A two-component ceramic tile backing adhesive, its preparation method and application

By using a two-component tile adhesive made of modified nano-silica and modified cement, a cross-linked network structure is formed through emulsion polymerization and hydration reaction, which solves the problem of insufficient bonding strength of tile adhesive in large-size tiles and harsh environments, and achieves excellent early and late bonding effects.

CN117304816BActive Publication Date: 2026-11-10中建材苏州防水研究院有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311250260.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-26
Publication Date
2026-11-10
Estimated Expiration
2043-09-26

AI Technical Summary

Technical Problem

Existing tile adhesives have insufficient bonding strength when bonding large tiles, especially in harsh environments, which can easily lead to problems such as hollowing and detachment.

Method used

The two-component tile adhesive consists of a liquid component containing modified nano-silica and epoxy resin, and a powder component containing modified cement and calcium chloride. Through in-situ emulsion polymerization and hydration reaction, a cross-linked network structure is formed, which improves the bonding strength. The organic modifier improves the retarding effect of gypsum powder, thus synergistically enhancing the early and late bonding strength.

Benefits of technology

It significantly improves the early and late bonding strength of tile backing adhesive, solves the problems of hollowing and falling off of large-sized tiles in harsh environments, and enhances the bonding interface force and sealing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

This invention discloses a two-component tile adhesive, its preparation method, and its application. The adhesive comprises a liquid component and a powder component with a mass ratio of 1:1.2-3.0. The liquid component consists of water, epoxy resin, styrene, acrylic monomer, modified nano-silica, and additives, including initiators and emulsifiers. The modified nano-silica contains double bonds on its surface. The powder component consists of modified cement, calcium chloride, and fillers. The modified cement includes cement clinker and gypsum powder coated with an organic modifier. The organic modifier can react with terminal hydroxyl groups and / or epoxy groups. The liquid and powder components are prepared separately and then mixed before use. This two-component tile adhesive possesses both excellent late-stage and early-stage bonding strength, solving problems such as hollowing and tile detachment when bonding large-size tiles or in harsh environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of tile adhesive technology, specifically to a two-component tile backing adhesive, its preparation method, and its application. Background Technology

[0002] With the rapid development of the ceramic tile industry, a large number of low-absorption, large-size ceramic tiles have emerged in recent years, leading to increasingly higher demands for matching tile adhesive materials. Traditionally, tile installation involves applying on-site mixed cement mortar to walls or floors. This method requires thick application, resulting in material waste and, due to insufficient bonding strength between early tiles and walls, issues such as hollow spots and tile detachment may occur. Therefore, tile adhesive has gradually replaced traditional cement mortar in the market.

[0003] Tile adhesive, as an organic bonding agent, offers better adhesion to polished tiles, vitrified tiles, and other tiles with low water absorption and smooth, dense surfaces compared to traditional cement mortar. However, most tile adhesive products on the market currently have a bonding strength of approximately 0.8-1.0 MPa. When applying large tiles, insufficient early bonding strength can easily lead to tile detachment. Furthermore, after installation, if the adhesive surface is exposed to harsh environments such as moisture or vibration, the slow curing speed and low bonding strength of the early adhesive material can easily damage the bond between the tile and the substrate, causing problems such as hollowing and detachment. Therefore, enhancing the bonding strength of existing tile adhesives and improving their performance in harsh environments is imperative. Summary of the Invention

[0004] The purpose of this invention is to overcome one or more shortcomings in the prior art and provide an improved two-component tile adhesive that can have both excellent late-stage bonding strength and early-stage bonding strength, solving problems such as hollowing between the tile and the substrate and tile detachment when bonding large-sized tiles and in harsh environments.

[0005] This invention also provides a method for preparing the above-mentioned two-component ceramic tile backing adhesive.

[0006] This invention also provides an application of the above-mentioned two-component tile adhesive in tile laying, especially for laying large-size tiles (400mm×800mm or 600mm×600mm, etc.).

[0007] To achieve the above objectives, the present invention provides a technical solution as follows: a two-component ceramic tile backing adhesive, comprising a liquid component and a powder component, wherein the mass ratio of the liquid component to the powder component is 1:1.2-3.0.

[0008] The raw materials of the liquid component include: water, epoxy resin, styrene, acrylic monomer, modified nano silica, and additives. The additives include initiators and emulsifiers, and the surface of the modified nano silica contains double bonds.

[0009] The raw materials of the powder component include: modified cement, calcium chloride, and filler. The modified cement includes cement clinker and gypsum powder coated with an organic modifier. The organic modifier can react with terminal hydroxyl groups and / or epoxy groups.

[0010] According to some preferred aspects of the present invention, the raw materials of the liquid component, by weight, are: 50-150 parts water, 2-15 parts epoxy resin, 5-30 parts styrene, 40-120 parts acrylic monomer, 0.2-5 parts modified nano silica, 0.1-3 parts initiator and 0.1-3 parts emulsifier.

