An intrinsically flame-retardant polydicyclopentadiene containing a dinorbornene flame-retardant monomer and its preparation method
By copolymerizing a bisnorbornene flame retardant containing a phenyl phosphate structure with dicyclopentadiene to form a multi-linked network, the flammability problem of polydicyclopentadiene is solved, achieving high-efficiency flame retardancy and improved mechanical properties.
Patent Information
- Application Number
- CN202311233680.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-22
AI Technical Summary
Polydicyclopentadiene is flammable, and when it burns, it drips and produces smoke and toxic gases. Furthermore, adding traditional flame retardants can impair its mechanical properties.
A bisnorbornene flame retardant containing a phenyl phosphate structure is copolymerized with dicyclopentadiene and (Z)-cyclooctyl-4-en-1-carboxylic acid via thermally driven self-propagating technology to form a multi-linked network. During combustion, the flame retardant generates phosphorus-containing free radicals that capture active free radicals, promoting carbonization and forming a dense char layer.
The polydicyclopentadiene material achieved a UL-94V-0 flame retardant rating, a tensile strength of 146MPa, an elongation at break of 79%, an impact strength of 121kJ/m², and a glass transition temperature of 219℃, while maintaining excellent mechanical and flame retardant properties.
Smart Images

Figure CN117327113B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials and engineering technology, specifically relating to a multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate structure bisnorbornene flame-retardant monomer, and also relating to a bisnorbornene-based flame retardant containing a phenyl phosphate structure. Background Technology
[0002] Polydicyclopentadiene is an important cross-linked polymer in industry, possessing high modulus, high impact strength, and chemical resistance. Its monomer, dicyclopentadiene, has advantages such as rapid reaction, low viscosity, and minimal post-processing, making it widely used in industry for the simple and rapid fabrication of large, complex structural components. However, as a fully carbon-chain polymer, polydicyclopentadiene is extremely flammable, dripping easily during combustion and producing large amounts of smoke and toxic gases, limiting its application in complex environments. Although the addition of additive flame retardants gives the composite material a better flame-retardant effect, its mechanical properties are significantly reduced.
[0003] To improve the flame retardant properties of polydicyclopentadiene while maintaining its high mechanical properties, researchers both domestically and internationally have conducted a series of studies. In patent CN104327205 A, researchers incorporated halogen-containing flame retardants into polydicyclopentadiene composites. However, the improvement in flame retardant performance was not significant, with a maximum LOI value of only 28.8%. Furthermore, the hydrogen halides and organohalides produced by using halogen flame retardants are not only toxic and corrosive, seriously threatening human life and property, but also damaging the ozone layer, placing enormous pressure on environmental protection and ecological construction. In patent CN105085984 A, researchers synthesized a halogen-free flame retardant and compounded it with polyamide to prepare a flame-retardant polymer material. This material exhibits excellent flame retardant properties, but its tensile and flexural properties are lower than those of the material without added flame retardant. In patent CN116396468 A, researchers provided a class of expandable norbornene-based flame retardants containing phenylphosphonic and piperazine structures. This flame retardant, copolymerized with dicyclopentadiene and 1,5-dimethyl-1,5-cyclooctadiene monomers, yields polydicyclopentadiene engineering materials. These materials exhibit excellent flame retardant properties, with a limiting oxygen index of 43%, a flame retardancy rating of UL-94V-0, a tensile strength of 131 MPa, an elongation at break of 48%, and an impact strength of 108 kJ / m². 2The heat distortion temperature reaches 199℃. However, the monomer copolymerized with DCPD in this patent has a mononorbornene structure. The introduction of this monomer leads to a decrease in the overall crosslinking density of the polydicyclopentadiene material, resulting in a reduction in the material's mechanical properties, fatigue resistance, and thermal stability. Furthermore, a single crosslinking network does not significantly improve the material's heat resistance. Therefore, in recent years, developing efficient and environmentally friendly flame retardants that can significantly improve the mechanical properties of materials has become a major trend in the field of flame retardant research.
[0004] This invention provides a class of bisnorbornene-based flame retardants containing a phenyl phosphate structure. These flame retardants can be copolymerized with dicyclopentadiene and (Z)-cyclooctyl-4-en-1-carboxylic acid monomers via thermally driven self-propagating technology. Simultaneously, this invention provides a multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-based bisnorbornene flame-retardant monomer. This material exhibits excellent flame retardant properties, strength, toughness, creep resistance, fatigue resistance, and glass transition temperature. Its limiting oxygen index reaches 43%, its flame retardant rating reaches UL-94V-0, its tensile strength reaches 146 MPa, its elongation at break reaches 79%, and its impact strength reaches 121 kJ / m². 2 The glass transition temperature reaches 219℃. Summary of the Invention
[0005] One objective of this invention is to provide a multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer.
