Injection molded parts formed from propylene polymer compositions

By combining propylene homopolymer and ethylene-α-olefin copolymer in a specific ratio, the problems of poor transparency and rigidity of polypropylene are solved, achieving high impact strength and transparency of injection molded parts, suitable for a variety of containers and shipping containers.

CN117321131BActive Publication Date: 2026-11-17PRIME POLYMER CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202280035863.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-05-26
Filing Date
2022-04-27
Publication Date
2026-11-17
Estimated Expiration
2042-04-27

AI Technical Summary

Technical Problem

In existing technologies, polypropylene has excellent transparency and rigidity, but poor cold resistance and impact resistance, making it difficult to improve impact strength while maintaining transparency and rigidity.

Method used

By using a combination of 60–90% by mass propylene homopolymer and 10–40% by mass ethylene-α-olefin copolymer, where the α-olefin in the ethylene-α-olefin copolymer is 1-hexene and does not contain nucleating agents, injection molded parts with excellent transparency, rigidity and impact strength are formed through the control of specific melt flow rate and density range.

Benefits of technology

It achieves an excellent balance of transparency, rigidity and impact strength, and is suitable for food containers, beverage containers, containers and other fields. It has good mechanical properties and transparency, especially in the case of thin-walled applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004554628970000101
    Figure BDA0004554628970000101
  • Figure BDA0004554628970000102
    Figure BDA0004554628970000102
Patent Text Reader

Abstract

The object of this invention is to obtain an injection-molded article formed from a propylene polymer composition that exhibits good transparency, rigidity, and impact strength; in other words, a good balance of transparency, impact strength, and rigidity. This invention relates to an injection-molded article formed from a propylene polymer composition containing: 60-90% by mass of a propylene polymer (A) satisfying conditions (a-i) and (a-ii) below; and 10-40% by mass of an ethylene-α-olefin copolymer (B) satisfying conditions (b-i) and (b-ii) below [wherein the total amount of (A) and (B) is set to 100% by mass]. Condition (a-i): The melt flow rate, measured according to JIS K6921 at a temperature of 230°C and a load of 2.16 kg, is in the range of 1-50 g / 10 min. Condition (a-ii): The content of α-olefins other than propylene, determined by infrared spectroscopy, is 1% by mass or less (including 0% by mass). Condition (b-i): The melt flow rate, measured according to JIS K6921 at a temperature of 190°C and a load of 2.16 kg, is in the range of 0.1–15 g / 10 min. Condition (b-ii): The density, measured according to JIS K6922, is in the range of 900–920 kg / m³. 3 The range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an injection-molded article formed from a propylene-based polymer composition, which exhibits good transparency, rigidity, and impact strength. Background Technology

[0002] Polyolefins (olefin polymers), represented by polyethylene and polypropylene, are highly regarded in various industries for their low energy consumption during production, lightweight nature, and excellent recyclability, making them a key component of the 3Rs (Reduce, Reuse, Recycle) for building a circular society. Polyolefins are used in a wide range of fields, including daily necessities, kitchenware, home appliances, machinery parts, electrical components, and automotive parts.

[0003] Among olefin polymers, polypropylene has excellent transparency, rigidity, and heat resistance, but compared with polyethylene, it has poor cold resistance and impact resistance. Therefore, many methods have been proposed to improve the impact resistance of polypropylene.

[0004] As a method to improve the impact strength without compromising the transparency and rigidity of polypropylene, a propylene block copolymer with a density of 900–919 kg / m³ is proposed. 3 The range of ethylene-α-olefin copolymers in propylene resin compositions (Patent Document 1).

[0005] Existing technical documents

[0006] Patent documents

[0007] Patent Document 1: International Publication No. 2010 / 074001 Summary of the Invention

[0008] The technical problem that the invention aims to solve

[0009] The purpose of this invention is to obtain an injection-molded body formed from a propylene polymer composition that has good transparency, rigidity and excellent impact strength, in other words, an excellent balance of transparency, impact strength and rigidity.

[0010] Technical solutions for solving technical problems

[0011] This invention relates to the following [1] to [8].

[0012] [1] An injection-molded article formed from a propylene polymer composition comprising: 60 to 90% by mass of a propylene polymer (A) satisfying conditions (a-i) and (a-ii) below; and 10 to 40% by mass of an ethylene-α-olefin copolymer (B) satisfying conditions (b-i) and (b-ii) below [wherein the total amount of (A) and (B) is set to 100% by mass].

