Slurry for ceramic copper-clad parts, ceramic copper-clad parts, and preparation method and application thereof

By using a specially configured complexing agent in the slurry of ceramic copper-clad parts to form a three-dimensional network structure, the existing problems of complex copper coating methods and high costs for ceramic substrates are solved, and ceramic copper coating with high peel strength and low resistance is achieved. Parts are prepared for a variety of applications.

CN117326886BActive Publication Date: 2024-10-29BYD CO LTD
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202210731114.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-24
Publication Date
2024-10-29
Estimated Expiration
2042-06-24

AI Technical Summary

Technical Problem

Existing copper coating methods for ceramic substrates, such as DBC and copper plating, have problems such as numerous processes, complex operations, high equipment requirements and high cost, making it difficult to prepare high-efficiency, low-resistance ceramic copper-clad parts.

Method used

Provides a slurry for ceramic copper-clad parts, which contains copper powder, solvent, adhesive, sintering aid and complexing agent. It forms a three-dimensional network structure through a specific complexing agent configuration, improves the three-dimensional sense of the slurry, and Through drying and sintering under vacuum or inert atmosphere, high thickness screen printing and high bonding force are achieved to prepare ceramic copper-clad parts with high peel strength and low resistance.

Benefits of technology

It achieves high-thickness screen printing and high bonding force of ceramic copper-clad parts, and obtains ceramic copper-clad parts with high peel strength and low resistivity, which are suitable for applications such as refrigeration chips and current-carrying plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003713525370000081
    Figure BDA0003713525370000081
Patent Text Reader

Abstract

The present application provides a slurry for a ceramic copper-clad part, which comprises, by mass, 75-88 parts of copper powder, 5-18 parts of solvent, 0.05-1 parts of adhesive, 5-15 parts of sintering aid, and 0.05-1 parts of complexing agent; the complexing agent comprises hydrogenated castor oil and / or polyamide wax. The present application adopts a specific complexing agent to be configured in the slurry, and forms a three-dimensional network structure in the slurry, thereby improving the three-dimensional sense of the slurry, so that the slurry can be screen-printed on a ceramic substrate with high thickness, and the ratio of each substance is controlled, thereby improving the bonding force between the copper layer and the ceramic substrate, and obtaining a ceramic copper-clad part with high peel strength and low resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of substrate process technology, and in particular to a slurry for a ceramic copper-clad component, a ceramic copper-clad component, and a preparation method and application thereof. Background Art

[0002] The mainstream copper-clad ceramic substrates currently use DBC and copper plating methods. DBC (Direct Bonding Copper) ceramic copper-clad boards refer to composite boards in which copper foil is directly bonded to the surface of a ceramic substrate at high temperature. The preparation process is usually to first oxidize the copper foil to form a copper oxide layer, then bond the copper oxide layer of the copper foil to the ceramic substrate, and then sinter at high temperature to achieve the bonding of the copper foil and the ceramic substrate. The copper plating method refers to depositing a uniform conductive layer on the hole wall through an oxidation-reduction reaction, and then thickening the copper plating through electroplating to achieve the required plating layer. The DBC method has many processes, cumbersome operation, high equipment requirements and relatively high costs. Summary of the invention

[0003] The purpose of the present application is to overcome the problems existing in the above-mentioned prior art and to provide a slurry for ceramic copper-clad parts, ceramic copper-clad parts and their preparation method and application.

[0004] The first aspect of the present application is to provide a slurry for ceramic copper-clad parts, which comprises, by mass, 75-88 parts of copper powder, 5-18 parts of solvent, 0.05-1 part of adhesive, 5-15 parts of sintering aid, and 0.05-1 part of complexing agent; the complexing agent comprises hydrogenated castor oil and / or polyamide wax.

[0005] Preferably, the slurry for the ceramic copper-clad part comprises, by weight: 80-85 parts of copper powder, 8-15 parts of solvent, 0.3-0.8 parts of binder, 8-12 parts of sintering aid, and 0.05-1 parts of complexing agent.

[0006] Preferably, the mass ratio of the copper powder to the sintering aid is 8-12.

[0007] Preferably, the sintering aid includes one or more of silicon dioxide, calcium carbonate, aluminum oxide, sodium oxide, cobalt oxide and barium sulfate.