[0006] The second objective of this invention is to provide a bisnorbornene flame retardant containing a phenyl phosphate structure, which solves the current problem of the flammability of polydicyclopentadiene and provides a novel, highly efficient, and environmentally friendly intrinsic flame retardant.
[0007] This invention further provides a preparation method in which the prepared bisnorbornene flame retardant containing a phenyl phosphate structure can be copolymerized with dicyclopentadiene and (Z)-cyclooctyl-4-en-1-carboxylic acid monomers via thermally driven self-propagating technology. This ultimately yields a multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate structure bisnorbornene flame retardant monomer. This material has a limiting oxygen index of 43%, a flame retardancy rating of UL-94V-0, a tensile strength of 146 MPa, an elongation at break of 79%, and an impact strength of 121 kJ / m². 2 With a glass transition temperature of 219℃, it possesses excellent flame retardant properties, mechanical properties, creep resistance, and fatigue resistance, enabling the material to be applied in a variety of complex scenarios.
[0008] The specific plan is as follows:
[0009] This invention provides a bisnorbornene-based flame retardant containing a phenyl phosphate structure, wherein the bisnorbornene-based flame retardant containing a phenyl phosphate structure has the structure shown in formula (1):
[0010]
[0011] In formula (1), R1 and R2 are each an aliphatic substituent with 1-8 carbon atoms or an aromatic substituent with 6-12 carbon atoms.
[0012] This invention also provides a method for preparing the aforementioned bisnorbornene-based flame retardant containing a phenyl phosphate structure, the method comprising:
[0013] Norbornene containing a monoamine and a dicarboxylic acid containing a phenyl phosphate structure undergo a condensation acylation reaction in an organic solvent under the action of a catalyst. First, under stirring conditions at 0℃~5℃, the catalyst is added in proportion to a solution containing a monoamine and an organic solvent to obtain a mixed solution. Then, the dicarboxylic acid containing a phenyl phosphate structure is added dropwise to the above mixed solution. Then, under stirring conditions at 20℃~70℃, the reaction is carried out for 2~40 hours. After the reaction is completed, the product is washed, filtered and dried, and finally enriched to obtain the bisnorbornene flame retardant containing a phenyl phosphate structure.
[0014] The catalyst is one or a mixture of several of the following: triethylamine, N,N-diisopropylethylamine, pyridine, sodium acetate, 4-N,N-dimethylpyridine, 4-dimethylaminopyridine, 1-hydroxybenzotriazole, dicyclohexylcarbodiimide, diisopropylcarbodiimide, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide.
[0015] The organic solvent is at least one of the following: tetrahydrofuran, dichloromethane, chloroform, N,N-dimethylformamide, acetonitrile, acetone, benzene, and toluene.
[0016] The molar ratio of the catalyst to norbornene containing a monoamine is 1:1, while the molar ratio of the catalyst, the dicarboxylic acid containing a phenyl phosphate structure, and norbornene containing a monoamine is 2.05:1:2.05 to 2.15:1:2.15.
[0017] The present invention also provides the use of a bisnorbornene flame retardant containing a phenyl phosphate structure as a raw material, wherein the bisnorbornene flame retardant containing a phenyl phosphate structure is copolymerized with dicyclopentadiene and (Z)-cyclooct-4-en-1-carboxylic acid monomers via thermally driven self-propagating technology to obtain the polydicyclopentadiene engineering material.
[0018] This invention also provides a multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-based dinorbornene flame-retardant monomer. The raw materials for preparing the polydicyclopentadiene engineering material include: dicyclopentadiene, (Z)-cyclooctyl-4-en-1-carboxylic acid, and the phenyl phosphate-based dinorbornene flame retardant. The polydicyclopentadiene engineering material includes the structure shown in formula (2).
[0019]
[0020] In equation (2), m, n, p, and q are all independent integers between 50 and 1500; R1 and R2 in equation (2) are the same as R1 and R2 in equation (1).
[0021] Furthermore, the mass percentage of the raw material is:
[0022] Dicyclopentadiene 49.40 wt%–79.70 wt%
[0023] Binorbornene flame retardant containing phenyl phosphate structure, 10.00 wt%–40.00 wt%.
[0024] (Z)-Cyclooct-4-ene-1-carboxylic acid 10.00 wt%
[0025] This invention also provides a method for preparing the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured bisnorbornene flame-retardant monomer, wherein the total mass percentage of each raw material used to prepare the polydicyclopentadiene engineering material is 100 wt%, characterized in that the mass percentage of each raw material is:
[0026]
[0027] The ruthenium-based catalyst is a second-generation Grubbs catalyst;
[0028] The inhibitor is a phosphate ester;
[0029] The preparation method of the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer includes:
[0030] (1) Disperse the bisnorbornene flame retardant containing phenyl phosphate structure into a mixture containing dicyclopentadiene, (Z)-cyclooct-4-en-1-carboxylic acid, Grubbs second-generation catalyst and inhibitor in proportion, and ultrasonically mix under ice-water bath conditions to obtain a dispersion.