[0013] Conditions (a-i): The melt flow rate, measured according to JIS K6921 at a temperature of 230°C and a load of 2.16 kg, is in the range of 1 to 50 g / 10 minutes.

[0014] Condition (a-ii): The content of α-olefins other than propylene, as determined by infrared spectroscopy, is less than 1% by mass (including 0% by mass).

[0015] Condition (b-i): The melt flow rate, measured according to JIS K6921 at a temperature of 190°C and a load of 2.16 kg, is in the range of 0.1 to 15 g / 10 minutes.

[0016] Condition (b-ii): Density measured according to JIS K6922 is 900-920 kg / m³ 3 The range.

[0017] [2] The injection-molded body as described in item [1], wherein the propylene polymer (A) is a propylene homopolymer.

[0018] [3] The injection-molded body as described in item [1], wherein the α-olefin of the ethylene-α-olefin copolymer (B) is 1-hexene.

[0019] [4] The injection-molded article as described in item [1], wherein the melt flow rate under the above conditions (b-i) is in the range of 1 to 5 g / 10 min.

[0020] [5] The injection-molded article as described in item [1], wherein the density under the above conditions (b-ii) is 903 to 915 kg / m³. 3 The range.

[0021] [6] The injection-molded article as described in item [1], wherein the content of the ethylene-derived structural units of the ethylene-α-olefin copolymer (B) is in the range of 83 to 93 mol%.

[0022] [7] The injection-molded article as described in item [1] is characterized in that: the above-mentioned propylene polymer composition does not contain a nucleating agent.

[0023] [8] The injection molded body as described in item [1] is any of the following: food container, beverage container, container and daily necessities.

[0024] Invention Effects

[0025] The injection-molded parts of the present invention have good transparency, rigidity and excellent impact strength, and are therefore suitable for use in food containers, beverage containers, containers, daily necessities and the like. Detailed Implementation

[0026] <Propylene Polymer (A)>

[0027] The propylene polymer (A) contained in the propylene polymer composition (hereinafter, sometimes simply referred to as the "composition") forming the injection-molded article (hereinafter, sometimes simply referred to as the "molded article") of the present invention is a propylene polymer that satisfies the following conditions (a-i) and conditions (a-ii).

[0028] Condition(a-i)

[0029] The melt flow rate (MFR) was measured according to JIS K6921 at a temperature of 230°C and a load of 2.16 kg. 230 The concentration is in the range of 1-50g / 10 minutes, preferably 1-30g / 10 minutes.

[0030] MFR 230 The propylene polymer (A) that meets the above range has good affinity with the ethylene-α-olefin copolymer (B) involved in the present invention.

[0031] MFR 230 When the above range is exceeded, the impact strength of the resulting molded article may be lower. If the above range is not met, the back pressure may be higher when the resulting composition is injection molded, making injection molding difficult.

[0032] The propylene polymer composition containing the propylene polymer (A) that meets the above range has good injection molding properties, and the resulting molded article has good mechanical properties and good transparency.

[0033] Condition (a-ii)

[0034] The α-olefin content, excluding propylene, determined by infrared spectroscopy, is 1% by mass or less (including 0% by mass), preferably 0.5% by mass or less (including 0% by mass), and more preferably a homopolymer of propylene.

[0035] As for the propylene-based polymer (A) involved in this invention, the resulting molded article has better heat resistance when using a homopolymer of propylene, and is therefore preferred.

[0036] The α-olefins other than propylene mentioned above are at least one α-olefin selected from ethylene and α-olefins with 4 to 8 carbon atoms.

[0037] The propylene polymer composition containing the propylene polymer (A) that meets the above range has good injection molding properties, and the resulting molded article has good mechanical properties and good transparency.

[0038] The propylene-based polymer (A) according to this invention can be obtained using various known manufacturing methods. Specifically, when the propylene-based polymer (A) contains only propylene, it can be obtained by homopolymerization of propylene or copolymerization with 1% by mass or less of an α-olefin in the presence of a known catalyst for olefin polymerization. Specific examples of catalysts for olefin polymerization include titanium-based catalysts and metallocene catalysts. Titanium-based catalysts are particularly preferred.