[0008] Preferably, the solvent includes one or more of ethylene glycol, ethanol, xylene, terpineol and glycerol.

[0009] Preferably, the binder comprises one or more of polyvinyl butyral, cellulose and dioctyl phthalate.

[0010] The second aspect of the present application is to provide a method for preparing a ceramic copper-clad component, comprising: coating the aforementioned slurry for the ceramic copper-clad component on the surface of a ceramic substrate; and then drying and sintering to obtain the ceramic copper-clad component.

[0011] Preferably, the sintering is performed in a vacuum environment or an inert atmosphere, and the sintering temperature is 600-1200°C.

[0012] Preferably, the material of the ceramic substrate includes one or more of zirconium oxide, aluminum oxide, aluminum nitride, silicon carbide, silicon oxide, zirconium nitride and zirconium carbide.

[0013] The third aspect of the present application is to provide a ceramic copper-clad component, which is prepared by the aforementioned method for preparing the ceramic copper-clad component.

[0014] The present application adopts a specific complexing agent to be configured in the slurry to form a three-dimensional network structure in the slurry, thereby improving the three-dimensional sense of the slurry. The fourth aspect of the present application is to provide an application of a ceramic copper-clad component, which includes: using the aforementioned ceramic copper-clad component to prepare a cooling plate or a current-carrying plate.

[0015] The slurry can be screen-printed on the ceramic substrate to achieve high thickness, and the ratio of each substance can be controlled, thereby improving the bonding force between the copper layer and the ceramic substrate, and obtaining a ceramic copper-clad part with high peel strength and low resistance. DETAILED DESCRIPTION

[0016] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0017] The present application provides a slurry for ceramic copper-clad parts, which comprises, by mass, 75-88 parts of copper powder, 5-18 parts of solvent, 0.05-1 part of adhesive, 5-15 parts of sintering aid, and 0.05-1 part of complexing agent; the complexing agent comprises hydrogenated castor oil and / or polyamide wax.

[0018] The present application adopts a specific complexing agent to be configured in the slurry to form a three-dimensional network structure in the slurry, thereby improving the three-dimensional sense of the slurry, enabling the slurry to be screen-printed on a ceramic substrate to achieve high thickness, and controlling the ratio of each substance, thereby improving the bonding strength between the copper layer and the ceramic substrate, and obtaining a ceramic copper-clad part with high peel strength and low resistivity.

[0019] Specifically, in the embodiment of the present application, the mass fraction of copper powder ranges from 75 to 88 parts. Within this range, the mass fraction of copper powder can play a role in low resistivity conduction and better improve the bonding force between the copper layer and the ceramic substrate. If the mass fraction of copper powder is less than 75 parts, the resistance of the ceramic copper-clad part is too high, affecting the conductive conduction effect; if the mass fraction of copper powder is greater than 88 parts, the strength of the copper layer is low and the bonding force with the ceramic substrate is poor. Preferably, the mass fraction of copper powder ranges from 80 to 85 parts.

[0020] In some embodiments, the copper powder may be pure copper powder, copper alloy powder, or a mixture of pure copper and copper alloy. The copper powder may have a particle size ranging from 0.5 to 100 μm, which can play a good role in dispersion and facilitate sintering.

[0021] In the embodiment of the present application, the mass fraction of the sintering aid is in the range of 5-15 parts. When the mass fraction of the sintering aid is within this range, the strength of the copper layer and the bonding force between the copper layer and the ceramic substrate can be enhanced. If the mass fraction of the sintering aid is less than 5 parts, the strength of the copper layer is poor and the bonding force with the ceramic substrate is poor; if the mass fraction of the sintering aid is greater than 15 parts, the resistance of the copper layer is too large. Preferably, the mass fraction of the sintering aid is in the range of 8-12 parts.

[0022] In some embodiments, in order to further improve the bonding strength between the copper layer and the ceramic substrate, the mass ratio of the copper powder to the sintering aid may be adjusted within a range of 8-12.

[0023] In some embodiments, the sintering aid includes one or more of silicon dioxide, calcium carbonate, aluminum oxide, sodium oxide, cobalt oxide and barium sulfate, which can better enhance the bonding force between the copper layer and the ceramic substrate.