[0031] (2) The dispersion is injected into the mold and local thermal initiation is carried out under heating conditions. Through its own thermal-driven self-propagating polymerization, the multi-crosslinked intrinsic flame-retardant polydicyclopentadiene engineering material containing the phenyl phosphate structure dinorbornene flame-retardant monomer is copolymerized to obtain the multi-crosslinked intrinsic flame-retardant polydicyclopentadiene engineering material.
[0032] This invention also provides an application of a multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer, characterized in that: the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer is used in rocket shells, missile tail fins, vehicle tracks, or engine cover components.
[0033] The present invention has the following beneficial effects:
[0034] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0035] (1) This invention provides a class of dinorbornene-based flame retardant monomers containing phenyl phosphate structures. During the combustion of polydicyclopentadiene materials, the flame retardant pyrolyzes to generate phosphorus-containing free radicals (PO·, PO2·, and HPO2·), which capture active H· and OH· free radicals and inhibit the combustion reaction. At the same time, the phosphoric acid, polyphosphoric acid, and polyphosphoric acid generated by the pyrolysis of the material can promote the dehydration and carbonization of the matrix, forming a dense and phosphorus-rich carbon layer. Furthermore, the dinorbornene structure in the flame retardant increases the crosslinking density of the material, which can effectively reduce the fluidity of the high-temperature melt during combustion, reduce the generation of molten droplets, and retard flame propagation while improving the mechanical properties of the material. In addition, the presence of a large number of benzene ring structures in the matrix can enable the material to form a graphitized carbon layer during combustion. Combined with the char-forming effect of the comonomer (Z)-cyclooctyl-4-ene-1-carboxylic acid, the overall density of the carbon layer is improved, ultimately achieving the intrinsic flame retardancy of polydicyclopentadiene.
[0036] (2) This invention provides a class of dinorbornene-based flame retardant monomers containing a phenyl phosphate structure, which are copolymerized with dicyclopentadiene and (Z)-cyclooctyl-4-en-1-carboxylic acid. The introduction of the dinorbornene structure endows the material with a high chemical crosslinking density. In addition, the introduction of a large number of benzene rings and functional groups with large polarity differences can introduce hydrogen bonds and π-π stacking interactions into the system, further constructing a dynamic physical crosslinking network. The multiple chemical and physical crosslinking networks play a role in strengthening and toughening, improving the mechanical properties of the material while ensuring excellent flame retardant properties. Furthermore, the multiple chemical and physical crosslinking network structure can effectively prevent molecular chain slippage, playing a role in creep resistance and fatigue resistance.
[0037] (3) Compared with the traditional reaction injection molding curing process, the polymerization process of the multi-crosslinked intrinsic flame-retardant polydicyclopentadiene engineering material containing phenyl phosphate structure dinorbornene flame-retardant monomer in this invention is simple and does not require secondary curing, and the industrialization process is simple. Attached Figure Description
[0038] Figure 1 A bisnorbornene flame retardant A containing a phenyl phosphate structure 1 H-NMR spectrum
[0039] Figure 2 A bisnorbornene flame retardant B containing a phenyl phosphate structure 1 H-NMR spectrum
[0040] Figure 3 C is a mononorbornene flame retardant containing a phenyl phosphate structure. 1 H-NMR spectrum
[0041] Figure 4 A flowchart illustrating the synthesis of a bisnorbornene flame retardant A containing a phenyl phosphate structure.
[0042] Figure 5 A flowchart illustrating the synthesis of a bisnorbornene flame retardant B containing a phenyl phosphate structure.
[0043] Figure 6 A flowchart illustrating the synthesis of a mononorbornene flame retardant C containing a phenyl phosphate structure. Detailed Implementation
[0044] The present invention will be further described below with reference to specific embodiments. However, the scope of protection of the present invention is not limited to the following embodiments. Any non-essential adjustments and modifications made to the present invention based on the above description shall still fall within the scope of protection of the present invention.
