqueous solution of dopamine hydrochloride and stirring for 3 minutes to adjust the pH value of the aqueous solution of dopamine hydrochloride to 8;
[0042] Dopamine monomer solution, under alkaline conditions of pH>7.5, uses oxygen in the air as an oxidant. The reaction process does not require complicated experimental instruments and steps. When an appropriate amount of alkaline solution (such as sodium hydroxide) is added to the dopamine monomer solution, a self-polymerization reaction can occur, and a layer of polydopamine PDA is polymerized on the surface of the riboflavin and carotenoid mixture:
[0043]
[0044] The speed of self-polymerization is greatly affected by pH and is also affected by time. During the polymerization process, the color of the solution will gradually change over time, from colorless to brown and finally to black.
[0045] Polydopamine PDA has similar light absorption properties to melanin in terms of optical properties. It has a wide-band absorption range from ultraviolet light to visible light, and the light absorption extends all the way to the near-infrared region. It can improve the light-blocking properties of riboflavin and carotenoids and reduce the damage to the effective structure during the molding process.
[0046] (3) 50 g of riboflavin and carotenoid solid mixture (W 核黄素 :W 类胡萝卜素 =1:1) was added to the solution. The solution was heated to 30°C and stirred for 30-45 min. 核黄素 represents the added weight of riboflavin, which is 25 g in this embodiment; W 类胡萝卜素 represents the added weight of carotenoids, which is 25 g in this embodiment;
[0047] Riboflavin (vitamin B2) is a B vitamin derived from isoalloxazine. The molecule is composed of isoalloxazine and ribitol. It has a melting point of 290°C and is a yellow needle-shaped crystal. It tastes bitter and is slightly soluble in water. It is unstable to light, and the absorbance of the photosensitive flavin is ≤0.025. There are three absorption peaks in the ultraviolet-visible light absorption spectrum: 444nm, 375nm, and 267nm. In this embodiment, it is used as a sacrificial protective light-blocking agent to protect the riboflavin in dairy products from being decomposed by external light to the maximum extent.
[0048] Carotenoids are a class of compounds with 040 tetraterpene structures and their derivatives. They are composed of 8 isoprenoid units and are yellow, orange-red or red pigments. Due to the presence of isoprenoid conjugated double bonds in the molecular structure of carotenoids, they have strong light absorption properties and strong absorption within 400-500nm, which can appear red, orange and yellow. They are relatively stable under alkaline conditions.
[0049] (4) The pH value of the reaction solution was adjusted to about 7 with dilute hydrochloric acid, and the solution was filtered with suction. The filter layer was rinsed three times with deionized water and dried in a vacuum dryer at 75° C. for 6 hours to obtain a mixture of riboflavin and carotenoids coated with a polydopamine layer on the surface.
[0050] Example 2
[0051] A method for preparing a light-blocking PETG heat-shrinkable label film, wherein the heat-shrinkable label film is prepared by a flat film method, wherein the heat-shrinkable label film comprises a surface layer A, a core layer and a surface layer B from top to bottom, and the thickness ratio of the surface layer A, the core layer and the surface layer B is 12.5:75:12.5; the preparation method comprises the following steps:
[0052] Step 1, weigh nano-montmorillonite, rutile titanium dioxide, ZnO powder, a mixture of riboflavin and carotenoids coated with a polydopamine layer, antioxidant 1010 and phosphite antioxidant according to the following weight proportions:
[0053] PETG powder 69 parts;
[0054] 8 parts of nano-montmorillonite;
[0055] 5 parts of rutile (R-type) titanium dioxide;
[0056] 5 parts of ZnO powder;
[0057] 10 parts of a mixture of riboflavin and carotenoids coated with a polydopamine layer (the ratio of the two is 1:1);
[0058] 1 part of antioxidant 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate);
[0059] 1 part of triphenyl phosphite.
[0060] The PETG powder was cryogenically ground to a particle size of 125 mesh; the above reagents and the ground PETG powder were added into a high-speed mixer and mixed for 5 minutes to mix evenly;
[0061] The ZnO film made of ZnO powder has a light transmittance of up to 90% in the visible light range, but its transmittance is relatively low in the ultraviolet (UV) and infrared (IR) spectrum ranges, and has a good reflection or protection effect on ultraviolet rays in the 310-370nm wavelength range. Based on this property, this embodiment selects ZnO powder as a barrier layer in the corresponding spectral region;
[0062] Rutile (R-type) titanium dioxide has good weather resistance, water resistance and is not easy to turn yellow; it has strong hiding power and tinting power; nano-montmorillonite is a special organic compound made of montmorillonite clay after exfoliation, dispersion, purification, modification, ultra-fine classification, and average chip thickness is less than 25nm, and the montmorillonite content is greater than 95%. It has good dispersion performance and can be widely used in the polymer material industry as an additive for nano-polymer polymer materials to improve impact resistance, fatigue resistance, dimensional stability and gas barrier properties, thereby playing a reinforcing role and improving material processing performance;
[0063] Step 2: Add the material obtained in step 1 into a twin-screw extruder and granulate at 210°C and 250 rpm to prepare a light-blocking masterbatch; the length-to-diameter ratio of the twin-screw extruder selected is 30:1.
