P-type GaN ohmic contact structure, its preparation method and application
By growing a high-purity Mg layer on the surface of P-type GaN and forming a loose contact layer structure, combined with metal electrode deposition, the problem of high contact resistivity in GaN-based optoelectronic devices was solved, and more efficient ohmic contact performance was achieved.
Patent Information
- Application Number
- CN202311358767.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-19
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-10-19
AI Technical Summary
Existing technologies make it difficult to achieve efficient P-type GaN ohmic contacts in GaN-based optoelectronic devices, resulting in high contact resistivity and affecting device performance.
A high-purity Mg layer is grown on the surface of P-type GaN, and a loose contact layer structure is formed by in-situ annealing and acid washing. Combined with metal electrode deposition, the tunneling effect is used to reduce the potential barrier and lower the contact resistance.
This significantly reduces the specific contact resistivity of the P-type GaN ohmic contact, thereby improving the electrical performance of the device.
Smart Images

Figure CN117317800B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor device technology, and in particular to a P-type GaN ohmic contact structure, its preparation method, and its application. Background Technology
[0002] Gallium nitride (GaN)-based materials (including GaN, AlN, InN, and their alloys) are the third generation of semiconductors after silicon and gallium arsenide. With a bandgap ranging from 0.7 to 6.2 eV, they have broad application prospects and research value in optoelectronics and microelectronics. GaN-based optoelectronic devices, such as Micro-LEDs and lasers, possess advantages such as small size, high efficiency, long lifetime, and fast response speed, making them of great application value in both military and civilian fields.
[0003] Optimizing the ohmic contact performance of p-type GaN is a crucial technical challenge to overcome in order to obtain high-efficiency GaN devices. Because GaN-based optoelectronic devices experience high current densities during operation, the metal-semiconductor contact at the electrodes is particularly important. The ionization energy of Mg doped during p-type GaN growth is relatively high, resulting in a low ionization probability of Mg at room temperature, making it difficult to obtain p-type GaN materials with high hole concentrations. The current mainstream approach is to increase the Mg doping concentration to 10⁻⁶. 20 While the above-mentioned quantities are significant, higher Mg doping concentrations can lead to reduced internal carrier mobility, affecting the device's electrical performance. Furthermore, high-performance ohmic contacts not only require high-quality p-type GaN material but also demand a specific contact resistivity as low as 10-1 at the gold-semiconductor contact. -5 Ω·cm 2 Obtaining high-quality P-type GaN gold-semiconductor ohmic contacts is a significant challenge, particularly given the extremely high work function of P-type GaN. This is primarily because P-type GaN has an exceptionally high work function, making it difficult to find a matching metal electrode to form an ohmic contact. This results in a high potential barrier at the gold-semiconductor contact interface, increasing contact resistance and impacting device efficiency. Current mainstream methods typically involve growing an additional heavily doped contact layer at the interface to utilize the tunneling effect and lower the potential barrier. Examples include highly Mg-doped P-type GaN or P-type InGaN. Furthermore, due to the high reactivity of Ga in GaN, GaO often adheres to the outermost GaN surface. x Before depositing metal electrodes, oxides such as those present in the GaN ohmic contact need to be removed by rinsing with dilute hydrochloric acid or KOH to prevent them from increasing the contact barrier and reducing device performance. Therefore, it is urgent to solve these problems and fabricate a novel ohmic contact structure to obtain a highly efficient P-type GaN ohmic contact, thereby reducing the device operating voltage and improving performance.
[0004] The information disclosed in this background section is intended only to enhance the understanding of the overall background of the invention and should not be construed as an admission or in any way implying that the information constitutes prior art known to those skilled in the art. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing and applying a P-type GaN ohmic contact structure, which can reduce the specific contact resistivity and improve the performance of the P-type GaN ohmic contact.