[0045] The raw materials used in the following examples and comparative examples are:
[0046] Dicyclopentadiene, preferably from Sigma-Aldrich;
[0047] (Z)-Cyclooct-4-ene-1-carboxylic acid, preferably a product of Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0048] Flame retardants A and B are self-synthesized bisnorbornene-based flame retardants containing a phenyl phosphate structure, as detailed in Examples 1 and 5. Flame retardant C is a self-synthesized mononorbornene-based flame retardant containing a phenyl phosphate structure, as detailed in Comparative Example 5. The synthetic raw materials and catalysts include: 5-norbornene-2-methylamine, phenyl phosphate dichloride, 4-hydroxymethylbenzoic acid, 3-hydroxypropionic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, dicyclohexylcarbodiimide, 1-hydroxybenzotriazole, and 4-dimethylaminopyridine. Among them, 5-norbornene-2-methylamine is preferably a product of Sigma-Aldrich; phenyl phosphate dichloride, 4-hydroxymethylbenzoic acid and 3-hydroxypropionic acid are preferably products of Shanghai Aladdin Biochemical Technology Co., Ltd.; 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, dicyclohexylcarbodiimide, 1-hydroxybenzotriazole and 4-dimethylaminopyridine are preferably products of Shanghai Maclean Biochemical Technology Co., Ltd.; the organic solvent used in the synthesis is preferably a product of Shanghai Aladdin Biochemical Technology Co., Ltd.
[0049] Pentaerythritol phosphate and melamine are intumescent flame retardants, and products from Shanghai Aladdin Biochemical Technology Co., Ltd. are preferred.
[0050] Decabromodiphenyl ethane is a halogenated flame retardant, and antimony trioxide is a synergistic flame retardant. Products from Shanghai Maclean Biochemical Technology Co., Ltd. are preferred.
[0051] Grubbs' second-generation catalyst is a ruthenium-based catalyst, and the inhibitor is a phosphite, preferably a product from Sigma-Aldrich.
[0052] Table 1 lists the raw materials and quantities used in each embodiment.
[0053]
[0054] To demonstrate the effectiveness of this invention, six comparative examples are provided:
[0055] Table 2 shows the raw materials and quantities used in each comparative example.
[0056]
[0057]
[0058] Example 1
[0059] This embodiment of the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer comprises the following raw materials: 79.55 wt% dicyclopentadiene, 10 wt% flame retardant, 10 wt% (Z)-cyclooctyl-4-en-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst, and 0.15 wt% inhibitor. The flame retardant is a dinorbornene-based flame retardant A containing a phenyl phosphate structure.
[0060] Its structural formula is:
[0061]
[0062] Flame retardant A (synthesis route diagram attached) Figure 4 Preparation of )
[0063] (1) First, 0.1 mol of 3-hydroxypropionic acid, 0.049 mol of phenyl phosphate dichloride, and 0.1 mol of 4-dimethylaminopyridine were added to a three-necked flask containing 250 mL of dichloromethane. The three-necked flask was connected to a condenser and a nitrogen inlet / outlet. Under nitrogen protection, the reaction was carried out at 25 °C with stirring for 15 h. After the reaction was completed, the resulting mixture was subjected to multiple extractions, washing, filtration, drying, and rotary evaporation. Then, the product was enriched to obtain a dicarboxylic acid containing a phenyl phosphate structure.
[0064] (2) At 0℃ and under stirring conditions, 0.21 mol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and 0.21 mol of 1-hydroxybenzotriazole were added to a three-necked flask containing 0.21 mol of 5-norbornene-2-methylamine in 250 mL of dichloromethane. The three-necked flask was connected to a condenser. Then, 0.1 mol of the dicarboxylic acid containing the phenyl phosphate structure obtained in step (1) was added dropwise to the above mixed solution. The temperature was then gradually increased to 25℃ and the reaction was continued for 36 h.
[0065] (3) After the reaction was completed, the resulting mixture was extracted, washed, filtered, dried, and rotary evaporated multiple times. The organic phase was collected and subjected to rapid column chromatography using a mixture of dichloromethane and methanol as the eluent. The product was then enriched. 1 HNMR characterization yielded a bisnorbornene flame retardant A containing a phenyl phosphate structure.
[0066] Preparation of multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering materials containing phenyl phosphate-structured dinorbornene flame-retardant monomers:
[0067] (1) 10 wt% (Z)-cyclooctyl-4-ene-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst and 0.15 wt% inhibitor were added to 79.55 wt% dicyclopentadiene to obtain a mixture;
[0068] (2) Add 10wt% of the synthesized flame retardant A to the mixture and ultrasonically disperse the vial containing the mixture in an ice-water bath for 60s to obtain the dispersion.
[0069] (3) Finally, the dispersion is injected into a pre-made mold, and after local thermal initiation at 200°C, polymerization is carried out through its own thermal-driven self-propagation. This yields a multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer.
[0070] Example 2
[0071] This embodiment of the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer comprises the following raw materials: 69.55 wt% dicyclopentadiene, 20 wt% flame retardant, 10 wt% (Z)-cyclooctyl-4-en-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst, and 0.15 wt% inhibitor. The flame retardant is a dinorbornene-based flame retardant A containing a phenyl phosphate structure.
[0072] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this embodiment is the same as in Embodiment 1.