[0011] According to some preferred aspects of the present invention, the raw materials of the powder component, by weight, are: 25-60 parts modified cement, 0.5-5 parts calcium chloride, and 30-70 parts filler.

[0012] Further, by weight, the raw materials of the liquid component are: 70-120 parts water, 4-12 parts epoxy resin, 8-25 parts styrene, 50-100 parts acrylic monomer, 0.5-2 parts modified nano silica, 0.5-1.5 parts initiator and 0.2-1.5 parts emulsifier;

[0013] By weight, the raw materials of the powder component are: 30-50 parts modified cement, 1-4 parts calcium chloride, and 35-65 parts filler.

[0014] According to some preferred and specific aspects of the present invention, the mass ratio of the liquid component to the powder component is 1:1.5-2.0.

[0015] According to some preferred and specific aspects of the present invention, the epoxy resin is a bisphenol A type epoxy resin.

[0016] Furthermore, in some preferred embodiments of the present invention, the bisphenol A type epoxy resin is selected from one or more combinations of compounds shown in formula (I), and has at least 3 active sites in each repeating unit, respectively on two -CH2- and one -CH(OH)-, which can remove hydrogen from carbon to form free radicals and then polymerize with double bonds;

[0017]

[0018] In equation (Ⅰ), R1 is C 1-6 Alkylene or -S(O)2-, n is an integer selected from 1 to 50;

[0019] Further, R1 is methylene, ethylene, -CH2-CH2-CH2-, -CH(CH3)-CH2-, -CH(CH3)-, -C(CH3)2-, -CH(CH3)-CH2-CH2- or -S(O)2-, and n is selected from 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10.

[0020] According to some preferred and specific aspects of the present invention, the acrylic monomers include butyl acrylate, methacrylic acid and hydroxyethyl acrylate, wherein the mass ratio of butyl acrylate, methacrylic acid and hydroxyethyl acrylate is 20-80:0.3-3:1.

[0021] According to some preferred and specific aspects of the present invention, the method for preparing the modified nano silica includes: dispersing nano silica and the silane coupling agent shown in formula (II) in an organic solvent, mixing them, reacting them under heating conditions, and separating the modified nano silica after the reaction is completed;

[0022] in, In equation (II), R2, R3, and R4 are each independently selected from C. 1-6 Alkyl, C 1-6 Alkyl group, and R2, R3, R4 have at least one selected from C 1-6 Alkoxy group, R5 is an organic group containing a double bond;

[0023] The mass ratio of the nano-silica to the silane coupling agent shown in formula (II) is 1:0.1-0.125.

[0024] In some embodiments of the present invention, R5 is CH2=C(CH3)COOCH2CH2CH2-, CH2=C(CH3)CH2-, CH2=CH-, etc., C 1-6 Alkyl groups can be methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, etc., C 1-6 Alkoxy groups can be methoxy, ethoxy, propoxy, etc.

[0025] In some embodiments of the present invention, the silane coupling agent represented by formula (II) can be vinyltriethoxysilane, methacryloxypropyltrimethoxysilane, etc.

[0026] In some embodiments of the present invention, the initiator is one or more combinations selected from sodium persulfate, potassium persulfate, and benzoyl peroxide.

[0027] In some embodiments of the present invention, the emulsifier is composed of a nonionic emulsifier and an anionic emulsifier, wherein the mass ratio of the nonionic emulsifier to the anionic emulsifier is 1:0.5-2. Further, the anionic emulsifier includes sodium dodecylbenzenesulfonate, and the nonionic emulsifier includes alkylphenol polyoxyethylene ether.

[0028] According to one specific aspect of the present invention, the mass ratio of the nonionic emulsifier to the anionic emulsifier is 1:0.8-1.2, for example, it can be 1:1.

[0029] In some embodiments of the present invention, the raw materials of the liquid component further include dispersants, preservatives, and defoamers. The preservatives include isothiazolinone preservatives, the defoamers include polysiloxane defoamers, and the dispersants include nonionic dispersants.

[0030] In some embodiments of the present invention, the organic modifier is maleic anhydride, which has a variety of polar or non-polar groups, including polar aldehyde groups and olefinic non-polar segments. This not only enables chemical bonding between the polymer and the powder, but also ensures good compatibility between the powder component and the liquid component.

[0031] In some embodiments of the present invention, the method for preparing the gypsum powder with the surface coated with the organic modifier includes: dispersing the organic modifier in anhydrous ethanol, then mixing and dispersing it with gypsum powder, and evaporating the anhydrous ethanol during stirring to obtain the gypsum powder with the surface coated with the organic modifier; wherein the mass ratio of the organic modifier to the gypsum powder is 0.3-0.8:1, and more preferably 0.4-0.7:1.

[0032] In some embodiments of the present invention, the filler includes sand and heavy calcium carbonate, wherein the mass ratio of sand to heavy calcium carbonate is 1:0.3-0.5, and further, the heavy calcium carbonate is 100-350 mesh heavy calcium carbonate.

