A novel lanthanum gallium silicate crystal and its electro-optic coefficient optimization method and application

By introducing Zr4+ and Ga3+ ions into the octahedral group of the gallium silicate group crystal, the electronic cloud structure and lattice vibration are regulated, the electro-optical coefficient is optimized, and the gallium silicate group crystal is solved in the high refrigeration mid-infrared pulse laser The problem of high driving voltage in the output reduces costs and expands the scope of application.

CN117305982BActive Publication Date: 2024-11-22SHANDONG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311305311.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-10
Publication Date
2024-11-22
Estimated Expiration
2043-10-10

AI Technical Summary

Technical Problem

The gallium silicate crystal has a high driving voltage in the output of high frequency mid-infrared pulse laser, resulting in high driving power supply costs and strict requirements on safety and circuit design during use, limiting its application range.

Method used

By introducing Zr4+ and Ga3+ ions into the octahedral group of the gallium silicate group crystal for mixing, the electron cloud structure and lattice vibration of the crystal are regulated, the response to the external field is enhanced, and the degree of change in refractive index and dielectric constant is optimized. This reduces the electro-optical switch driving voltage.

Benefits of technology

The optimization of electro-optical coefficient is achieved, which reduces the driving voltage and reduces the cost, while retaining other excellent performances of the crystal, such as laser damage threshold, expanding its application potential in mid-infrared high-frequency pulsed laser output.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117305982B_ABST
    Figure CN117305982B_ABST
Patent Text Reader

Abstract

The present invention discloses a novel lanthanum gallium silicate crystal and an electro-optic coefficient optimization method and application thereof. The optimization method is as follows: the general structure formula of the lanthanum gallium silicate crystal is A3BC3D2O 14 , by La3Ga5SiO 14 Zr is introduced into the BO6 polyhedral group of the crystal 4+ ions and their Ga 3+ The ions are mixed and the group electronic cloud structure and lattice vibration are regulated to grow lanthanum gallium zirconium silicate La3Zr x Ga5Si 1‑ x O 14 (0<x<1) crystal, to achieve optimization of electro-optic coefficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electro-optical crystals and laser technology, and more specifically to a method for growing a novel lanthanum gallium silicate crystal and optimizing its electro-optical coefficient. Background Art

[0002] High repetition rate mid-infrared pulse lasers have important applications in military fields such as infrared active jamming, laser radar, laser ranging, and civilian fields such as laser communications, remote sensing satellites, and laser precision processing. Currently, electro-optical Q-switching is a practical technical means to obtain such lasers. The refractive index of electro-optical crystals can change with the applied electric field, that is, they have an electro-optic effect, and are an indispensable key material in electro-optical Q-switched pulse lasers. Ideal electro-optical crystals must not only have a more obvious electro-optical effect, but also have high requirements in terms of light transmission range, laser damage threshold, large-size growth characteristics, physical and chemical property stability, temperature characteristics, hardness characteristics, etc.

[0003] The existing practical electro-optic crystals mainly include potassium dideuterium phosphate (DKDP), lithium niobate (LN), rubidium titanyl phosphate (RTP), barium metaborate (BBO) and lanthanum gallium silicate (LGS), etc., which have been widely used in various types of pulsed laser systems, but they all have certain limitations. For example, the DKDP crystal has a large electro-optic coefficient (γ63=25pm / V) and a high laser damage threshold, but it is easy to absorb moisture; the LN crystal has stable physical and chemical properties, but the laser damage threshold is not high, and both crystals have a large "ringing effect" at high frequencies, which affects the efficiency. RTP crystals can be used in the mid-infrared band above 2μm, but due to low symmetry, a temperature compensation configuration needs to be designed. LGS crystals have advantages in transmission band, laser damage threshold, symmetry, physical and chemical stability, etc., and have achieved a series of results in mid-infrared and high repetition rate electro-optical Q-switched pulse laser output. However, its electro-optic coefficient is relatively small (γ 11 =2.1pm / V), higher repetition rate and longer wavelength pulse laser output requires higher driving voltage, the corresponding driving power supply cost is high, and the safety and circuit design requirements during use are stringent, which limits the scope of application.