[0064] Step 3, in terms of mass fraction, the extrusion raw materials of the extruders corresponding to the surface layer A and the surface layer B are prepared according to the following chemical components: 98% of PETG raw materials and 2% of open and smooth masterbatch (purchased from Swiss Sukarno Company TA10-08 MB13); the extrusion raw materials of the extruder corresponding to the core layer are prepared according to the following chemical components: 94% of PETG raw materials and 6% of light-blocking masterbatch;
[0065] Step 4, the extrusion raw materials corresponding to the surface layer A and the surface layer B are conveyed to the extruder A for plasticization at 245°C, and the extrusion raw materials corresponding to the core layer are conveyed to the extruder B for plasticization at 245°C; the extrusion raw materials corresponding to the surface layer A and the surface layer B after extrusion and plasticization, and the extrusion raw materials corresponding to the core layer are respectively metered by a metering pump, and then filtered through a filter, and enter the convection flow channel of the distributor before the die through a melt pipe to merge into one, and are cast onto the casting cold roller through a die head with a temperature of 265°C, and the casting is cast by the casting cold roller, and the water inlet temperature of the cooling water of the casting cold roller is 28°C; in the transverse stretching zone (preheating zone 90°C, stretching zone 85°C, shaping zone 70°C and cooling zone 40°C are set), the casting is transversely stretched at a ratio of 1:5.2, and the film being formed is shaped in the rear section of the transverse stretching, the stretched film is pulled, and the pulled film is wound by a winder, and the wound film is inspected and packaged to obtain a light-blocking PETG heat shrinkable label film.
[0066] Example 3
[0067] A method for preparing a light-blocking PETG heat-shrinkable label film, wherein the heat-shrinkable label film is prepared by a flat film method, wherein the heat-shrinkable label film comprises a surface layer A, a core layer and a surface layer B from top to bottom, and the thickness ratio of the surface layer A, the core layer and the surface layer B is 11:78:11; the preparation method comprises the following steps:
[0068] Step 1, weigh nano-montmorillonite, rutile titanium dioxide, ZnO powder, a mixture of riboflavin and carotenoids coated with a polydopamine layer, antioxidant 1010 and phosphite antioxidant according to the following weight proportions:
[0069] PETG powder 69 parts;
[0070] 8 parts of nano-montmorillonite;
[0071] 5 parts of rutile (R-type) titanium dioxide;
[0072] 5 parts of ZnO powder;
[0073] 10 parts of a mixture of riboflavin and carotenoids coated with a polydopamine layer (the ratio of the two is 1:1);
[0074] 1 part of antioxidant 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate);
[0075] 1 part of triphenyl phosphite.
[0076] The PETG powder was cryogenically ground to a particle size of 125 mesh; the above reagents and the ground PETG powder were added into a high-speed mixer and mixed for 5 minutes to mix evenly;
[0077] Step 2: Add the material obtained in step 1 into a twin-screw extruder and granulate at 260° C. and 375 rpm to prepare a light-blocking masterbatch; the length-to-diameter ratio of the twin-screw extruder selected is 30:1.
[0078] Step 3, in terms of mass fraction, the extrusion raw materials of the extruders corresponding to the surface layer A and the surface layer B are prepared according to the following chemical components: 98% of PETG raw materials and 2% of open and smooth masterbatch; the extrusion raw materials of the extruder corresponding to the core layer are prepared according to the following chemical components: 94% of PETG raw materials and 7% of light-blocking masterbatch;
[0079] Step 4, the extrusion raw materials corresponding to the surface layer A and the surface layer B are conveyed to the extruder A for plasticization at 270°C, and the extrusion raw materials corresponding to the core layer are conveyed to the extruder B for plasticization at 270°C; the extrusion raw materials corresponding to the surface layer A and the surface layer B after extrusion and plasticization, and the extrusion raw materials corresponding to the core layer are respectively metered by a metering pump, and then filtered through a filter, and enter the convection flow channel of the distributor before the die head through a melt pipe to merge into one, and are cast onto the casting cold roller through a die head with a temperature of 270°C, and the casting is cast by the casting cold roller, and the water inlet temperature of the cooling water of the casting cold roller is 28°C; in the transverse stretching zone (preheating zone 115°C, stretching zone 95°C, shaping zone 82°C and cooling zone 45°C are set), the casting is transversely stretched at a ratio of 1:5.2, and the film being formed is shaped in the rear section of the transverse stretching, the stretched film is pulled, and the pulled film is wound by a winder, and the wound film is inspected and packaged to obtain a light-blocking PETG heat shrinkable label film.