[0006] To achieve the above objectives, embodiments of the present invention provide a method for fabricating a P-type GaN ohmic contact structure, comprising: growing an epitaxial layer on a substrate, the epitaxial layer comprising a Mg-doped P-type GaN layer at the top layer; forming a Mg layer on the surface of the Mg-doped P-type GaN layer; in-situ annealing and acid washing to form a loose contact layer structure in the Mg layer; and fabricating a metal electrode on the surface of the Mg layer.
[0007] In one or more embodiments of the present invention, the epitaxial layer is grown using a molecular beam epitaxy apparatus, and the Mg layer is deposited within the same growth chamber of the molecular beam epitaxy apparatus.
[0008] In one or more embodiments of the present invention, the thickness of the Mg-doped P-type GaN layer is 20 nm to 500 nm.
[0009] In one or more embodiments of the present invention, the doping concentration of Mg in the Mg-doped p-type GaN layer is 5*10⁻⁶. 17 cm -3 -1*10 21 cm -3 .
[0010] In one or more embodiments of the present invention, the ambient temperature for depositing the Mg layer is 250°C-1000°C.
[0011] In one or more embodiments of the present invention, the deposition time of the Mg layer is 1 min to 30 min.
[0012] In one or more embodiments of the present invention, the thickness of the Mg layer is 1 nm to 10 nm.
[0013] In one or more embodiments of the present invention, the in-situ annealing temperature is 300°C-800°C.
[0014] In one or more embodiments of the present invention, the in-situ annealing time is 1 min to 30 min.
[0015] In one or more embodiments of the present invention, the in-situ annealing atmosphere includes nitrogen, oxygen, or a mixture of nitrogen and oxygen.
[0016] In one or more embodiments of the present invention, the atmosphere for in-situ annealing is a mixture of nitrogen and oxygen, wherein the ratio of nitrogen to oxygen is 4:1.
[0017] In one or more embodiments of the present invention, the solution used for pickling is an inorganic acid solution, including hydrochloric acid, sulfuric acid, and nitric acid.
[0018] In one or more embodiments of the present invention, the solution used for pickling is a dilute hydrochloric acid solution with a ratio of HCl:H2O = 1:3.
[0019] In one or more embodiments of the present invention, the metal electrode can be prepared using electron beam evaporation or magnetron sputtering.
[0020] In one or more embodiments of the present invention, a metal electrode is prepared on the surface of the Mg layer, comprising: preparing a first metal electrode on the surface of the Mg layer, wherein the material of the first metal electrode includes one or more of Pd, Pt, Ni, Pt, Al, Ti, etc., and the thickness of the first metal electrode is 1 nm-300 nm; and forming a second metal electrode on the surface of the first metal electrode, wherein the material of the second metal electrode includes Au, and the thickness of the second metal electrode is greater than or equal to 30 nm.
[0021] In one or more embodiments of the present invention, the epitaxial layer further includes a GaN buffer layer formed on the surface of the substrate, an undoped GaN layer formed on the surface of the GaN buffer layer, and the Mg-doped P-type GaN layer formed on the surface of the undoped GaN layer.
[0022] In one or more embodiments of the present invention, the epitaxial layer and the Mg layer are formed in an ultra-high vacuum environment, wherein the pressure range of the ultra-high vacuum environment is 10. -10 Torr~10 -11 Torr.
[0023] In one or more embodiments of the present invention, the purity of the Mg source used to deposit the Mg layer is 6N (99.9999%).
[0024] In one or more embodiments of the present invention, after the metal electrode is prepared, a secondary annealing process is performed.
[0025] The present invention also provides a P-type GaN ohmic contact structure, comprising: a substrate; an epitaxial layer formed on the surface of the substrate, the epitaxial layer comprising a Mg-doped P-type GaN layer at the top layer; a Mg layer formed on the surface of the Mg-doped P-type GaN layer; and a metal electrode formed on the surface of the Mg layer.
[0026] The present invention also provides an application of the P-type GaN ohmic contact structure prepared according to the above preparation method in laser devices.