[0004] Therefore, on the basis of maintaining the excellent performance of lanthanum gallium silicate crystals, optimizing the electro-optical coefficient of this family of crystals through effective means and then reducing the driving voltage is a new way to promote the further development of mid-infrared high-repetition-rate pulsed laser technology. Summary of the invention

[0005] In view of the current problem that the driving voltage required for high-repetition-rate mid-infrared pulse laser output by lanthanum gallium silicate crystals is high and the cost of purchasing driving power is high, the present invention provides a novel electro-optic coefficient optimization method for lanthanum gallium silicate crystals to reduce the driving voltage of electro-optic switches and thus reduce costs. By introducing different ions into the octahedral group of lanthanum gallium silicate crystals for mixing, the electron cloud structure and lattice vibration of the crystal polyhedral group are regulated, the response to the external field is enhanced, the refractive index and dielectric constant variation are adjusted, and the linear electro-optic coefficient is optimized.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A novel electro-optic coefficient optimization method for a novel lanthanum gallium silicate crystal, wherein the general structure formula of the lanthanum gallium silicate crystal is A3BC3D2O 14 By introducing different ions into the BO6 octahedral group for mixing, the electron cloud structure and lattice vibration of the group are regulated to achieve the optimization of the electro-optical coefficient.

[0008] Preferably, Ga is used at the B position. 3+ 、Zr 4+ The La3ZrGa5O 14 and La3Ga5SiO 14 The formation of lanthanum gallium zirconium silicate La3Zr in different proportions x Ga5Si 1-x O 14 (0<x<1) crystal.

[0009] Preferably, the lanthanum gallium silicate electro-optical crystal is prepared by a Czochralski method, which specifically comprises the following steps:

[0010] (1) Calculating and weighing raw materials according to the molar ratio of the lanthanum gallium silicate electro-optical crystal, mixing them evenly, pressing them into blocks, and then sintering them at a sintering temperature of 1300 to 1400° C. for a holding time of 10 to 20 hours to obtain a polycrystalline material;

[0011] (2) Tie the seed crystal to the seed crystal rod with platinum wire and place it in a pulling furnace;

[0012] (3) Using an iridium crucible to melt the material, the polycrystalline material is placed in an iridium crucible and heated to fully melt, and the temperature is kept for 5 to 8 hours, and then the temperature is further raised by 25 to 50° C., and after keeping the temperature for 3 to 5 hours, the seed is planted to grow the crystal;

[0013] (4) During the crystal growth stage, the necking, shoulder release, equal diameter, and lifting and cooling stages are carried out in sequence, and the crystal is taken out after cooling to room temperature.

[0014] Preferably, the pulling speed in the necking stage is 1.0-2.0 mm / h, and the rotation speed is 15-25 rpm; the pulling speed in the shoulder expansion and equal diameter stage is 0.8-1.5 mm / h, and the rotation speed is 15-25 rpm; the pulling and cooling stage adopts a slow-first-fast-then cooling method, and the cooling time is 75-90 hours.

[0015] Preferably, the purity of the raw materials lanthanum oxide (La2O3), gallium oxide (Ga2O3), and silicon oxide (SiO2) is 99.99%, and the purity of the raw material zirconium oxide (ZrO2) is 99.975%.

[0016] Preferably, the raw materials are mixed in step (1) using a mixer.

[0017] Preferably, the seed crystal is a lanthanum gallium silicate crystal, the cross-sectional shape of the seed crystal is square, and the seed crystal orientation is <0001> , the dimensions are 4mm×4mm×26mm.

[0018] Preferably, the iridium crucible is heated by a medium frequency induction coil, the diameter of the medium frequency induction coil is 180 mm, and the medium frequency induction power supply and the pulling furnace are cooled by an industrial water cooler.

[0019] The present invention also discloses La3Zr obtained according to the above method. x Ga5Si 1-x O 14 Application of (0<x<1) crystal in the manufacture of electro-optical devices.