[0033] In some embodiments of the present invention, the raw materials of the powder component further include 0.1-1 parts by weight of a thickener; further, the thickener includes starch ether, and the thickener is 0.2-0.5 parts.

[0034] In some embodiments of the present invention, the raw materials of the liquid component, by weight, are: 70-100 parts water, 5-10 parts epoxy resin, 10-25 parts styrene, 60-80 parts butyl acrylate, 1-3 parts methacrylic acid, 1-3 parts hydroxyethyl acrylate, 0.5-1.5 parts modified nano silica, 0.5-1.0 parts initiator, and 0.2-1.0 parts emulsifier;

[0035] By weight, the raw materials of the powder components are: 35-40 parts modified cement, 2-3 parts calcium chloride, 30-40 parts sand, and 12-15 parts heavy calcium carbonate.

[0036] In some embodiments of the present invention, the preparation of the modified cement includes:

[0037] S1: Mix 80-90 parts limestone, 10-15 parts clay raw materials, and 1-2 parts iron ore powder evenly and then grind them to obtain a powdery mixture with a thickness of 0.05-0.35mm.

[0038] S2: The powdered mixture after crushing and grinding is conveyed to the preheater and preheated at a temperature of 450-900℃ for 30-60 minutes;

[0039] S3: Next, the preheated mixture is sent into the decomposition furnace and decomposed at a temperature of 800-900℃ for 40-60 minutes to complete the decomposition of most of the mixture;

[0040] S4: The decomposed mixture is transported into a calcining furnace and calcined at a high temperature of 1200-1500℃ for 1-2 hours to finally obtain cement clinker;

[0041] S5: Finally, the cement clinker is sent to a cooling device for cooling and temperature reduction. Then, 3-5 parts of gypsum powder with surface-coated organic modifier and 0.1-0.3% of grinding aid (such as triethanolamine, triisopropanolamine, etc.) are added. The mixture is stirred evenly and then ground in a cement mill to obtain modified cement.

[0042] Another technical solution provided by this invention is a method for preparing the above-mentioned two-component ceramic tile back adhesive, the preparation method comprising:

[0043] (1) Preparation of liquid components

[0044] The emulsifier is dispersed in water and mixed to obtain an aqueous emulsifier solution;

[0045] Styrene, acrylic monomer, part of the initiator and epoxy resin are mixed to obtain a mixture;

[0046] Modified nano-silica was added to the emulsifier aqueous solution, mixed and dispersed, and then the mixture was added dropwise after the temperature was raised to the preset reaction temperature. After the dropwise addition was completed, the reaction was kept at the temperature and the remaining initiator was added during the reaction. After the reaction was completed, the remaining raw materials were added to obtain the liquid component.

[0047] (2) Preparation of powder components

[0048] The raw materials of the powder component are mixed evenly to obtain the powder component.

[0049] In some preferred embodiments of the present invention, the mixing is controlled to be carried out at 35-45°C during the preparation of the emulsifier aqueous solution.

[0050] In some preferred embodiments of the present invention, during the preparation of the mixture, the epoxy resin is added after being diluted with an alcohol solvent, including n-propanol. The use of alcohol solvents is beneficial for dispersion and will evaporate in subsequent processes, so they will basically not remain in the final product.

[0051] In some preferred embodiments of the present invention, during the preparation of the mixture, the initiator accounts for 70%-90% of the total initiator by mass percentage.

[0052] In some preferred embodiments of the present invention, during the preparation of the liquid components, the preset reaction temperature is controlled at 70-90°C, and the dropping time of the mixture is controlled at 2-6 hours.

[0053] In some preferred embodiments of the present invention, the time for the heat preservation reaction is controlled to be 0.5-2 hours during the preparation of the liquid component.

[0054] In some preferred embodiments of the present invention, the heat preservation reaction is controlled to be carried out under stirring conditions during the preparation of the liquid component.

[0055] According to certain aspects of the present invention, embodiments for preparing liquid components include:

[0056] (1) Add the emulsifier to deionized water and stir it in a water bath at 35-45℃ using a mechanical stirrer at a speed of 150-300r / min (for example, for 6-10min) to prepare an emulsifier aqueous solution (soap solution) for later use.

[0057] (2) Styrene, butyl acrylate, methacrylic acid, hydroxyethyl acrylate, 70%-90% of the initiator used in the formulation, and epoxy resin diluted with n-propanol are shaken and mixed evenly, and then set aside.

[0058] (3) Add dispersant and modified nano silica to the emulsifier aqueous solution, disperse by ultrasonication, transfer to a container, stir and heat, slowly add the mixture obtained in step (2) to the emulsifier aqueous solution for 3-4 hours, keep warm for 0.5-2 hours after the addition is completed, increase the speed to 2000-3000 r / min and stir for 30-60 minutes, add the remaining initiator during the process, stop heating, and obtain a composite polymer emulsion system of nano-modified acrylic emulsion, nano-modified waterborne epoxy resin emulsion and epoxy acrylic emulsion;

[0059] (4) When the temperature drops to room temperature, add preservative and defoamer, and stir at a speed of 200-300 r / min for 10-20 min to obtain the liquid component.