[0027] Compared with the prior art, the method for fabricating a P-type GaN ohmic contact structure according to the present invention can significantly prevent GaN oxidation, reduce the P-type GaN doping concentration, and reduce the potential barrier by utilizing the tunneling effect at the gold-semiconductor interface, thereby reducing the contact resistance and improving device performance.
[0028] The method for preparing a P-type GaN ohmic contact structure according to an embodiment of the present invention can reduce the specific contact resistivity and improve the performance of the P-type GaN ohmic contact. Attached Figure Description
[0029] Figure 1 This is a process flow diagram of a method for preparing a P-type GaN ohmic contact structure according to an embodiment of the present invention.
[0030] Figure 2 This is a schematic diagram of a P-type GaN ohmic contact structure according to an embodiment of the present invention.
[0031] Figure 3 This is an atomic force microscope image of a p-type GaN ohmic contact structure according to an embodiment of the present invention. Detailed Implementation
[0032] The specific embodiments of the present invention will now be described in detail with reference to the accompanying drawings, but it should be understood that the scope of protection of the present invention is not limited to the specific embodiments.
[0033] Unless otherwise expressly stated, throughout the specification and claims, the term "comprising" or its variations such as "including" or "comprises" shall be understood to include the stated elements or components without excluding other elements or other components.
[0034] As mentioned in the background section, existing methods for improving ohmic contacts at gold-semiconductor interfaces mainly focus on highly doped GaN layers and highly doped InGaN layers. However, these methods all have some drawbacks. For example, increasing the doping concentration of Mg to a high level may lead to a series of problems such as decreased carrier mobility and reduced device performance. In traditional gold-semiconductor contact structures, GaO is often present at the electrode-semiconductor interface. xOxides (the outer layer of Ga exposed to air is easily oxidized to form GaO) X These oxides reduce hole concentration, increase contact barriers, and thus increase contact resistance, thereby affecting the electrical performance of the device. In addition, although conventional acid washing can temporarily remove oxides from the device surface, it is difficult to maintain a completely vacuum environment during the transport process after cleaning and before metal deposition. Secondary oxidation of the surface often easily occurs during this exposure to air, leading to a decrease in device performance.
[0035] To address the aforementioned technical problems, this invention proposes a method for fabricating a p-type GaN ohmic contact structure. The p-type GaN ohmic contact structure is prepared by growing or depositing a thin layer of high-purity Mg on the surface of p-type GaN. Following this, the sample undergoes annealing and acid washing, and a metal electrode is deposited. This significantly prevents GaN oxidation, reduces the p-type GaN doping concentration, and utilizes the tunneling effect at the gold-semiconductor interface to lower the potential barrier, reduce contact resistance, and improve device performance. Using this method, the specific contact resistivity can be reduced, and the performance of the p-type GaN ohmic contact can be improved.
[0036] like Figure 1 As shown, a method for preparing a P-type GaN ohmic contact structure according to an embodiment of the present invention includes: s1, growing an epitaxial layer on a substrate, the epitaxial layer including a Mg-doped P-type GaN layer at the top layer; s2, forming a Mg layer on the surface of the Mg-doped P-type GaN layer; s3, annealing and acid washing in situ to make the Mg layer form a loose contact layer structure; s4, preparing a metal electrode on the surface of the Mg layer.
[0037] In this process, steps s1 and s2 are both performed within the same growth chamber of a molecular beam epitaxy (MBE) apparatus. Specifically, the epitaxial layer is first grown within the MBE chamber, and then the Mg source is directly activated within the MBE chamber to deposit the Mg layer. This high-purity Mg layer not only serves as a contact layer to lower the potential barrier but also reduces the doping concentration of Mg-doped p-type GaN, eliminating the need for high Mg doping of GaN and thus improving overall carrier mobility and electrical performance. Furthermore, the deposited Mg layer prevents oxidation of the top GaN layer. In step s3, in-situ annealing eliminates material stress. The MgO layer formed after annealing the thin Mg layer is not dense; subsequent rinsing with an inorganic acid solution creates a porous contact layer structure, facilitating subsequent contact between the metal electrode and the semiconductor.