[0020] Beneficial effects of the present invention:

[0021] The present invention discloses a method for optimizing the electro-optic coefficient of a novel lanthanum gallium silicate crystal. The method comprises: using Zr in the B-position octahedral group of the lanthanum gallium silicate crystal to optimize the electro-optic coefficient of the lanthanum gallium silicate crystal. 4+ Ions and Ga 3+ The mixing of ions makes La3ZrGa5O 14 and La3Ga5SiO 14 By forming lanthanum gallium zirconium silicate crystals in different proportions, the electron cloud structure and lattice vibration of the crystal octahedral group are regulated, the response to the external field is enhanced, the refractive index is increased, and the change in relative dielectric constant when pressurized is increased, thereby optimizing the electro-optical coefficient. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0023] Figure 1 The attached figure shows the lanthanum gallium silicate crystal A3BC3D2O provided by the present invention. 14 Schematic diagram of the structure.

[0024] Figure 2 The accompanying figure shows the Zr provided in Example 1 of the present invention. 4+ :Si 4+ The ratio of 5:5 is lanthanum gallium zirconate (La3Zr 0.5 Ga5Si 0.5 O 14 )Crystal diagram.

[0025] Figure 3 The accompanying figure shows the Zr provided in Example 1 of the present invention. 4+ :Si 4+ The ratio of 5:5 is lanthanum gallium zirconate (La3Zr 0.5 Ga5Si 0.5 O 14 ) crystal and lanthanum gallium silicate (LGS) crystal. At the same wavelength, La3Zr 0.5 Ga5Si 0.5 O 14 The refractive index of the crystal is greater than that of the LGS crystal, which is beneficial to increase the electro-optic coefficient.

[0026] Figure 4 The accompanying figure shows the Zr provided in Example 1 of the present invention. 4+ :Si 4+ The ratio of 5:5 is lanthanum gallium zirconate (La3Zr 0.5 Ga5Si 0.5 O 14 ) The laser damage threshold of the crystal. The test spot diameter is 1mm, the pulse width is 10ns, the wavelength is 1064nm, and the laser damage threshold is 955MW / cm 2 Its laser damage threshold is similar to that of LGS (950MW / cm 2 ) is equivalent, retaining the excellent property of high laser damage threshold of lanthanum gallium silicate crystals.

[0027] Figure 5 The accompanying figure shows the Zr provided in Example 1 of the present invention. 4+ :Si 4+ The ratio of 5:5 is lanthanum gallium zirconate (La3Zr 0.5 Ga5Si 0.5 O 14 ) A graph showing the relationship between light intensity transmittance and voltage when the crystal is pressurized. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example:

[0030] A La3Zr x Ga5Si 1-x O 14 (0<x<1) crystal: in the lanthanum gallium silicate crystal structure (general formula is A3BC3D2O 14 ) uses Zr 4+ and Ga 3+ Mixed to form La3Zr x Ga5Si 1-x O 14 Crystal, by regulating Zr 4+ Ions and Si 4+ The ratio of ions is 5:5, and La3Zr is designed. 0.5 Ga5Si 0.5 O 14 Crystal (abbreviated as LZGS).

[0031] The above-mentioned La3Zr 0.5 Ga5Si 0.5 O 14 The crystal preparation method specifically comprises the following steps:

[0032] (1) Weigh the raw materials with a molar ratio of La2O3, Ga2O3, ZrO2, and SiO2 of 0.3:0.5:0.1:0.1. The purity of lanthanum oxide (La2O3), gallium oxide (Ga2O3), and silicon dioxide (SiO4) is 99.99%, and the purity of zirconium dioxide (ZrO4) is 99.975%. Put the prepared raw materials in a mixer and mix them thoroughly. Put the mixed materials in a press to press them into blocks, and then put them into a muffle furnace for sintering. Set the muffle furnace sintering temperature to 1380°C and the insulation time to 20h to allow them to undergo sufficient solid-phase reaction to obtain polycrystalline materials.

[0033] (2) The orientation is <0001> LGS is used as the seed crystal. The cross-section of the seed crystal is square and the size is 4mm×4mm×26mm. The seed crystal is tied to the seed crystal rod with platinum wire and placed in a pulling furnace. The polycrystalline material is placed in an iridium crucible and heated to melt completely. The melting point is 1500℃ and the temperature is kept for 5 to 8 hours. Then the temperature is raised by 50℃ and kept for 10 hours before the seed is planted to grow the crystal.

[0034] (3) Crystal growth stage: The pulling speed in the necking stage is 2.0 mm / h and the rotation speed is 20 rpm; the pulling speed in the shoulder expansion and equal diameter stages is 1.2 mm / h and the rotation speed is 20 rpm; the cooling stage adopts a slow-first-fast-then cooling method, first cooling at a rate of 10 °C / h for 68 h, and then cooling at a rate of 20 °C / h for 14 h to room temperature, and the total cooling time is 80 h.