[0039] <Ethylene-α-olefin copolymer (B)>

[0040] The ethylene-α-olefin copolymer (B), one of the components contained in the propylene polymer composition forming the injection-molded article (hereinafter sometimes simply referred to as "molded article") of the present invention, is an ethylene-α-olefin copolymer that satisfies the following conditions (b-i) and (b-ii).

[0041] Condition(b-i)

[0042] Melt flow rate (MFR) measured according to JIS K6921 at a temperature of 190°C and a load of 2.16 kg. 190 The concentration is in the range of 0.1–15 g / 10 minutes, preferably 1–10 g / 10 minutes, and even more preferably 1–5 g / 10 minutes.

[0043] The ethylene-α-olefin copolymer (B) that meets the above-mentioned range has good affinity with the propylene polymer (A) involved in this invention. This is especially true when using MFR. 190 In the case of ethylene-α-olefin copolymer (B) in the range of 1 to 5 g / 10 minutes, the resulting molded articles have better impact resistance.

[0044] MFR 190 When the above range is exceeded, the impact strength of the resulting molded article may be lower. If the above range is not met, the back pressure may be higher when the resulting composition is injection molded, making injection molding difficult.

[0045] The propylene polymer composition containing an ethylene-α-olefin copolymer (B) that meets the above range has good injection molding properties, and the resulting molded article has good mechanical properties and good transparency.

[0046] Condition (b-ii)

[0047] The density, measured according to JIS K6922, is between 900 and 920 kg / m³. 3 Optimal weight is 903-915 kg / m³. 3 The range.

[0048] Molded articles obtained from propylene polymer compositions containing ethylene-α-olefin copolymers (B) that meet the above-mentioned range can greatly improve the impact strength of molded articles obtained from propylene polymers (A) alone. The impact strength is excellent, and the transparency and rigidity are hardly reduced. The balance of transparency, impact strength and rigidity is excellent.

[0049] The ethylene-α-olefin copolymer (B) involved in this invention is a copolymer with structural units derived from ethylene as the main component. The α-olefin is preferably at least one α-olefin selected from α-olefins having 3 to 8 carbon atoms, more preferably at least one α-olefin selected from propylene, 1-butene, 1-hexene, and 1-octene. Of particular preference is 1-hexene.

[0050] Typically, the content of ethylene-derived structural units in the ethylene-α-olefin copolymer (B) involved in this invention is in the range of 83 to 93 mol%, preferably 86 to 90 mol%.

[0051] Propylene polymer compositions

[0052] The propylene polymer composition forming the injection-molded article (hereinafter sometimes simply referred to as the "molded article") of the present invention is a composition containing 60-90% by mass, preferably 70-90% by mass, more preferably 70-80% by mass of the above-mentioned propylene polymer (A); and 10-40% by mass, preferably 10-30% by mass, more preferably 10-20% by mass of the above-mentioned ethylene-α-olefin copolymer (B) [wherein the total amount of (A) and (B) is set to 100% by mass].

[0053] Typically, the MFR of the propylene polymer compositions involved in this invention 230 The range is 1–50 g / 10 minutes, preferably 3–30 g / 10 minutes, and more preferably 5–20 g / 10 minutes.

[0054] In addition to the aforementioned propylene polymer (A) and ethylene-α-olefin copolymer (B), the propylene polymer composition involved in this invention may, without prejudice to the purpose of this invention, appropriately contain additives such as neutralizers, antioxidants, heat stabilizers, weathering agents, lubricants, ultraviolet absorbers, antistatic agents, anti-blocking agents, anti-fogging agents, dispersants, flame retardants, antibacterial agents, fluorescent whitening agents, crosslinking agents, and crosslinking aids; and the components exemplified by dyes, pigments, and other colorants (hereinafter referred to as "other components").

[0055] The propylene polymer compositions involved in this invention are preferably free of nucleating agents. Injection molded articles formed from compositions containing nucleating agents have improved transparency and rigidity, thus making it easier to optimize the balance of transparency, impact strength, and rigidity for applications requiring flexibility without the addition of nucleating agents.

[0056] The injection molded articles formed from the propylene polymer composition involved in this invention can greatly improve the impact strength of the molded articles obtained from the propylene polymer (A) alone. The impact strength is excellent, and the transparency and rigidity are hardly reduced. The balance between transparency, impact strength and rigidity is excellent.