[0038] The following section elaborates on the preparation method of the p-type GaN ohmic contact structure of this application to facilitate understanding of the content of this application.
[0039] First, a p-type GaN epitaxial layer 20 is epitaxially grown on substrate 10 using a molecular beam epitaxy (MBE) apparatus. Epitaxial layer 20 includes a GaN buffer layer 21, an undoped GaN layer 22, and a Mg-doped p-type GaN layer 23, grown sequentially. Figure 2 As shown. All p-type GaN materials were grown using molecular beam epitaxy (MBE). For p-type materials, the growth chamber of the MBE equipment was an ultra-high vacuum environment (10⁻⁶ m² / 40⁻¹²). -10 Torr~10 -11 The source material (Tor) is a high-purity element (99.9999%), and the prepared single-crystal material has extremely high purity. Therefore, it can alleviate the compensation effect of Mg atoms when preparing Mg-doped P-type GaN layers. In this embodiment, the thickness of the Mg-doped P-type GaN layer is 20nm-500nm. The doping concentration of Mg in the Mg-doped P-type GaN layer can be 5*10¹⁷cm⁻³-1*10²¹cm⁻³.
[0040] Secondly, the Mg source is directly turned on in the growth chamber of the molecular beam epitaxy (MBE) equipment, and a high-purity thin Mg atomic layer (Mg layer 30) is deposited or evaporated on the surface of the already grown p-type GaN layer, such as... Figure 2 As shown. The Mg source had a purity of 6N (99.9999%), and the deposition rate was approximately 0.5 nm / min. The surface of the epitaxially grown sample can be found in [reference needed]. Figure 3 The atomic force microscopy images still show good step flow growth morphology and low roughness (RMS roughness: 1.98 nm). This high-purity Mg layer not only serves as a contact layer to lower the potential barrier, but also reduces the doping concentration of the underlying P-type GaN layer, eliminating the need for high Mg doping of GaN and thus improving overall carrier mobility and electrical performance. Furthermore, the Mg layer prevents oxidation of the top GaN layer. Specifically, during direct cavity Mg deposition, the Mg furnace temperature in the molecular beam epitaxy equipment can be 250℃–1000℃, the deposition time can be 1–30 minutes, and the thickness of the thin Mg atomic layer can be 1 nm–10 nm.
[0041] Next, the sample undergoes in-situ annealing to relieve material stress. The in-situ annealing temperature can be 300℃–800℃, the annealing time can be 1 min–30 min, and the annealing atmosphere can be nitrogen, oxygen, or a mixture of nitrogen and oxygen. Preferably, the annealing atmosphere is a mixture of nitrogen and oxygen, with a nitrogen:oxygen ratio of 4:1. The MgO layer formed after annealing is not dense; subsequent rinsing with an inorganic acid solution can create loose pores, which facilitates subsequent contact between the metal electrode and the semiconductor.
[0042] Then, the sample is acid-washed to remove the residual MgO layer on the surface and to form a contact layer structure with loose pores. This Mg layer is not dense after acid washing and has channels similar to pores inside, through which charge carriers can complete the transport process. The inorganic acid solution used to remove the oxide layer can be an inorganic acid solution such as hydrochloric acid, sulfuric acid, or nitric acid, preferably a dilute hydrochloric acid solution with a ratio of HCl:H2O = 1:3.
[0043] Finally, the CTLM transport ring pattern is prepared through photolithography, deposition of contact metal electrodes, lift-off, and secondary annealing, followed by contact resistivity testing. The deposition equipment used for the contact metal electrodes can be electron beam evaporation, magnetron sputtering, or other coating equipment. The deposited metal electrodes consist of two layers: the first layer is a first metal electrode, commonly made of one or more of Pd, Pt, Ni, Al, and Ti, with a common thickness of 1 nm to 300 nm. The second layer is a second metal electrode, commonly made of Au, with a thickness generally greater than or equal to 30 nm. When the aforementioned P-type GaN material is used in a laser, the preferred electrode material is Pd / Pt / Au (30 nm / 30 nm / 50 nm).