[0060] Another technical solution provided by the present invention is the application of the above-mentioned two-component tile adhesive in tile laying.

[0061] Due to the application of the above-mentioned technical solution, the present invention has the following advantages compared with the prior art:

[0062] Addressing the shortcomings in the bonding strength of existing tile adhesives, this invention provides an improved two-component tile adhesive. In the liquid component, modified nano-silica with double bonds on its surface is used as a modification method. Under the action of an initiator, it can be prepared via in-situ emulsion polymerization to produce nano-modified acrylic emulsion and nano-modified waterborne epoxy resin emulsion. Simultaneously, the methylene or methine groups in the epoxy resin molecules become active sites, participating in the polymerization of acrylic monomers and modified nano-silica with double bonds on their surface, generating various mixed emulsion systems such as epoxy resin-modified acrylic emulsions. This results in better and more stable dispersion of nano-silica in the system. The surface of silica is rich in highly active Si-O bonds and Si-OH groups. The Si-O bonds promote the uniform dispersion of silica nanoparticles in the tile adhesive system, while the Si-OH groups enable strong intermolecular forces between the nano-silica and the polar groups of the polymer. This allows the gel material formed after the powder and liquid are mixed to further form a cross-linked network structure, inhibiting the flow of the gel, increasing the curing rate, and enhancing the bonding interface force. Consequently, this improves the bonding strength between the tile adhesive system and the substrate and the tile, while also increasing the sealing performance of the tile adhesive. In addition, the introduction of epoxy resin into the tile adhesive can effectively improve the adhesion between the cementitious material and the substrate.

[0063] Furthermore, this invention adds an appropriate amount of calcium chloride to the powder component. After mixing with the liquid component, the calcium chloride can dissociate into positive and negative ions, resulting in a strong hydration and water competition effect. This reduces the number of free water molecules in the mixture and dehydrates the organic oil droplets. The water-oil imbalance leads to demulsification, which accelerates the evaporation of excess water. Using this principle, the inventors found that it can improve the early curing speed of tile back adhesive, which helps to solve the problems of hollowing and falling off caused by insufficient bonding strength, especially early bonding strength, when tile back adhesive is applied to the construction of large-size wall tiles.

[0064] Furthermore, this invention addresses the coating modification of gypsum powder in cement by introducing an organic modifier onto the surface of the gypsum powder that can react with terminal hydroxyl and / or epoxy groups. Specifically, this organic modifier can react with the terminal hydroxyl or epoxy groups contained in the resin of the liquid component, or with the terminal hydroxyl groups contained in nano-silica. When the liquid component and powder component are mixed, cement hydration occurs. Since gypsum powder itself acts as a retarder in cement, its retarding effect is difficult to take effect immediately due to its initial coated state. This allows the hydration process to proceed rapidly in the early stages, thereby increasing early bond strength. As the hydration reaction progresses... The heat generated during the continuous process can promote the reaction between the epoxy groups on the epoxy resin or the silanol groups on the nano silica and the organic modifier. On the one hand, it can promote the formation of a three-dimensional network structure in the system. Combined with the introduction of polar groups such as hydroxyl groups, it can further improve the bonding strength between the tile backing adhesive and the substrate and the back of the tile. On the other hand, once the reaction occurs, it is equivalent to slowly reacting away the organic modifier coated on the surface of the gypsum powder. Especially during the cement hydration process, the resin will continuously penetrate and fill the pores. When the gypsum powder is released from the coated state, it will immediately play a retarding role and can also avoid the negative impact that may be caused by the hydration reaction occurring too quickly in a limited time.

[0065] Ultimately, through synergistic improvements to the liquid and powder components, the resulting tile adhesive possesses both excellent late-stage and early-stage bonding strength, solving problems such as hollowing and tile detachment when using common tile adhesives for bonding large-sized tiles or in harsh environments. Detailed Implementation

[0066] The above-mentioned solution will be further described below with reference to specific embodiments; it should be understood that these embodiments are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following embodiments; the implementation conditions used in the embodiments can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in conventional experiments.

[0067] The examples involve the addition of various substances, and unless otherwise specified, "parts" refers to "parts by weight". Unless otherwise specified, all raw materials can be commercially available or prepared using conventional methods in the art.

[0068] The modified nano-silica described below is prepared by the following method:

[0069] Weigh 5g of nano-silica (particle size 15±5nm) and 0.625g of silane coupling agent KH-570 (purchased from Shanghai Koraman Reagent Co., Ltd.) and disperse them together in 150mL of xylene. After ultrasonic dispersion for 10min, heat to reflux. After reacting for a period of time, stop the reaction and cool. Centrifuge at 13000r / min. After precipitation, wash several times with anhydrous ethanol and dry to obtain modified nano-silica.

[0070] The modified cement described below is prepared by the following method:

[0071] S1: Mix 85 parts limestone, 12 parts clay raw materials, and 1 part iron ore powder evenly and then grind them to obtain a powdery mixture with a particle size of 0.05-0.35mm.