[0057] <Method for manufacturing propylene-based polymer compositions>

[0058] Regarding the propylene polymer composition involved in this invention, the propylene polymer (A) and the ethylene-α-olefin copolymer (B) are mixed by dry mixing, Henschel mixer, Banbury mixer, etc., or by melt mixing after mixing using a single-screw extruder, twin-screw extruder, high-speed twin-screw extruder, etc., thereby obtaining the propylene polymer composition.

[0059] <Injection Molded Parts>

[0060] The injection-molded article of the present invention is a molded article formed by injection molding the propylene polymer composition involved in the present invention described above.

[0061] Manufacturing Method of Injection Molded Articles

[0062] Using a known injection molding machine, the propylene polymer composition involved in the present invention is heated and melted, injected into a mold, cooled and solidified, and then removed from the mold, thereby manufacturing the injection-molded article of the present invention.

[0063] More specifically, the process can be carried out as follows: A propylene polymer composition is fed into the hopper of an injection molding machine; the propylene polymer composition is then fed into a barrel heated to approximately 200°C–250°C for mixing and plasticizing until it reaches a molten state. This molten composition is then expelled from the nozzle at high pressure and high speed (maximum pressure 700–1500 kg / cm²). 3 The propylene polymer composition is injected into a mold that is heated to 5–50°C, preferably 10–40°C, using cooling water or warm water and closed by a mold-closing device. The injected propylene polymer composition is cooled and solidified by cooling from the mold, and the mold is opened using the mold-closing device to obtain the injection-molded body.

[0064] Alternatively, injection stretch blow molding can be performed, for example, as described below: a propylene-based polymer composition is fed into the hopper of an injection molding machine, and resin is fed into a barrel heated to approximately 200°C to 250°C, where it is mixed and plasticized to a molten state. This molten resin is then expelled from a nozzle at high pressure and high speed (maximum pressure 700–1500 kg / cm²). 3 Injection molding is performed in a mold that is heated to 5-80°C, preferably 10-60°C, using cooling water or warm water and closed by a mold clamping device. The mold is cooled for 1.0-3.0 seconds to form a preform. The mold is then immediately opened, and the mold is stretched and oriented longitudinally using a stretching rod. The mold is then stretched and oriented laterally by blow molding to obtain the injection molded body.

[0065] Applications of Injection Molded Parts

[0066] The injection-molded articles of the present invention can be used in various applications, including food containers, beverage containers, shipping containers, and daily necessities. More specifically, they can be widely used as solid food containers (dessert cups) for jelly, pudding, yogurt, etc., pharmaceutical containers, and industrial liquid containers.

[0067] As a dessert cup, the wall thickness of the main body of the container (the thinnest part) is preferably in the range of 0.3 to 2.0 mm. Even with such a thin wall, the acrylic resin composition of the present invention has sufficient impact strength and will not break or fragment during the manufacturing process.

[0068] Regarding the injection molded articles of the present invention, these articles also exhibit an excellent balance between impact resistance, transparency, and rigidity.

[0069] Example

[0070] The present invention will now be described in more detail based on embodiments. However, the present invention is not limited to these embodiments.

[0071] The following shows the polymers, etc., used in the examples and comparative examples.

[0072] (1) Propylene polymers (A)

[0073] As propylene polymer (A), the following propylene polymer is used.

[0074] (1-1) Propylene polymers (A-1)

[0075] Using MFR 230 = 15g / 10min propylene homopolymer: manufactured by Prime Polypro Co., Ltd., trade name Prime Polypro J106MG.

[0076] (2) Ethylene-α-olefin copolymer (B)

[0077] The following ethylene-α-olefin copolymer is used as ethylene-α-olefin copolymer (B).

[0078] (2-1) Ethylene-1-hexene copolymer (B-1)

[0079] Using MFR 190 =3.8g / 10min, density =903kg / m³ 3 Ethylene-1-hexene copolymer (B-1): manufactured by Praman Polymer Co., Ltd., trade name EVOLUE SP0540.

[0080] (2-2) Ethylene-1-hexene copolymer (B-2)

[0081] Using MFR 190 =3.8g / 10 minutes, density =918kg / m³ 3 Ethylene-1-hexene copolymer (B-2): manufactured by Praman Polymer Co., Ltd., trade name EVOLUE SP2040.