[0073] Example 3
[0074] This embodiment of the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer comprises the following raw materials: 59.55 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% (Z)-cyclooctyl-4-ene-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst, and 0.15 wt% inhibitor. The flame retardant is a dinorbornene-based flame retardant A containing a phenyl phosphate structure.
[0075] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this embodiment is the same as in Embodiment 1.
[0076] Example 4
[0077] This embodiment of the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer comprises the following raw materials: 49.55 wt% dicyclopentadiene, 40 wt% flame retardant, 10 wt% (Z)-cyclooctyl-4-ene-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst, and 0.15 wt% inhibitor. The flame retardant is a dinorbornene-based flame retardant A containing a phenyl phosphate structure.
[0078] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this embodiment is the same as in Embodiment 1.
[0079] Example 5
[0080] This embodiment of the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer comprises the following raw materials: 59.55 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% (Z)-cyclooctyl-4-ene-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst, and 0.15 wt% inhibitor. The flame retardant is a dinorbornene-based flame retardant B containing a phenyl phosphate structure.
[0081] Its structural formula is:
[0082]
[0083] Flame retardant B (synthesis route diagram attached) Figure 5 Preparation of )
[0084] (1) First, 0.1 mol of 4-hydroxymethylbenzoic acid, 0.049 mol of phenyl phosphate dichloride and 0.1 mol of 4-dimethylaminopyridine were added to a three-necked flask containing 250 mL of dichloromethane. The three-necked flask was connected to a condenser and a nitrogen inlet / outlet. Under nitrogen protection, the reaction was carried out at 25 °C with stirring for 15 h. After the reaction was completed, the resulting mixture was subjected to multiple extractions, washing, filtration, drying and rotary evaporation. Then the product was enriched to obtain a dicarboxylic acid containing a phenyl phosphate structure.
[0085] (2) At 0℃ and under stirring conditions, 0.21 mol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and 0.21 mol of 1-hydroxybenzotriazole were added to a three-necked flask containing 0.21 mol of 5-norbornene-2-methylamine in 250 mL of dichloromethane. The three-necked flask was connected to a condenser. Then, 0.1 mol of the dicarboxylic acid containing the phenyl phosphate structure obtained in step (1) was added dropwise to the above mixed solution. The temperature was then gradually increased to 35℃ and the reaction was continued for 10 h.
[0086] (3) After the reaction was completed, the resulting mixture was extracted, washed, filtered, dried, and rotary evaporated multiple times. The organic phase was collected and subjected to rapid column chromatography using a mixture of dichloromethane and methanol as the eluent. The product was then enriched. 1 HNMR characterization yielded a bisnorbornene flame retardant B containing a phenyl phosphate structure.
[0087] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this embodiment is the same as in Embodiment 1.
[0088] Example 6
[0089] This embodiment of the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer comprises the following raw materials: 59.55 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% (Z)-cyclooctyl-4-ene-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst, and 0.15 wt% inhibitor. The flame retardant consists of two dinorbornene-based flame retardants, A and B, containing a phenyl phosphate structure, in a ratio of 1:1.
[0090] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this embodiment is the same as in Embodiment 1.
[0091] Comparative Example 1
[0092] The basic process and target structure in this comparative example are the same as in Example 1, but the preparation method is different. The specific preparation process is as follows:
[0093] (1) First, 0.1 mol of 3-hydroxypropionic acid, 0.049 mol of phenyl phosphate dichloride, and 0.1 mol of 4-dimethylaminopyridine were added to a three-necked flask containing 250 mL of dichloromethane. The three-necked flask was connected to a condenser and a nitrogen inlet / outlet. Under nitrogen protection, the reaction was carried out at 25 °C with stirring for 15 h. After the reaction was completed, the resulting mixture was subjected to multiple extractions, washing, filtration, drying, and rotary evaporation. Then, the product was enriched to obtain a dicarboxylic acid containing a phenyl phosphate structure.
[0094] (2) At 0℃, 0.21 mol of 5-norbornene-2-methylamine, 0.1 mol of the dicarboxylic acid containing the phenyl phosphate structure obtained in step (1), and 0.21 mol of dicyclohexylcarbodiimide were added to a three-necked flask containing 250 mL of dichloromethane. The temperature was then gradually increased to 40℃, and the reaction was carried out for 8 h under stirring.
[0095] (3) After the reaction was completed, the resulting mixture was extracted, washed, filtered, dried, and rotary evaporated multiple times. The organic phase was collected and subjected to rapid column chromatography using a mixture of tetrachloromethane and methanol as the eluent. The product was then enriched. 1 HNMR characterization revealed that the target product could not be obtained.
[0096] Comparative Example 2
[0097] The flame-retardant polydicyclopentadiene engineering material of this comparative example includes the following raw materials: 99.55 wt% dicyclopentadiene, 0 wt% flame retardant, 0 wt% (Z)-cyclooct-4-en-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst, and 0.15 wt% inhibitor.