[0044] In the above embodiments, the Mg layer was deposited directly in an MBE apparatus with a vacuum environment. In other embodiments, it can also be achieved by electron beam metal deposition, as long as an oxygen-free environment is maintained throughout the subsequent transfer process to eliminate any potential oxidation risks.
[0045] refer to Figure 2 As shown, based on the above-described method for fabricating a p-type GaN ohmic contact structure, this application also proposes a p-type GaN ohmic contact structure, including a substrate 10, an epitaxial layer 20 formed on the surface of the substrate 10, a Mg layer 30 formed on the surface of the epitaxial layer 20, and a metal electrode (not shown) formed on the surface of the Mg layer 30. The epitaxial layer 20 includes a GaN buffer layer 21 formed on the surface of the substrate 10, an undoped GaN layer 22 formed on the surface of the GaN buffer layer 21, and a Mg-doped p-type GaN layer 23 formed on the surface of the undoped GaN layer 22. The thickness of the Mg-doped p-type GaN layer is 20 nm-500 nm. The doping concentration of Mg in the Mg-doped p-type GaN layer is 5*10⁻⁶. 17 cm -3 ~1*10 21 cm -3The thickness of the Mg layer is 1 nm to 10 nm. The metal electrode includes a first metal electrode and a second metal electrode. The material of the first metal electrode includes one or more of Pd, Pt, Ni, Al, and Ti, and the thickness of the first metal electrode is 1 nm to 300 nm. The material of the second metal electrode includes Au, and the thickness of the second metal electrode is greater than or equal to 30 nm.
[0046] The present invention also provides an application of the P-type GaN ohmic contact structure prepared according to the above preparation method in laser devices.
[0047] Compared with existing technologies, the method for fabricating a P-type GaN ohmic contact structure according to the embodiments of the present invention is a novel method for fabricating a P-type GaN ohmic contact structure by depositing a Mg atomic layer in a growth chamber using an MBE device. This method utilizes the high-purity Mg atomic beam provided by the MBE device to directly grow a thin high-purity Mg layer on the surface of the P-type GaN. Annealing and acid washing form a new contact layer structure, which not only protects the underlying GaN layer but also reduces the required impurity concentration and lowers the potential barrier at the contact interface. The loose, thin Mg layer as a contact layer can effectively reduce contact resistance and improve device performance, making it a feasible method for improving ohmic contact efficiency.
[0048] The p-type GaN ohmic contact structure and its performance of this application will be described in detail below with reference to specific embodiments and corresponding comparative examples.
[0049] Example 1:
[0050] Step 1: Using molecular beam epitaxy (MBE), a 500 nm undoped GaN layer is epitaxially grown on the GaN buffer layer of a sapphire substrate. Then, a Mg-doped P-type GaN layer is grown, with a thickness of 200 nm. The Mg doping concentration can be reduced to 5 × 10⁻⁶. 18 cm -3 .
[0051] Step 2: Using molecular beam epitaxy (MBE), a high-purity thin Mg layer is grown on the P-type GaN epitaxial layer grown in Step 1. When the substrate temperature drops to 70°C, the Mg source is turned on, the Mg furnace temperature is adjusted to 350°C, and the baffle is opened for 15 minutes to deposit several atomic layers of Mg onto the outermost P-type GaN layer.
[0052] Step 3: The epitaxial wafer obtained in Step 2 above is annealed in a rapid annealing furnace at 650°C for 2 minutes in an atmosphere of nitrogen:oxygen = 4:1, so that a loose Mg / MgO contact layer is formed on the surface of the epitaxial wafer.