[0082] (2-3) Ethylene-1-hexene copolymer (B-3)

[0083] Using MFR 190 =1g / 10 minutes, density =915kg / m³ 3 Ethylene-1-hexene copolymer (B-3): manufactured by Praman Polymer Co., Ltd., trade name EVOLUE SP0510.

[0084] (2-4) Ethylene-1-hexene copolymer (B-4)

[0085] Using MFR 190 =2g / 10 minutes, density =913kg / m³ 3 Ethylene-1-hexene copolymer (B-4): manufactured by Praman Polymer Co., Ltd., trade name EVOLUE SP1520.

[0086] (2-5) Ethylene-1-hexene copolymer (B-5)

[0087] Using MFR 190 =10g / 10min, density =911kg / m³ 3 Ethylene-1-hexene copolymer (B-5): manufactured by Praman Polymer Co., Ltd., trade name EVOLUE SP1071C.

[0088] (3) Ethylene-α-olefin copolymer (C)

[0089] The following ethylene-α-olefin copolymers are used as ethylene-α-olefin copolymers.

[0090] (3-1) Ethylene-α-olefin copolymer (C-1)

[0091] Using MFR 190 =1.5g / 10min, density =862kg / m³ 3 Ethylene-propylene copolymer (C-1): Manufactured by ExxonMobil, trade name VISTAMAXX 6102FL.

[0092] (3-2) Ethylene-α-olefin copolymer (C-2)

[0093] Using MFR 190 =4g / 10 minutes, density =879kg / m³ 3 Ethylene-propylene copolymer (C-2): Manufactured by ExxonMobil, trade name VISTAMAXX 3980FL.

[0094] The physical properties of the injection-molded articles obtained in the examples and comparative examples were determined according to the following methods.

[0095] (1) Transparency

[0096] For the central portion of the injection-molded part, the haze was measured according to JIS K7136. The total haze is the sum of the internal haze and the external haze.

[0097] (2) High-speed surface impact test (high-speed impact)

[0098] Using an injection-molded body formed from a 200mm × 200mm × 2.0mm flat plate, the test piece for measurement was placed in an opening with an inner diameter. On the support platform of the hole, use the inner diameter After the sample plate is fixed, the diameter of the impact surface with a hemispherical shape is used. A hammer was used to strike the test piece at an impact velocity of 1 m / s, and the puncture energy (J) was calculated according to JIS K7211-2. The average value of the puncture energies of the four test pieces was taken as the surface impact strength (high-speed impact).

[0099] (3) Rigid

[0100] The tensile modulus of elasticity of dumbbell test pieces was determined according to JIS K7161 and K7162-1.

[0101] [Example 1]

[0102] For the propylene polymer composition obtained by mixing 90% by mass of the above-mentioned propylene polymer (A-1) and 10% by mass of the above-mentioned ethylene-1-hexene copolymer (B-1), injection molded bodies for high-speed surface impact testing and transparency (haze) measurement, formed from a 200mm×200mm×2.0mm flat plate, are produced using an injection molding machine (FANUC ROBOSHOT α100C manufactured by FANUC Corporation) under the conditions of melt resin temperature 200°C, mold temperature 40°C, average injection speed 35mm / s, holding pressure time 10 seconds, and total cycle time 45 seconds.

[0103] The physical properties of the obtained injection-molded articles were determined according to the methods described above.

[0104] The results are shown in Table 1.

[0105] [Examples 2-11]

[0106] The propylene polymer composition described in Table 1 (A-1) and the ethylene-1-hexene copolymer (B-1) were used instead of the propylene polymer composition used in Example 1. Otherwise, the same procedure as in Example 1 was followed to produce the injection molded body.

[0107] The physical properties of the obtained injection-molded articles were determined according to the methods described above.

[0108] The results are shown in Table 1.

[0109] [Comparative Example 1]

[0110] The same procedure as in Example 1 was followed to produce injection-molded articles, except that a propylene polymer (A-1) was used alone instead of the propylene polymer composition used in Example 1.

[0111] The physical properties of the obtained injection-molded articles were determined according to the methods described above.

[0112] The results are shown in Table 2.

[0113] [Comparative Examples 2-8]

[0114] The propylene polymer composition described in Table 2 (A-1) and the propylene polymer composition of the ethylene-α-olefin copolymer (C-1) were used instead of the propylene polymer composition used in Example 1. Otherwise, the same procedure as in Example 1 was followed to produce the injection molded body.