[0098] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this comparative example is the same as that in Example 1.
[0099] Comparative Example 3
[0100] The flame-retardant polydicyclopentadiene engineering material of this comparative example comprises the following raw materials: 59.55 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% (Z)-cyclooctyl-4-ene-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst, and 0.15 wt% inhibitor. The flame retardant is an intumescent flame retardant, pentaerythritol phosphate, and melamine, in a ratio of 2:1.
[0101] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this comparative example is the same as that in Example 1.
[0102] Comparative Example 4
[0103] The flame-retardant polydicyclopentadiene engineering material of this comparative example comprises the following raw materials: 59.55 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% (Z)-cyclooctyl-4-en-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst, and 0.15 wt% inhibitor. The flame retardant is a halogenated flame retardant, decabromodiphenyl ethane, and a synergist, antimony trioxide, in a ratio of 5:1.
[0104] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this comparative example is the same as that in Example 1.
[0105] Comparative Example 5
[0106] The flame-retardant polydicyclopentadiene engineering material of this comparative example comprises the following raw materials: 59.55 wt% dicyclopentadiene, 30 wt% flame retardant, 10 wt% (Z)-cyclooctyl-4-en-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst, and 0.15 wt% inhibitor. The flame retardant is a mononorbornene-based flame retardant C containing a phenyl phosphate structure.
[0107] Its structural formula is:
[0108]
[0109] Flame retardant C (synthesis route diagram attached) Figure 6 Preparation of )
[0110] 0.1 mol of triethylamine was added to a 250 mL three-necked flask containing 0.1 mol of phenyl dichloride phosphate. The flask was connected to a condenser and a nitrogen inlet / outlet. Then, 0.11 mol of 5-norbornene-2-methanol was added dropwise to the mixture. The reaction was carried out at 50 °C with stirring under nitrogen protection for 2 h. Afterward, the mixture was cooled to 25 °C and stirred for 30 min. After the reaction was complete, the resulting mixture was subjected to multiple extractions, washing, filtration, drying, and rotary evaporation. The organic phase was collected and subjected to rapid column chromatography using a mixture of dichloromethane and methanol as eluent. The product was then enriched. 1 HNMR characterization yielded a mononorbornene flame retardant C containing a phenyl phosphate structure.
[0111] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this comparative example is the same as that in Example 1.
[0112] Comparative Example 6
[0113] The flame-retardant polydicyclopentadiene engineering material of this comparative example comprises the following raw materials: 69.55 wt% dicyclopentadiene, 30 wt% flame retardant, 0 wt% (Z)-cyclooctyl-4-en-1-carboxylic acid, 0.3 wt% Grubbs second-generation catalyst, and 0.15 wt% inhibitor. The flame retardant is a dinorbornene-based flame retardant A containing a phenyl phosphate ester structure.
[0114] The preparation process of the flame-retardant polydicyclopentadiene engineering material in this comparative example is the same as that in Example 1.
[0115] Tests and Results
[0116] The materials prepared in the above embodiments and comparative examples were cut to prepare test strips, and the testing method was as follows:
[0117] Enthalpy of polymerization and degree of cure: The enthalpy of polymerization and degree of cure were determined under a N2 atmosphere. For the enthalpy of polymerization test, the sample was first cooled to -10℃, held at that temperature for 5 min, and then heated to 200℃, with a heating and cooling rate of 5℃ / min throughout the process. For the residual heat of reaction test, the sample was first heated to 250℃, held at that temperature for 5 min, then cooled to -20℃, and finally heated from -20℃ to 250℃, with a heating and cooling rate of 10℃ / min throughout the process. The enthalpy of polymerization (H2) was obtained. r ) and waste heat of reaction (H res The degree of curing α of the sample is calculated using the following formula, as shown in the formula below:
[0118]
[0119] molecular weight M between cross-linking points c M c Calculate using the following formula:
[0120]
[0121] In the formula, the value of ρ is taken as 1 g·cm³. -3 R is the ideal gas constant, with a value of 8.314 J·mol⁻¹. -1 ·K -1 T is T g +50K, E′ Tg+50K The temperature is T g Storage modulus of the sample at +50K.
[0122] Thermal stability: Thermogravimetric analysis was performed on the samples in an N2 atmosphere using a Q500 thermogravimetric analyzer. The test temperature range was 30–800℃, and the heating rate was 10℃ / min.
[0123] Tensile strength: Tested according to ISO 527-2:1993 standard at a speed of 50 mm / min.
[0124] Elongation at break: Tested according to ISO 527-2:1993 standard at a speed of 50 mm / min.
[0125] Impact resistance: Tested according to ISO 180:2000 standard.
[0126] Heat distortion temperature: tested according to ISO 75-2:2004 standard.
[0127] Hardness: Tested according to ISO 7619-973 standard.