[0072] S2: The powdered mixture after crushing and grinding is conveyed to the preheater and preheated at 700℃ for 30 minutes;

[0073] S3: Next, the preheated mixture is sent into the decomposition furnace and decomposed at 900℃ for 40 minutes to complete the decomposition of most of the mixture;

[0074] S4: The decomposed mixture is fed into a calcining furnace and calcined at 1100℃ for 1.5 hours to finally obtain cement clinker;

[0075] S5: Finally, the cement clinker is sent to a cooling device for cooling and temperature reduction. Then, 4 parts of gypsum powder with surface-coated organic modifier and 0.2% of triethanolamine in the cement clinker are added, mixed and stirred evenly, and then ground in a cement mill to obtain modified cement.

[0076] The gypsum powder with surface-coated organic modifier was prepared as follows: 60 parts by weight of gypsum powder and 36 parts by weight of maleic anhydride were weighed, the maleic anhydride was dissolved in anhydrous ethanol to prepare a solution, the gypsum powder was added, and the mixture was thoroughly mixed to form a mixture. The mixture was placed in the mixing chamber of a dispersion mixer, covered, and thoroughly stirred. During the stirring process, the anhydrous ethanol vaporized and condensed at the cover, separating it from the sample. The sample was dried and stored to obtain the gypsum powder with surface-coated organic modifier.

[0077] Example 1

[0078] This example provides a method for preparing a two-component tile backing adhesive and the resulting two-component tile backing adhesive. The method for preparing the two-component tile backing adhesive includes:

[0079] 1. Preparation of liquid components

[0080] (1) Add 0.3 parts of sodium dodecylbenzenesulfonate (Adamas, product number 25701l) and 0.3 parts of emulsifier OP-10 (Aladdin, product number 0304931) to 70 parts of deionized water, and stir for 8 minutes at 200 r / min using a mechanical stirrer under 40℃ water bath conditions to prepare an emulsifier aqueous solution (soap solution) for later use;

[0081] (2) Mix 20 parts styrene (Adamas, product number 10289B), 70 parts butyl acrylate (Greagent, product number G23168A), 2 parts methacrylic acid (Adamas, 83760C), 2 parts hydroxyethyl acrylate (Adamas, 87221K), 0.4 parts ammonium persulfate (Shandong Jinyueyuan New Material Co., Ltd., product number 51101) and 5 parts epoxy resin E-44 (purchased from Shanghai Resin Factory Co., Ltd.) diluted with 1 part n-propanol (Merck, product number PHR1208) by shaking until homogeneous, and then transfer the mixture to a constant temperature funnel for later use.

[0082] (3) Add 0.01 parts of dispersant (TEGO, product number Dispers 760W) and 0.5 parts of modified nano silica to the soap solution. After ultrasonic dispersion for 10 min, transfer to a three-necked flask, stir and heat to 80°C. Connect the constant pressure funnel to the three-necked flask and slowly add it dropwise to the soap solution for 3.5 h. After the dropwise addition is completed, keep warm for 1 h, increase the speed to 3000 r / min and stir for 60 min. During this period, add the remaining 0.1 parts of ammonium persulfate and stop heating to obtain the composite polymer emulsion system.

[0083] (4) When the temperature drops to room temperature, add 0.3 parts of isothiazolinone preservative (Zaozhuang Shibang Biotechnology Co., Ltd., product number TB10) and 0.1 parts of polysiloxane defoamer (Shanghai Boran New Material Technology Co., Ltd., product number 1234), and stir at 200 r / min for 20 min to obtain the liquid composition.

[0084] 2. Preparation of powder components

[0085] Weigh out 35 parts sand, 36 parts modified cement, 12 parts heavy calcium carbonate (200 mesh), 2 parts calcium chloride and 0.2 parts starch ether (purchased from McKem Chemical, brand name Avebe S301) according to the weight ratio, pour them into a mixer and mix thoroughly until uniform to obtain the powder composition.

[0086] 3. When needed, mix the liquid component and the powder component at a weight ratio of 1:1.5 to obtain a two-component tile adhesive, which can be used for tiling.

[0087] Example 2

[0088] This example provides a method for preparing a two-component tile backing adhesive and the resulting two-component tile backing adhesive. The method for preparing the two-component tile backing adhesive includes:

[0089] 1. Preparation of liquid components

[0090] (1) Add 0.25 parts of sodium dodecylbenzenesulfonate (Adamas, product number 25701l) and 0.25 parts of emulsifier OP-10 (Aladdin, product number 0304931) to 80 parts of deionized water, and stir for 8 minutes at 200 r / min using a mechanical stirrer under 40℃ water bath conditions to prepare an emulsifier aqueous solution (soap solution) for later use.