[0035] The crystal prepared in this example belongs to the same trigonal system and 32 point group as the LGS crystal. 4+ The introduction of ions changes the crystal vibration and the electron cloud structure, which is beneficial to increase the electro-optic coefficient. 0.5 Ga5Si 0.5 O 14 The crystal has two different electro-optic coefficients γ 11 and γ 41 , electro-optic coefficient γ 11 Ratio 41 Large. According to the formula γ=γ e +γ o +γ a It can be seen that the electro-optic coefficient of a crystal is related to the response of the charge movement and lattice vibration in the crystal to the external field (reference: Natl Sci Rev, 2021, Vol. 8, nwaa104). Under the action of an external electric field, the additional electric polarization ΔP is related to the slight distortion of the ion lattice in the crystal and the redistribution of the charge on the bond. Introducing cations of different valence states and radii into the B-site octahedral group of the lanthanum gallium silicate crystal can change the charge distribution, and thus the electron energy band distribution. Due to the differences in the electron cloud structures of different ions, the interaction between different electron clouds changes the relative dielectric constant of the crystal and adjusts the refractive index of the crystal. The lattice vibration can be regulated by ion mixing in the B-site octahedral group. Under the action of an external electric field, the joint contribution of charge movement and lattice vibration to the electro-optic coefficient increases the change in the relative dielectric constant Δε and the change in the refractive index of the principal axis of the new optical index body Δn, ultimately achieving the purpose of optimizing the electro-optic coefficient.

[0036] For the La3Zr 0.5 Ga5Si 0.5 O 14 When measuring the electro-optic coefficient of a LZGS crystal, the voltage is related to the transmittance as follows: Figure 5 As shown, the LZGS electro-optic coefficient γ is fitted 11 2.5pm·V -1 Under the same conditions, the LGS electro-optic coefficient γ was measured 11 2.18 pm·V -1 When used for 2μm electro-optical Q switches, LZGS and LGS crystals with the same specifications are used, and their V λ / 4The voltage can be reduced by about 11%. For example, when L / d=5, the quarter voltage can be reduced from 6600V to 5900V.

[0037] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A lanthanum gallium silicate crystal La 3 Zr 0.5 Ga 5 Si 0.5 O 14 Application in the manufacture of electro-optical devices.

2. The use according to claim 1, It is characterized in that The lanthanum gallium silicate electro-optical crystal is prepared by a Czochralski method, which specifically includes the following steps: (1) Calculate and weigh the raw materials according to the chemical formula molar ratio, mix them evenly, press them into blocks, and then sinter them at a sintering temperature of 1300-1400°C for a holding time of 10-20 h to obtain polycrystalline materials; (2) Tie the seed crystal to the seed crystal rod with platinum wire and place it in the pulling furnace; (3) Using an iridium crucible to melt the material, place the polycrystalline material in an iridium crucible and heat until it is fully melted. Keep the temperature for 5-8 hours, then continue to raise the temperature by 25-50°C. Keep the temperature for 3-5 hours before planting seeds to grow crystals. (4) During the crystal growth stage, the necking, shoulder release, equal diameter, and lifting and cooling stages are carried out in sequence. The crystal is taken out after cooling to room temperature.

3. The use according to claim 2, It is characterized in that The pulling speed in the necking stage is 1.0~2.0 mm / h, and the rotation speed is 15~25 rmp; the pulling speed in the shoulder expansion and equal diameter stage is 0.8~1.5 mm / h, and the rotation speed is 15~25 rmp; the pulling and cooling stage adopts a slow-first-fast-later cooling method, and the cooling time is 75~90 h.

Citation Information

Patent Citations

  • Niobium barium gallium silicate crystal, preparation and use thereof

    CN101275277A

  • Lanthanum gallium silicate series crystal growing method

    CN106222750A

  • Effective nonlinear optical coefficient optimization method of silicic acid gallium lanthanum family solid solution crystal

    CN115185137A

  • Effective nonlinear optical coefficient optimization method for langasite group solid solution crystals

    US20230015923A1