[0128] Fatigue resistance: The fatigue life of the samples was studied using uniaxial tensile-tensile fatigue tests according to ASTM D7791-12 standard. The tests were conducted under a constant stress amplitude of 20 MPa, a constant stress ratio (R = 0.1), and a frequency of 3 Hz. All fatigue tests used sinusoidal waveforms.
[0129] Creep resistance: Tested according to GB / T 6059-1985 standard, sample size is 120mm×10mm×4mm, test temperature is 23℃, stress is 23MPa, and the strain (%) of the outermost layer of the sample is recorded after 48h.
[0130] Limiting oxygen index: Tested according to GB / T 2406-1993 standard, sample size is 110mm×6mm×2mm.
[0131] UL-94: Tested according to GB / T 2048-1996 standard.
[0132] Conical calorimetry: Tested according to ISO 5660-1-2002 standard, the radiant power is 35kW / m².2 The sample size is 100mm×100mm×3mm.
[0133] I D / I G The graphitization structure of the samples was characterized using Raman microscopy. The samples were placed on a glass slide for testing, with an excitation wavelength of 532 nm and a sampling range of 500–3000 cm⁻¹. -1 .
[0134] Table 3. Polymerization kinetics, mechanical properties, and flame retardant properties of the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering materials containing phenyl phosphate-structured dinorbornene flame-retardant monomers prepared in Examples 1-6.
[0135]
[0136]
[0137] Table 4 shows the polymerization kinetics, mechanical properties, and flame retardant properties of the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering materials containing phenyl phosphate-structured dinorbornene flame-retardant monomers prepared in Comparative Examples 1-6.
[0138]
[0139]
[0140] Tables 1 and 2 show the experimental formulations of Examples 1-6 and Comparative Examples 1-6, while Tables 3 and 4 show the polymerization kinetics, mechanical properties, and flame retardant performance indicators of the flame-retardant polydicyclopentadiene engineering materials prepared in the corresponding Examples 1-6 and Comparative Examples 1-6.
[0141] The polymerization kinetics data in Table 3 for Examples 1-6 show that the introduction of comonomers did not significantly reduce the polymerization enthalpy and degree of cure of the materials. This is because the synthesized dinorbornene flame retardant containing a phenyl phosphate structure participates in the copolymerization reaction, causing minimal damage to the crosslinking network of the system. The degree of cure in all examples exceeded 99%, and the materials maintained a high crosslinking density. In Examples 1-6, with the increase of flame retardant content, the glass transition temperature of the polydicyclopentadiene engineering material increased from 161°C to a maximum of approximately 219°C, the heat distortion temperature increased from 146°C to a maximum of 205°C, and the initial decomposition temperature T... 5%The thermal stability of the material was significantly improved, reaching a maximum of 489.38℃ from 460.65℃. Characterization of the mechanical properties of the material revealed that the introduction of a bisnorbornene flame retardant containing a phenyl phosphate structure and (Z)-cyclooctyl-4-ene-1-carboxylic acid into the copolymer system significantly increased the tensile strength, elongation at break, and impact strength. This is because the material maintains a high degree of chemical cross-linking after the introduction of comonomers into the system. Simultaneously, hydrogen bonds and π-π stacking interactions are introduced, further constructing a dynamic physical cross-linking network. Due to the relatively low bond energy of hydrogen bonds, they can break before covalent bonds when the material is subjected to load deformation, thus dissipating energy and preventing premature failure due to stress concentration, thereby strengthening and toughening the material. The multiple cross-linking network structure of chemical and physical components also effectively prevents molecular chain slippage, contributing to creep resistance and fatigue resistance. Finally, characterization of the flame retardant properties of the above materials revealed that the limiting oxygen index (LOI) increased from 18% to 43%, the peak heat release rate (pHRR) decreased by 87.64%, the fire growth rate (FIGRA) decreased by 98.11%, the peak smoke generation rate (pSPR) decreased by 89.47%, and the fire performance index (FPI) increased by more than 13 times. D / I G The flame retardancy was reduced by 80.83%, the char residue was increased by 182.91%, and the material achieved a UL-94V-0 flame retardancy rating. These results indicate that the introduction of a bisnorbornene flame retardant containing a phenyl phosphate structure and (Z)-cyclooctyl-4-ene-1-carboxylic acid significantly improved the flame retardant properties of polydicyclopentadiene engineering materials.