[0091] (2) Mix 15 parts of styrene (Adamas, product number 10289B), 75 parts of butyl acrylate (Greagent, product number G23168A), 2 parts of methacrylic acid (Adamas, 83760C), 2 parts of hydroxyethyl acrylate (Adamas, 87221K), 0.48 parts of ammonium persulfate (Shandong Jinyueyuan New Material Co., Ltd., product number 51101) and 6 parts of epoxy resin E-44 (purchased from Shanghai Resin Factory Co., Ltd.) diluted with 1.2 parts of n-propanol (Merck, product number PHR1208) by shaking until homogeneous, and then transfer the mixture to a constant temperature funnel for later use.

[0092] (3) Add 0.01 parts of dispersant (TEGO, product number Dispers 760W) and 0.6 parts of modified nano silica to the soap solution. After ultrasonic dispersion for 10 min, transfer to a three-necked flask, stir and heat to 80°C. Connect the constant pressure funnel to the three-necked flask and slowly add it dropwise to the soap solution. The dropwise addition time is 3.5 h. After the dropwise addition is completed, keep warm for 1 h, increase the speed to 3000 r / min and stir for 60 min. During this period, add the remaining 0.12 parts of ammonium persulfate and stop heating to obtain the composite polymer emulsion system.

[0093] (4) When the temperature drops to room temperature, add 0.3 parts of isothiazolinone preservative (Zaozhuang Shibang Biotechnology Co., Ltd., product number TB10) and 0.1 parts of polysiloxane defoamer (Shanghai Boran New Material Technology Co., Ltd., product number 1234), and stir at 200 r / min for 20 min to obtain the liquid composition.

[0094] 2. Preparation of powder components

[0095] Weigh out 36 parts sand, 35 parts modified cement, 13 parts heavy calcium carbonate (200 mesh), 2 parts calcium chloride, and 0.2 parts starch ether (purchased from McKem Chemical, brand name Avebe S301) according to the weight ratio, pour them into a mixer and mix thoroughly until uniform to obtain the powder composition.

[0096] 3. When needed, mix the liquid component and the powder component at a weight ratio of 1:1.8 to obtain a two-component tile adhesive, which can be used for tiling.

[0097] Example 3

[0098] This example provides a flame-retardant liquid composition suitable for waterproof mortar, the preparation method of which includes:

[0099] (1) Add 0.3 parts of sodium dodecylbenzenesulfonate (Adamas, product number 25701l) and 0.3 parts of emulsifier OP-10 (Aladdin, product number 0304931) to 90 parts of deionized water, and stir for 8 minutes at 200 r / min using a mechanical stirrer under 40℃ water bath conditions to prepare an emulsifier aqueous solution (soap solution) for later use;

[0100] (2) Mix 25 parts of styrene (Adamas, product number 10289B), 80 parts of butyl acrylate (Greagent, product number G23168A), 3 parts of methacrylic acid (Adamas, 83760C), 3 parts of hydroxyethyl acrylate (Adamas, 87221K), 0.64 parts of ammonium persulfate (Shandong Jinyueyuan New Material Co., Ltd., product number 51101) and 7 parts of epoxy resin E-44 (purchased from Shanghai Resin Factory Co., Ltd.) diluted with 1.4 parts of n-propanol (Merck, product number PHR1208) by shaking until homogeneous, and then transfer the mixture to a constant temperature funnel for later use.

[0101] (3) Add 0.01 parts of dispersant (TEGO, product number Dispers 760W) and 0.8 parts of modified nano silica to the soap solution. After ultrasonic dispersion for 10 min, transfer to a three-necked flask, stir and heat to 80°C. Connect the constant pressure funnel to the three-necked flask and slowly add it dropwise to the soap solution. The dropwise addition time is 3.5 h. After the dropwise addition is completed, keep warm for 1 h, increase the speed to 3000 r / min and stir for 60 min. During this period, add the remaining 0.16 parts of ammonium persulfate and stop heating to obtain the composite polymer emulsion system.

[0102] (4) When the temperature drops to room temperature, add 0.4 parts of isothiazolinone preservative (Zaozhuang Shibang Biotechnology Co., Ltd., product number TB10) and 0.15 parts of polysiloxane defoamer (Shanghai Boran New Material Technology Co., Ltd., product number 1234), and stir at 200 r / min for 20 min to obtain the liquid composition.

[0103] 2. Preparation of powder components

[0104] Weigh out 40 parts sand, 36 parts modified cement, 12 parts heavy calcium carbonate (200 mesh), 2 parts calcium chloride, and 0.3 parts starch ether (purchased from McKem Chemical, brand name Avebe S301) according to the weight ratio, pour them into a mixer and mix thoroughly until uniform to obtain the powder composition.

[0105] 3. When needed, mix the liquid component and the powder component in a weight ratio of 1:2 to obtain a two-component tile adhesive, which can be used for tiling.

[0106] Comparative Example 1

[0107] The process is basically the same as in Example 1, except that the liquid component uses commercially available acrylic emulsion (purchased from Shanghai Baolijia New Materials Co., Ltd., brand name BLJ-6100D) and the same amount of preservative and defoamer are added.