[0053] Step 4: The epitaxial wafer obtained in Step 3 above is acid-washed with HCl:H2O (1:3) for 10 minutes, rinsed with deionized water, and then ultrasonicated with acetone, isopropanol and anhydrous ethanol for 10 minutes each. Then it is rinsed with deionized water 5 times and dried with a nitrogen gun to remove excess MgO and other surface oxides, ensuring that the contact interface is clean and free of impurities.
[0054] Step 5: After cleaning, the surface of the epitaxial wafer is pretreated with HMDS (hexamethyldisilazane) for 10 minutes, then photoresist is spin-coated and dried on a hot plate at 95°C for 90 seconds. After that, the transport ring is photolithographically ...
[0055] Step 6: Deposit three metal layers of Pd / Pt / Au (30nm / 30nm / 50nm) on the photolithographically lithographic P-type GaN using an electron beam evaporation device, and then strip it with acetone / NMP solution (N-methylpyrrolidone) to remove residual photoresist. After multiple cleanings, the transport ring metal pattern is obtained.
[0056] Step 7: Perform secondary annealing using a rapid annealing furnace. Anneal the metal pattern of the transfer ring at 650℃ in a nitrogen atmosphere for 90 seconds. Then, use a four-probe system to test the circular transfer ring model to obtain multiple sets of resistivity data. Calculate the specific contact resistivity data.
[0057] Comparative Example 1:
[0058] Step 1: Using molecular beam epitaxy, a 500 nm undoped GaN layer is epitaxially grown on the GaN buffer layer of a sapphire substrate, followed by the growth of a Mg-doped P-type GaN layer. The thickness of the Mg-doped P-type GaN layer is 200 nm, and the Mg doping concentration is increased to 5 × 10⁻⁶. 20 cm -3 .
[0059] Step 2: The epitaxial wafer obtained in Step 1 is acid-washed with HCl:H2O (1:3) for 10 minutes, rinsed with deionized water, and then ultrasonicated with acetone, isopropanol and anhydrous ethanol for 10 minutes each. Then it is rinsed with deionized water 5 times and dried with a nitrogen gun to ensure that the contact interface is clean and free of impurities.
[0060] Step 3: After cleaning, the surface of the epitaxial wafer is pretreated with HMDS (hexamethyldisilazane) for 10 minutes, then photoresist is spin-coated and dried on a hot plate at 95°C for 90 seconds. After that, the transport ring is photolithographically ...
[0061] Step 4: The P-type GaN after photolithography is deposited with three metal layers of Pd / Pt / Au (30nm / 30nm / 50nm) using an electron beam evaporation device, and then stripped with acetone / NMP solution (N-methylpyrrolidone) to remove residual photoresist. After multiple cleanings, the transport ring metal pattern is obtained.
[0062] Step 5: Anneal the metal pattern of the transfer ring using a rapid annealing furnace. Anneal the metal pattern of the transfer ring at 650℃ in a nitrogen atmosphere for 90s. Then, use a four-probe system to test the circular transfer ring model to obtain multiple sets of resistivity data. Calculate the specific contact resistivity data.
[0063] Comparative Example 2:
[0064] Step 1: Using an MOCVD device, an epitaxial growth of a 2 μm n-GaN layer is performed on the GaN buffer layer of a sapphire substrate, followed by the growth of a Mg-doped p-GaN layer. The thickness of the Mg-doped p-GaN layer is 400 nm, and the Mg doping concentration is 5 × 10⁻⁶. 18 cm -3 .
[0065] Step 2: The P-type GaN epitaxial layer grown in Step 1 was acid-washed with HCl:H2O (1:1) for 10 min, rinsed with deionized water, and then sonicated with acetone, isopropanol, and anhydrous ethanol for 10 min each, followed by rinsing with deionized water five times and drying with a nitrogen gun. The cleaned sample was then rapidly transferred to the electron beam evaporation chamber for Mg metal layer deposition. The metal source purity was 5N, and the evaporation rate was... The Mg layer has a vapor deposition thickness of 5 nm.