[0080] Example 4
[0081] A method for preparing a light-blocking PETG heat-shrinkable label film, wherein the heat-shrinkable label film is prepared by a flat film method, wherein the heat-shrinkable label film comprises a surface layer A, a core layer and a surface layer B from top to bottom, and the thickness ratio of the surface layer A, the core layer and the surface layer B is 15:70:15; the preparation method comprises the following steps:
[0082] Step 1, weigh nano-montmorillonite, rutile titanium dioxide, ZnO powder, a mixture of riboflavin and carotenoids coated with a polydopamine layer, antioxidant 1010 and phosphite antioxidant according to the following weight proportions:
[0083] PETG powder 69 parts;
[0084] 8 parts of nano-montmorillonite;
[0085] 5 parts of rutile (R-type) titanium dioxide;
[0086] 5 parts of ZnO powder;
[0087] 10 parts of a mixture of riboflavin and carotenoids coated with a polydopamine layer (the ratio of the two is 1:1);
[0088] 1 part of antioxidant 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate);
[0089] 1 part of trimethyl phosphite.
[0090] The PETG powder was cryogenically ground to a particle size of 125 mesh; the above reagents and the ground PETG powder were added into a high-speed mixer and mixed for 5 minutes to mix evenly;
[0091] Step 2: Add the material obtained in step 1 into a twin-screw extruder and granulate at 240° C. and 300 rpm to prepare a light-blocking masterbatch; the length-to-diameter ratio of the twin-screw extruder selected is 30:1.
[0092] Step 3, in terms of mass fraction, the extrusion raw materials of the extruders corresponding to the surface layer A and the surface layer B are prepared according to the following chemical components: 98% of PETG raw materials and 2% of open and smooth masterbatch; the extrusion raw materials of the extruder corresponding to the core layer are prepared according to the following chemical components: 94% of PETG raw materials and 8% of light-blocking masterbatch;
[0093] Step 4, the extrusion raw materials corresponding to the surface layer A and the surface layer B are conveyed to the extruder A for plasticization at 260°C, and the extrusion raw materials corresponding to the core layer are conveyed to the extruder B for plasticization at 250°C; the extrusion raw materials corresponding to the surface layer A and the surface layer B after extrusion and plasticization, and the extrusion raw materials corresponding to the core layer are respectively metered by a metering pump, and then filtered through a filter, and enter the convection flow channel of the distributor before the die head through a melt pipe to merge into one, and are cast onto the casting cold roller through a die head with a temperature of 268°C, and the casting is cast through the casting cold roller. The water inlet temperature of the cooling water of the casting cold roller is 28°C; in the transverse stretching zone (preheating zone 100°C, stretching zone 90°C, shaping zone 80°C and cooling zone 43°C are set), the casting is transversely stretched at a ratio of 1:5.2, and the film being formed is shaped in the rear section of the transverse stretching, the stretched film is pulled, and the pulled film is wound by a winder, and the wound film is inspected and packaged to obtain a light-blocking PETG heat shrinkable label film.
[0094] In summary, the performance parameters of the light-blocking PETG heat shrinkable label films prepared in Examples 2 to 4 are shown in Table 1 below; wherein the comparative sample is an ordinary transparent PETG heat shrinkable label film.
[0095] Table 1 Performance parameters of light-blocking PETG heat shrinkable label film
[0096]
Claims
1. A method for preparing a mixture of riboflavin and carotenoids coated with a polydopamine layer on the surface, It is characterized in that The following steps are involved: Step 1, weigh a set mass of dopamine hydrochloride into deionized water, and stir until the dopamine hydrochloride is dissolved to prepare an aqueous solution of dopamine hydrochloride; Step 2, adding 10% by mass sodium hydroxide solution to the aqueous solution of dopamine hydrochloride and stirring, and adjusting the pH of the aqueous solution of dopamine hydrochloride to a set value; Step 3, weighing a set amount of riboflavin and carotenoids, adding them to the solution prepared in step 2, heating the solution to a set temperature and stirring for a certain period of time; Step 4, adding a set amount of dilute hydrochloric acid to the reaction solution of step 3, adjusting the pH of the reaction solution to a set value, filtering by suction, rinsing the filter layer with deionized water, and vacuum drying to obtain a riboflavin and carotenoid mixture with a polydopamine layer coated on the surface; The addition ratio of dopamine hydrochloride in step 1 to the total addition ratio of riboflavin and carotenoids in step 3 is 1:5, and the addition ratio of riboflavin and carotenoids is 1:1; Step 2: adjusting the pH value of the dopamine hydrochloride aqueous solution to 8; In step 3, the solution is heated to 30° C. and stirred for 30 to 45 minutes; In step 4, dilute hydrochloric acid is added to adjust the pH of the reaction solution to 7, and the solution is filtered by suction. The filter layer is rinsed with deionized water for 2 to 3 times, and vacuum dried at 75° C. for 4 to 6 hours in a vacuum dryer.