[0108] Comparative Example 2

[0109] The basic structure is the same as in Example 1, except that no modified nano-silica is added to the liquid component.

[0110] Comparative Example 3

[0111] The basic structure is the same as in Example 1, except that calcium chloride is not added to the powder components.

[0112] Comparative Example 4

[0113] The basic structure is the same as in Example 1, except that ordinary 42.5 silicate cement is used instead of modified cement in the powder component. Otherwise, they are the same.

[0114] Performance testing

[0115] Multiple conventional bond strength and early bond strength tests were conducted on the two-component tile adhesives prepared in Examples 1-3 and Comparative Examples 1-4.

[0116] All routine bond strength tests were conducted according to standard JC / T 547-2017 "Ceramic Tile Adhesives". Early bond strength was determined by shortening the curing period to 5 days.

[0117] The test results are shown in Table 1.

[0118] Table 1

[0119]

[0120]

[0121] The results show that the two-component tile backing adhesive disclosed in this embodiment has excellent early and late bonding strength.

[0122] The test results of Example 1 and Comparative Example 1 show that the liquid component prepared by the modified nano-silica and water-based epoxy resin composite modification of the present invention can significantly improve the bonding strength of the tile back adhesive. Compared with Comparative Example 1, Example 1 showed a 26.1% increase in tensile bonding strength, a 26.3% increase in tensile bonding strength after immersion in water, a 26.4% increase in tensile bonding strength after heat treatment, a 26.1% increase in tensile bonding strength after freeze-thaw cycles, and a 25.8% increase in early bonding strength.

[0123] Comparing the test results of Comparative Example 2 with those of Example 1, it can be seen that the incorporation of modified nano-silica can effectively improve the bonding strength of the tile back adhesive. Compared with Comparative Example 2, Example 1 showed a 17.8% increase in tensile bond strength and a 10.7% increase in early bond strength.

[0124] Comparing the test results of Comparative Example 3 with those of Example 1, it can be seen that an appropriate amount of calcium chloride in the powder component can significantly improve the early bonding strength of the tile back adhesive, indicating that the incorporation of calcium chloride can accelerate the early curing speed of the tile back adhesive, thereby improving the early bonding strength. Compared with Comparative Example 3, Example 1 improved by 104.9%.

[0125] Comparing the test results of Comparative Example 4 with those of Example 1, it can be seen that the modified cement component can effectively improve the bonding strength of the tile back adhesive, especially the early bonding strength (16.9% higher than that of Comparative Example 4 in Example 1) and the bonding strength after freeze-thaw cycles (11.2% higher than that of Comparative Example 4 in Example 1). This indicates that the modified cement component, when mixed with the liquid component, has good stability and adhesion, and can further enhance the ability of the tile back adhesive to resist climate damage.

[0126] The above embodiments are only for illustrating the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.

[0127] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

Claims

1. A two-component ceramic tile backing adhesive, comprising a liquid component and a powder component, characterized in that, The mass ratio of the liquid component to the powder component is 1:1.2-3.0; The raw materials of the liquid component include: water, epoxy resin, styrene, acrylic monomer, modified nano-silica, and additives. The additives include an initiator and an emulsifier. The modified nano-silica has double bonds on its surface. By weight, the raw materials of the liquid component are: 50-150 parts water, 2-15 parts epoxy resin, 5-30 parts styrene, 40-120 parts acrylic monomer, 0.2-5 parts modified nano-silica, 0.1-3 parts initiator, and 0.1-3 parts emulsifier. The acrylic monomers include butyl acrylate, methacrylic acid, and hydroxyethyl acrylate; The epoxy resin is a bisphenol A type epoxy resin, and the bisphenol A type epoxy resin is selected from one or more combinations of the compounds shown in formula (I); In equation (Ⅰ), R1 is C 1-6 Alkylene or -S(O)2-, n is an integer selected from 1 to 50; The raw materials of the powder component include: modified cement, calcium chloride, and filler. The modified cement includes cement clinker and gypsum powder coated with an organic modifier. The organic modifier can react with terminal hydroxyl groups and / or epoxy groups, and the organic modifier is maleic anhydride. The mass ratio of the organic modifier to the gypsum powder is 0.3-0.8:

1. By weight, the raw materials of the powder component include: 25-60 parts of modified cement, 0.5-5 parts of calcium chloride, and 30-70 parts of filler.

2. The two-component ceramic tile adhesive according to claim 1, characterized in that, By weight, the raw materials of the liquid component are: 80-120 parts water, 4-12 parts epoxy resin, 8-25 parts styrene, 50-100 parts acrylic monomer, 0.5-2 parts modified nano silica, 0.5-1.5 parts initiator and 0.2-1.5 parts emulsifier; By weight, the raw materials of the powder component are: 30-50 parts modified cement, 1-4 parts calcium chloride, and 35-65 parts filler.

3. The two-component ceramic tile backing adhesive according to claim 1 or 2, characterized in that, The mass ratio of the liquid component to the powder component is 1:1.5-2.

0.