[0066] Step 3: The epitaxial wafer obtained in Step 2 above is annealed in a rapid annealing furnace at 650°C for 2 minutes in an atmosphere of nitrogen:oxygen = 4:1, so that a loose Mg / MgO contact layer is formed on the surface of the epitaxial wafer.
[0067] Step 4: The epitaxial wafer obtained in Step 3 above is acid-washed with HCl:H2O (1:3) for 10 minutes, rinsed with deionized water, and then ultrasonicated with acetone, isopropanol and anhydrous ethanol for 10 minutes each. Then it is rinsed with deionized water 5 times and dried with a nitrogen gun to remove excess MgO and other surface oxides, ensuring that the contact interface is clean and free of impurities.
[0068] Step 5: After cleaning, the surface of the epitaxial wafer is pretreated with HMDS (hexamethyldisilazane) for 10 minutes, then photoresist is spin-coated and dried on a hot plate at 95°C for 90 seconds. After that, the transport ring is photolithographically ...
[0069] Step 6: Deposit three metal layers of Pd / Pt / Au (30nm / 30nm / 50nm) on the photolithographically lithographic P-type GaN using an electron beam evaporation device, and then strip it with acetone / NMP solution (N-methylpyrrolidone) to remove residual photoresist. After multiple cleanings, the transport ring metal pattern is obtained.
[0070] Step 7: Perform secondary annealing using a rapid annealing furnace. Anneal the metal pattern of the transfer ring at 650℃ in a nitrogen atmosphere for 90 seconds. Then, use a four-probe system to test the circular transfer ring model to obtain multiple sets of resistivity data. Calculate the specific contact resistivity data.
[0071] Conclusion: The specific contact resistivity obtained in Example 1 was 4.1 x 10⁻⁶. -4 Ω·cm 2 Comparative Example 1 showed a specific contact resistivity of 2.1 x 10⁻⁶. -2 Ω·cm 2 Comparative Example 2 showed a specific contact resistivity of 5.4 x 10⁻⁶. -3 Ω·cm 2 .
[0072] As demonstrated by Examples 1, 1, and 2, the ohmic contact structure proposed in this invention exhibits lower resistivity and better contact performance, demonstrating its superiority. In Comparative Example 1, where the Mg doping concentration was increased, the performance degradation primarily stemmed from the decreased carrier mobility and deteriorated electrical performance caused by the high impurity doping concentration. In Comparative Example 2, the conventional method of evaporating the Mg layer cannot avoid interface oxidation during the transfer process. Furthermore, the presence of numerous impurities within the electron beam evaporation chamber reduces the purity of the deposited metal, ultimately leading to a decrease in ohmic contact performance.
[0073] The contact layer structure proposed in this invention utilizes the high-purity Mg atom beam provided by the MBE device to directly epitaxially thin a high-purity Mg layer on the surface of P-type GaN, and forms the layer after annealing and acid washing. This reduces the required impurity concentration and the potential barrier at the contact interface, effectively reducing contact resistance and improving device performance. It is a feasible method to improve ohmic contact efficiency.
[0074] The foregoing description of specific exemplary embodiments of the invention is for illustrative and explanatory purposes. These descriptions are not intended to limit the invention to the precise forms disclosed, and it will be apparent that many changes and variations can be made in accordance with the foregoing teachings. The exemplary embodiments were chosen and described in order to explain the specific principles of the invention and its practical application, thereby enabling those skilled in the art to implement and utilize various different exemplary embodiments of the invention, as well as various different choices and variations. The scope of the invention is intended to be defined by the claims and their equivalents.