[0115] The physical properties of the obtained injection-molded articles were determined according to the methods described above.

[0116] The results are shown in Table 2.

[0117] [Table 1]

[0118]

[0119] [Table 2]

[0120]

[0121] As shown in Tables 1 and 2, the injection molded articles obtained in Examples 1 to 11 exhibited better haze compared to the injection molded article obtained in Comparative Example 1, which was formed solely from propylene polymer (A). Furthermore, the impact strength at 23°C, 0°C, and -20°C was improved.

[0122] On the other hand, the samples obtained in Comparative Examples 2-5 contained a density of 862 kg / m³ 3 The haze of the injection-molded parts formed from the propylene polymer composition of the ethylene-α-olefin copolymer deteriorated, and the impact strength at -20°C did not improve.

[0123] In addition, the samples obtained in Comparative Examples 6-8 contained a density of 879 kg / m³ 3 Although the haze of the injection-molded parts formed from the propylene polymer composition of the ethylene-α-olefin copolymer did not deteriorate, the impact strength at 0°C and the impact strength at -20°C did not improve.

Claims

1. An injection-molded article, characterized in that: The composition is formed from a propylene-based polymer composition consisting solely of: 60–90% by mass of a propylene-based polymer (A) satisfying conditions (a–i) and (a–ii) below; 10–40% by mass of an ethylene-α-olefin copolymer (B) satisfying conditions (b–i), (b–ii) and (b–iii) below; and additives and / or colorants as desired, wherein the total amount of (A) and (B) is set to 100% by mass, and the additives are selected from at least one of neutralizing agents, weathering agents, lubricants, antistatic agents, antiblocking agents, antifogging agents, dispersants, flame retardants, antibacterial agents, and fluorescent whitening agents. The propylene-based polymer composition is free of nucleating agents, has a melt flow rate MFR measured according to JIS K6921 at a temperature of 230 °C, a load of 2.16 kg 230 in the range of 5 to 50 g / 10 min, Conditions (a-i): The melt flow rate, measured according to JIS K6921 at a temperature of 230°C and a load of 2.16 kg, is in the range of 1 to 50 g / 10 minutes; Condition (a-ii): The content of α-olefins other than propylene, as determined by infrared spectroscopy, is less than 1% by mass, including 0% by mass; Condition (b-i): The melt flow rate, measured according to JIS K6921 at a temperature of 190℃ and a load of 2.16kg, is in the range of 2 to 15 g / 10 minutes; Condition (b-ii): density in the range of 903 to 915 kg / m3measured according to JIS K6922 3 ; Conditions (b-iii): The content of structural units derived from ethylene is in the range of 83-90 mol%.

2. The injection-molded article as described in claim 1, characterized in that: The propylene polymer (A) is a propylene homopolymer.

3. The injection-molded article as described in claim 1, characterized in that: The α-olefin of the ethylene-α-olefin copolymer (B) is 1-hexene.

4. The injection-molded article as described in claim 1, characterized in that: The melt flow rate under condition (b-i) is in the range of 2 to 5 g / 10 minutes.

5. The injection-molded article as described in claim 1, characterized in that: The additive is selected from at least one of neutralizing agents, weathering agents, antistatic agents, anti-blocking agents, anti-fogging agents, flame retardants, and fluorescent whitening agents.

6. The injection-molded article as described in claim 1 or 5, characterized in that: The weathering agent is selected from at least one of antioxidants, heat stabilizers, and ultraviolet absorbers.

7. The injection-molded article as described in claim 1, characterized in that: The injection molded part can be either a container or a daily necessity.

8. The injection-molded article as described in claim 1, characterized in that: Injection molded parts are used to make food containers.

9. The injection-molded article as described in claim 1, characterized in that: Injection molded parts are used for beverage containers.

Citation Information

Patent Citations

  • Propylene-based resin composition, moldings, and container

    WO2010074001A1

  • Polypropylene resin composition and polypropylene film obtained from the same

    JP1998077373A

  • Propylenic resin composition and its molded article

    JP2008255326A

  • Propylene-based resin composition and its molded article

    JP2009120800A

  • Olefin resin composition, sheet, and thermoformed body

    JP2012158703A