2. A light-blocking masterbatch comprising a mixture of riboflavin and carotenoids coated with a polydopamine layer prepared by the method of claim 1, It is characterized in that In parts by mass, it is composed of the following components: PETG powder 67-77 parts; Nano-montmorillonite 5-10 parts; 3.75-5 parts of rutile titanium dioxide; 3.75-5 parts of ZnO powder; 7.5 to 10 parts of a mixture of riboflavin and carotenoids coated with a polydopamine layer; 2 parts of antioxidant 1010; 1 to 2 parts of phosphite antioxidant.
3. The light-blocking masterbatch according to claim 2, Features: The average chip thickness of nano-montmorillonite is less than 25nm, and the montmorillonite content in nano-montmorillonite is greater than 95%; the density of rutile titanium dioxide is 4.26g / cm 3 , refractive index is 2.72; the purity of titanium dioxide in rutile titanium dioxide is ≥99%; the purity of ZnO in ZnO powder is ≥99%; the phosphite antioxidant is triphenyl phosphite or trimethyl phosphite.
4. A method for preparing a light-blocking PETG heat-shrinkable label film using the light-blocking masterbatch as claimed in claim 2, It is characterized in that A heat shrinkable label film is prepared by a flat film method. The heat shrinkable label film comprises a surface layer A, a core layer and a surface layer B from top to bottom. The thickness ratio of the surface layer A, the core layer and the surface layer B is 10-15:70-80:10-15. The preparation method comprises the following steps: Step 1, grinding the PETG powder at low temperature; weighing nano-montmorillonite, rutile titanium dioxide, ZnO powder, a mixture of riboflavin and carotenoids coated with a polydopamine layer, antioxidant 1010 and phosphite antioxidant according to set weight proportions, adding them together with the ground PETG powder into a high-speed mixer, and mixing them evenly; Step 2, adding the material obtained in step 1 into a twin-screw extruder for granulation to prepare a light-blocking masterbatch; Step 3, in terms of mass fraction, the extrusion raw materials of the extruders corresponding to the surface layer A and the surface layer B are prepared according to the following chemical components: 98% of PETG raw materials and 2% of open and smooth masterbatch; the extrusion raw materials of the extruder corresponding to the core layer are prepared according to the following chemical components: 90-94% of PETG raw materials and 6-10% of light-blocking masterbatch; Step 4, conveying the extrusion raw materials corresponding to the surface layer A and the surface layer B to the extruder A for plasticization, and conveying the extrusion raw materials corresponding to the core layer to the extruder B for plasticization; respectively metering the extrusion raw materials corresponding to the surface layer A and the surface layer B after extrusion plasticization and the extrusion raw materials corresponding to the core layer by a metering pump, and then filtering through a filter, entering the convection flow channel of the distributor before the die through a melt pipe to merge into one, casting through the die head onto the casting cold roller, casting through the casting cold roller, transversely stretching the casting in the transverse stretching zone, shaping the film in the process of forming in the rear section of the transverse stretching, pulling the stretched film, and then winding the pulled film through a winder, inspecting and packaging the wound film to obtain a light-blocking PETG heat shrinkable label film.
5. The method for preparing the light-blocking PETG heat shrinkable label film according to claim 4, Features: The particle size of the PETG powder after cryogenic grinding in step 1 is 125 mesh.
6. The method for preparing the light-blocking PETG heat-shrinkable label film according to claim 4, It is characterized in that In step 4: the plasticizing temperature of extruder A and extruder B is 245-270°C, the temperature of the die head is 265-270°C; the casting cold roller is equipped with cooling water, and the inlet temperature of the casting cold roller cooling water is 28°C.
7. The method for preparing the light-blocking PETG heat shrinkable label film according to claim 4, Features: In step 4, the transverse stretching zone is provided with a preheating zone, a stretching zone, a shaping zone and a cooling zone; the temperature of the preheating zone is 90-115°C, the temperature of the stretching zone is 85-95°C, the temperature of the shaping zone is 70-82°C, and the temperature of the cooling zone is 40-45°C.
8. The method for preparing the light-blocking PETG heat-shrinkable label film according to claim 4, Features: The transverse stretching ratio of the transverse stretching zone in step 4 is 1:5.2.
Citation Information
Cited By
A heat-insulating and water-resistant high-permeability plastic masterbatch, its preparation method and application
CN123062914A