Claims
1. A method for preparing a p-type GaN ohmic contact structure, characterized in that, include: Within the growth chamber of the molecular beam epitaxy apparatus, the range is maintained at 10. -10 Torr~10 -11 Torr's ultra-high vacuum environment allows for the growth of epitaxial layers on a substrate, the epitaxial layers including a Mg-doped P-type GaN layer at the top. Within the growth chamber of the same molecular beam epitaxy apparatus, the range is maintained at 10. -10 Torr~10 -11 Torr's ultra-high vacuum environment allows a Mg layer to be formed directly on the surface of the Mg-doped P-type GaN layer; In-situ annealing and pickling are performed to form a loose contact layer structure in the Mg layer; A metal electrode is fabricated on the surface of the Mg layer; The acid pickling is performed before the preparation of the metal electrode.
2. The method for preparing the p-type GaN ohmic contact structure as described in claim 1, characterized in that, The thickness of the Mg-doped P-type GaN layer is 20 nm-500 nm; and / or, the doping concentration of Mg in the Mg-doped P-type GaN layer is 5*10⁻⁶. 17 cm -3 -1*10 21 cm -3 .
3. The method for preparing the p-type GaN ohmic contact structure as described in claim 1, characterized in that, The ambient temperature for depositing the Mg layer is 250℃-1000℃; and / or the deposition time for the Mg layer is 1min-30min; and / or the thickness of the Mg layer is 1nm-10nm.
4. The method for preparing the p-type GaN ohmic contact structure as described in claim 1, characterized in that, The in-situ annealing temperature is 300℃-800℃; and / or the in-situ annealing time is 1min-30min; and / or the in-situ annealing atmosphere includes nitrogen, oxygen, or a mixture of nitrogen and oxygen.
5. The method for preparing the p-type GaN ohmic contact structure as described in claim 1, characterized in that, The in-situ annealing atmosphere is a mixture of nitrogen and oxygen, wherein the ratio of nitrogen to oxygen is 4:
1.
6. The method for preparing the p-type GaN ohmic contact structure as described in claim 1, characterized in that, The pickling solution is an inorganic acid solution, including hydrochloric acid, sulfuric acid, and nitric acid.
7. The method for preparing the p-type GaN ohmic contact structure as described in claim 1, characterized in that, The solution used for pickling is a dilute hydrochloric acid solution with a ratio of HCl:H2O = 1:
3.
8. The method for preparing the p-type GaN ohmic contact structure as described in claim 1, characterized in that, Fabricating a metal electrode on the surface of the Mg layer includes: A first metal electrode is prepared on the surface of the Mg layer. The material of the first metal electrode includes one or more of Pd, Pt, Ni, Al, and Ti, and the thickness of the first metal electrode is 1 nm to 300 nm. A second metal electrode is formed on the surface of the first metal electrode, the material of the second metal electrode including Au, and the thickness of the second metal electrode being greater than or equal to 30 nm.
9. The method for preparing the p-type GaN ohmic contact structure as described in claim 1, characterized in that, The epitaxial layer further includes a GaN buffer layer formed on the surface of the substrate, an undoped GaN layer formed on the surface of the GaN buffer layer, and a Mg-doped P-type GaN layer formed on the surface of the undoped GaN layer.
10. The method for preparing the p-type GaN ohmic contact structure as described in claim 1, characterized in that, The purity of the Mg source used to deposit the Mg layer is not less than 6N.
11. The method for preparing the p-type GaN ohmic contact structure as described in claim 1, characterized in that, After the metal electrode is prepared, a secondary annealing process is performed.
12. A p-type GaN ohmic contact structure, prepared by the method for preparing a p-type GaN ohmic contact structure as described in any one of claims 1-11, characterized in that, include: Substrate; An epitaxial layer is formed on the surface of the substrate, the epitaxial layer comprising a Mg-doped P-type GaN layer at the top layer; A Mg layer is formed on the surface of the Mg-doped P-type GaN layer, and the Mg layer has a loose porous structure; A metal electrode is formed on the surface of the Mg layer.
13. The application of the P-type GaN ohmic contact structure prepared by the preparation method according to any one of claims 1 to 11 in laser devices.
Citation Information
Patent Citations
P-GaN ohmic contact electrode, preparation method thereof and electronic element
CN116364768A