[0024] In the embodiment of the present application, the mass fraction of the solvent ranges from 5 to 18 parts. When the mass fraction of the solvent is within this range, the slurry can be well mixed and well formed. If the mass fraction of the solvent is less than 5 parts, the slurry is unevenly mixed and has poor formability; if the mass fraction of the solvent is greater than 18 parts, the slurry has poor formability. Preferably, the mass fraction of the solvent ranges from 8 to 15 parts.

[0025] In some embodiments, the solvent includes one or more of ethylene glycol, ethanol, xylene, terpineol, and glycerol.

[0026] In the embodiment of the present application, the mass fraction of the adhesive ranges from 0.05 to 1 part. Within this range, the mass fraction of the adhesive promotes the forming strength of the copper layer screen printing and the shape retention during the sintering process. If the mass fraction of the adhesive is less than 0.05 parts, the effect is not obvious and the strength difference of the copper layer after screen printing is easily lost; if the mass fraction of the adhesive is greater than 1 part, the sintering effect of the copper layer is affected. Preferably, the mass fraction of the adhesive ranges from 0.3 to 0.8 parts.

[0027] In some embodiments, the binder includes one or more of polyvinyl butyral (PVB), cellulose, and dioctyl phthalate (DOP).

[0028] In the embodiment of the present application, the mass fraction of the complexing agent ranges from 0.05 to 1 part. When the mass fraction of the complexing agent is within this range, a specific complexing agent is used to configure the slurry to form a three-dimensional network structure in the slurry, thereby improving the three-dimensional sense of the slurry, so that the slurry can be screen-printed on a ceramic substrate with high thickness. If the mass fraction of the complexing agent is less than 0.05 parts, the slurry has a poor three-dimensional sense and low thickness; if the mass fraction of the complexing agent is greater than 1 part, the slurry viscosity is too large to affect the screen printing. The complexing agent includes hydrogenated castor oil and / or polyamide wax.

[0029] The present application also provides a method for preparing a ceramic copper-clad component, comprising: coating the aforementioned slurry for the ceramic copper-clad component on the surface of a ceramic substrate; and then drying and sintering to obtain the ceramic copper-clad component.

[0030] In some embodiments, the slurry for the ceramic copper-clad part can be coated on the surface of the ceramic substrate in the form of: the prepared slurry is screen-printed on the surface of the ceramic substrate with a preset pattern or circuit through a screen. Then the slurry is dried to form. Specifically, it can be placed in a drying oven at 50-200°C to evaporate the organic solvent and pre-form.

[0031] In some embodiments, the sintering is performed in a vacuum environment or an inert atmosphere, which can effectively protect copper and its alloys from oxidation. The inert atmosphere can be a nitrogen atmosphere. Preferably, the sintering temperature is 600-1200° C. and the sintering time is 1-10 h.

[0032] In some embodiments, the material of the ceramic substrate includes one or more of zirconium oxide, aluminum oxide, aluminum nitride, silicon carbide, silicon oxide, zirconium nitride and zirconium carbide.

[0033] The present application also provides a ceramic copper-clad component, which is prepared by the above-mentioned method for preparing a ceramic copper-clad component. The ceramic copper-clad component has high peel strength and low resistance characteristics.

[0034] The present application also provides an application of a ceramic copper-clad component, which includes: using the aforementioned ceramic copper-clad component to prepare a cooling plate or a current-carrying plate. The cooling plate or the current-carrying plate can be used in the fields of automobiles, medical treatment, and daily electrical appliances. The present application will be described in detail below through examples, but the present application is not limited to the following examples.

[0035] Example 1

[0036] (1) Mix the slurry according to the following components, disperse it at 500r / min and disperse it for 2h:

[0037] Copper and copper alloy powder: 80 parts;

[0038] Solvent: terpineol, 10 parts;

[0039] Adhesive: PVB, 0.5 parts;

[0040] Sintering aid: silicon dioxide: sodium carbonate = 1:1, 9 parts in total;

[0041] Complexing agent: hydrogenated castor oil, 0.5 parts.

[0042] (2) The prepared slurry is used to screen print the preset circuit on the zirconia ceramic substrate through a screen plate.