4. The two-component ceramic tile adhesive according to claim 1, characterized in that, In formula (Ⅰ), R1 is methylene, ethylene, -CH2-CH2-CH2-, -CH(CH3)-CH2-, -CH(CH3)-, -C(CH3)2-, -CH(CH3)-CH2-CH2- or -S(O)2-, and n is selected from 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10.

5. The two-component ceramic tile adhesive according to claim 1, characterized in that, The mass ratio of butyl acrylate, methacrylic acid and hydroxyethyl acrylate is 20-80:0.3-3:

1.

6. The two-component ceramic tile adhesive according to claim 1, characterized in that, The method for preparing the modified nano silica includes: dispersing nano silica and the silane coupling agent shown in formula (II) in an organic solvent, mixing them, reacting them under heating conditions, and separating the modified nano silica after the reaction is completed; in, In equation (II), R2, R3, and R4 are each independently selected from C. 1-6 Alkyl, C 1-6 Alkyl groups, and at least one of R2, R3, and R4 is selected from C. 1-6 Alkoxy group, R5 is an organic group containing a double bond; The mass ratio of the nano-silica to the silane coupling agent shown in formula (II) is 1:0.1-0.

125.

7. The two-component ceramic tile adhesive according to claim 1, characterized in that, The initiator is selected from one or more combinations of sodium persulfate, potassium persulfate, and benzoyl peroxide; and / or, the raw materials of the liquid component also include dispersants, preservatives, and defoamers, wherein the preservatives include isothiazolinone preservatives, the defoamers include polysiloxane defoamers, and the dispersants include nonionic dispersants.

8. The two-component ceramic tile adhesive according to claim 1, characterized in that, The emulsifier is composed of a nonionic emulsifier and anionic emulsifier, and the mass ratio of the nonionic emulsifier to the anionic emulsifier is 1:0.5-2.

9. The two-component ceramic tile adhesive according to claim 8, characterized in that, The anionic emulsifier includes sodium dodecylbenzenesulfonate, and the nonionic emulsifier includes alkylphenol polyoxyethylene ether.

10. The two-component ceramic tile adhesive according to claim 1, characterized in that, The preparation method of the gypsum powder with surface-coated organic modifier includes: dispersing the organic modifier in anhydrous ethanol, then mixing and dispersing it with gypsum powder, and evaporating the anhydrous ethanol during stirring to obtain the gypsum powder with surface-coated organic modifier; wherein the mass ratio of the organic modifier to the gypsum powder is 0.4-0.7:

1.

11. The two-component ceramic tile adhesive according to claim 1, characterized in that, The filler includes sand and heavy calcium carbonate, and the mass ratio of sand to heavy calcium carbonate is 1:0.3-0.

5.

12. The two-component ceramic tile adhesive according to claim 11, characterized in that, The heavy calcium carbonate is 100-350 mesh heavy calcium carbonate.

13. The two-component ceramic tile adhesive according to claim 1, characterized in that, The raw materials of the powder component also include 0.1-1 parts by weight of thickener.

14. The two-component ceramic tile adhesive according to claim 13, characterized in that, The thickener includes starch ether, and the thickener is present in quantities of 0.2-0.5 parts.

15. A method for preparing a two-component ceramic tile backing adhesive according to any one of claims 1-14, characterized in that, The preparation method includes: (1) Preparation of liquid components The emulsifier is dispersed in water and mixed to obtain an aqueous emulsifier solution; Styrene, acrylic monomer, part of the initiator and epoxy resin are mixed to obtain a mixture; Modified nano-silica was added to the emulsifier aqueous solution, mixed and dispersed, and then the mixture was added dropwise after the temperature was raised to the preset reaction temperature. After the dropwise addition was completed, the reaction was kept at the temperature and the remaining initiator was added during the reaction. After the reaction was completed, the remaining raw materials were added to obtain the liquid component. (2) Preparation of powder components The raw materials of the powder component are mixed evenly to obtain the powder component.

16. The method for preparing a two-component ceramic tile backing adhesive according to claim 15, characterized in that, In the preparation of the emulsifier aqueous solution, the mixing is controlled to be carried out at 35-45°C; and / or, in the preparation of the mixture, the epoxy resin is added after being diluted with an alcohol solvent, the alcohol solvent including n-propanol; and / or, in the preparation of the mixture, the initiator accounts for 70%-90% of the total initiator by mass percentage; and / or, in the preparation of the liquid component, the preset reaction temperature is controlled to be 70-90°C, and the dropping time of the mixture is controlled to be 2-6 hours; and / or, in the preparation of the liquid component, the heat preservation reaction time is controlled to be 0.5-2 hours; and / or, in the preparation of the liquid component, the heat preservation reaction is controlled to be carried out under stirring conditions.

17. The application of a two-component tile adhesive according to any one of claims 1-14 in tile laying.

Citation Information

Patent Citations

  • Single-component ceramic tile back coating adhesive composition and application thereof

    CN114163881A

  • Water-resistant single-component ceramic tile back adhesive and preparation method thereof

    CN114806469A