[0043] (3) The ceramic substrate with the silk-screened circuit was dried at 100° C. and then vacuum sintered at a temperature of 800° C. for 4 h to obtain a ceramic copper-clad component.

[0044] Example 2

[0045] Same as Example 1, except that the composition of the slurry is:

[0046] Copper and copper alloy powder: 85 parts;

[0047] Solvent: terpineol, 5 parts;

[0048] Adhesive: PVB, 0.5 parts;

[0049] Sintering aid: silicon dioxide: sodium carbonate = 1:1, 9 parts in total;

[0050] Complexing agent: hydrogenated castor oil, 0.5 parts.

[0051] Example 3

[0052] Same as Example 1, except that the composition of the slurry is:

[0053] Copper and copper alloy powder: 84 parts;

[0054] Solvent: terpineol, 10 parts;

[0055] Adhesive: PVB, 0.5 parts;

[0056] Sintering aid: silicon dioxide: sodium carbonate = 1:1, 5 parts in total

[0057] Complexing agent: hydrogenated castor oil, 0.5 parts

[0058] Example 4

[0059] Same as Example 1, except that the composition of the slurry is:

[0060] Copper and copper alloy powder: 88 parts;

[0061] Solvent: terpineol, 15 parts;

[0062] Adhesive: PVB, 0.5 parts;

[0063] Sintering aid: silicon dioxide: sodium carbonate = 1:1, a total of 11 parts;

[0064] Complexing agent: polyamide wax, 0.5 parts.

[0065] Example 5

[0066] Same as Example 1, except that the composition of the slurry is:

[0067] Copper and copper alloy powder: 80 parts;

[0068] Solvent: terpineol, 10 parts;

[0069] Adhesive: PVB, 0.5 parts;

[0070] Sintering aid: silicon dioxide: sodium carbonate = 1:1, 9 parts in total;

[0071] Complexing agent: hydrogenated castor oil and polyamide wax, 0.8 parts.

[0072] Comparative Example 1

[0073] Same as Example 1, except that the composition of the slurry is:

[0074] Copper and copper alloy powder: 65 parts;

[0075] Solvent: terpineol, 3 parts;

[0076] Adhesive: PVB, 0.5 parts;

[0077] Sintering aid: silicon dioxide: sodium carbonate = 1:1, 9 parts in total;

[0078] Complexing agent: hydrogenated castor oil, 0.5 parts.

[0079] Comparative Example 2

[0080] Same as Example 1, except that the composition of the slurry is:

[0081] Copper and copper alloy powder: 84 parts;

[0082] Solvent: terpineol, 10 parts;

[0083] Adhesive: PVB, 0.5 parts;

[0084] Sintering aid: silicon dioxide: sodium carbonate = 1:1, 4 parts in total;

[0085] Complexing agent: hydrogenated castor oil, 0.5 parts.

[0086] Comparative Example 3

[0087] Same as Example 1, except that the composition of the slurry is:

[0088] Copper and copper alloy powder: 80 parts;

[0089] Solvent: terpineol, 10 parts;

[0090] Adhesive: PVB, 0.5 parts;

[0091] Sintering aid: silicon dioxide: sodium carbonate = 1:1, 9 parts in total;

[0092] Complexing agent: sodium hexametaphosphate, 0.5 parts.

[0093] Comparative Example 4

[0094] Same as Example 1, except that the composition of the slurry is:

[0095] Copper and copper alloy powder: 80 parts;

[0096] Solvent: terpineol, 10 parts;

[0097] Adhesive: PVB, 0.5 parts;

[0098] Sintering aid: silicon dioxide: sodium carbonate = 1:1, 9 parts in total;

[0099] Complexing agent: hydrogenated castor oil, 2 parts.

[0100] Comparative Example 5

[0101] Same as Example 1, except that the composition of the slurry is:

[0102] Copper and copper alloy powder: 80 parts;

[0103] Solvent: terpineol, 10 parts;

[0104] Adhesive: PVB, 0.5 parts;

[0105] Sintering aid: silicon dioxide: sodium carbonate = 1:1, 9 parts in total.

[0106] Performance Testing:

[0107] The resistance of the sample was tested. The copper foil size of the resistance test sample was 3mm*1.2mm*0.3mm (the copper layer size of comparative example 5 was 3mm*1.2mm*0.01mm). A DC resistance tester model YP2512 was used.

[0108] Pull-out force test: The test was conducted using a TS2000M universal material testing machine.

[0109] Adhesion test: First use a grid knife to make a grid, then use 3M tape to stick to the test surface and roll it with a rubber roller. Then pull the tape at a constant speed in a 90° vertical direction. Test results: Good: no shedding or warping of the copper layer; Average: slight warping or partial peeling of the copper layer; Poor: all or most of the copper layer is shedding or warping.

[0110] Table 1

[0111]

[0112] It can be seen from the results in Table 1 that the slurry for the ceramic copper-clad parts of the present application can achieve high thickness of the slurry screen printing, and the copper layer thickness of the prepared ceramic copper-clad parts is greater than 100 μm; and low resistance, less than 7 mΩ, the ceramic copper-clad parts have good thermal conductivity; and the copper layer has high bonding strength with the ceramic substrate. However, the ceramic copper-clad parts prepared in Comparative Examples 1-5 cannot meet the above requirements at the same time.

[0113] The preferred embodiments of the present application are described in detail above; however, the present application is not limited to the specific details in the above embodiments. Within the technical concept of the present application, a variety of simple modifications can be made to the technical solution of the present application, and these simple modifications all fall within the protection scope of the present application.

[0114] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, this application will not further describe various possible combinations.

[0115] In addition, the various implementation modes of the present application may be arbitrarily combined, and as long as they do not violate the concept of the present application, they should also be regarded as the contents disclosed in the present application.

Claims

1. A slurry for ceramic copper-clad parts, characterized in that: Calculated by mass, including: 75-88 parts of copper powder, 5-18 parts of solvent, 0.05-1 parts of binder, 5-15 parts of sintering aid, 0.05-1 parts of complexing agent; the complexing agent includes hydrogenated castor oil and / or polyamide wax; The sintering aid includes one or more of silicon dioxide, calcium carbonate, aluminum oxide, sodium oxide, cobalt oxide and barium sulfate; the solvent includes one or more of ethylene glycol, ethanol, xylene, terpineol and glycerol; the binder includes one or more of polyvinyl butyral, cellulose and dioctyl phthalate.

2. The slurry for ceramic copper-clad parts according to claim 1, characterized in that: Calculated by weight, the composition comprises: 80-85 parts of copper powder, 8-15 parts of solvent, 0.3-0.8 parts of binder, 8-12 parts of sintering aid, and 0.05-1 parts of complexing agent.

3. The slurry for ceramic copper-clad parts according to claim 1, characterized in that: The mass ratio of the copper powder to the sintering aid is 8-12.

4. A method for preparing a ceramic copper-clad part, characterized in that: include: The slurry for the ceramic copper-clad component according to any one of claims 1 to 3 is coated on the surface of a ceramic substrate; and then dried and sintered to obtain the ceramic copper-clad component.

5. The method for preparing a ceramic copper-clad part according to claim 4, characterized in that: The sintering is performed in a vacuum environment or an inert atmosphere, and the sintering temperature is 600-1200°C.

6. The method for preparing a ceramic copper-clad part according to claim 4, characterized in that: The material of the ceramic substrate includes one or more of zirconium oxide, aluminum oxide, aluminum nitride, silicon carbide, silicon oxide, zirconium nitride and zirconium carbide.

7. A ceramic copper-clad part, characterized in that: The ceramic copper-clad part is prepared by the preparation method of any one of claims 4 to 6.

8. An application of a ceramic copper-clad part, the application comprising: The ceramic copper-clad component according to claim 7 is used to prepare a cooling plate or a current-carrying plate.

Citation Information

Patent Citations

  • Preparation method of ceramic substrate for high-power LED packaging

    CN102432346A

  • Conductive paste for thick film circuit, thick film circuit board employing same and manufacturing method thereof

    CN102760934A

  • Copper electronic paste and preparation method and application thereof

    CN103559940A

  • Method for preparing copper / ceramic composite substrate on basis of low-melting-point glass powder

    CN105439643A

  • Electroless plating solution, preparation method and nonmetal electroless plating method

    CN106637159A