[0142] Table 4 shows the relevant data results for Comparative Examples 1-6. In Comparative Examples 3-4, an additive intumescent flame retardant and a halogenated flame retardant were introduced into polydicyclopentadiene, respectively. The results showed that although the addition of the intumescent flame retardant improved the flame retardant performance of the material, it also reduced the mechanical properties. The addition of the halogenated flame retardant, while providing flame retardancy, released a large amount of toxic fumes, polluting the environment and greatly limiting its application areas. Furthermore, the flame retardant and mechanical properties of the polydicyclopentadiene material obtained were significantly worse than those of the embodiments in this patent. In Comparative Example 5, a self-synthesized mononorbornene flame retardant C containing a phenyl phosphate structure was introduced into the system. The results showed that, compared with the polydicyclopentadiene engineering material containing a mononorbornene flame retardant monomer with a phenyl phosphate structure, the material containing a dinorbornene flame retardant monomer with a phenyl phosphate structure not only had higher strength and toughness but also better flame retardant effect. In Comparative Example 6, the comonomer (Z)-cyclooctyl-4-ene-1-carboxylic acid was not introduced into the system. Due to the weakening of hydrogen bond interactions in the system, the mechanical properties of the material decreased compared to the embodiments in this patent. At the same time, during combustion, the char-forming ability of the material was weakened, and the flame retardant performance was significantly worse than that of the embodiments in this patent.
[0143] In summary, the introduction of bisnorbornene flame retardants containing phenyl phosphate structure and (Z)-cyclooctyl-4-ene-1-carboxylic acid improves the flame retardant properties of polydicyclopentadiene engineering materials while maintaining a good balance between rigidity and toughness, enabling the materials to be used in a variety of complex scenarios.
[0144] Although the present invention has been described in detail through the above preferred embodiments, it should be understood that the above description should not be considered as a limitation of the present invention.
Claims
1. A bisnorbornene flame retardant containing a phenyl phosphate structure, characterized in that: The bisnorbornene flame retardant containing a phenyl phosphate structure has the structure shown in formula (1): ; In formula (1), R1 and R2 are each an aliphatic substituent with 1-8 carbon atoms or an aromatic substituent with 6-12 carbon atoms.
2. A process for preparing the bisnorbornene-based flame retardant containing a phenyl phosphate structure according to claim 1, characterized by, The method includes: A condensation acylation reaction is carried out in an organic solvent with 5-norbornene-2-methylamine and a dicarboxylic acid containing a phenyl phosphate structure, under the action of a catalyst. First, under stirring conditions at 0℃–5℃, the catalyst is added proportionally to a solution containing a monoamine, norbornene, and an organic solvent to obtain a mixed solution. Then, the dicarboxylic acid containing a phenyl phosphate structure is added dropwise to the mixed solution. The reaction is then carried out at 20℃–70℃ under stirring conditions for 2–40 hours. After the reaction, the product is washed, filtered, and dried, and finally enriched to obtain the bisnorbornene flame retardant containing a phenyl phosphate structure. The dicarboxylic acid containing a phenyl phosphate structure is prepared by the following method: 0.1 mol of 3-hydroxypropionic acid, 0.049 mol of phenyl phosphate dichloride, and 0.1 mol of... 4-Dimethylaminopyridine was added to a three-necked flask containing 250 mL of dichloromethane. The three-necked flask was connected to a condenser and a nitrogen inlet / outlet. Under nitrogen protection, the reaction was carried out at 25 °C with stirring for 15 h. After the reaction was completed, the resulting mixture was subjected to multiple extractions, washing, filtration, drying, and rotary evaporation. The product was then enriched to obtain a dicarboxylic acid containing the phenyl phosphate structure.
3. The production method according to claim 2, wherein The catalyst is one or a mixture of several of the following: triethylamine, N,N-diisopropylethylamine, pyridine, sodium acetate, 4-N,N-dimethylpyridine, 4-dimethylaminopyridine, 1-hydroxybenzotriazole, dicyclohexylcarbodiimide, diisopropylcarbodiimide, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide. The organic solvent is at least one of the following: tetrahydrofuran, dichloromethane, chloroform, N,N-dimethylformamide, acetonitrile, acetone, benzene, and toluene.
4. The production method according to claim 2 or 3, characterized by, The molar ratio of the catalyst to norbornene containing a monoamine is 1:1, while the molar ratio of the catalyst, the dicarboxylic acid containing a phenyl phosphate structure, and norbornene containing a monoamine is 2.05:1:2.05 to 2.15:1:2.
15.
5. Use of a bisnorbornene-based flame retardant containing a phenyl phosphate structure as a raw material according to claim 1, characterized by, The bisnorbornene flame retardant containing a phenyl phosphate structure is copolymerized with dicyclopentadiene and (Z)-cyclooct-4-en-1-carboxylic acid monomers via thermally driven self-propagating technology to obtain polydicyclopentadiene engineering materials.
6. A multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured bisnorbornene flame-retardant monomer, characterized in that: The raw materials for preparing the polydicyclopentadiene engineering material include: dicyclopentadiene, (Z)-cyclooct-4-en-1-carboxylic acid, and a bisnorbornene flame retardant containing a phenyl phosphate structure as shown in formula (1): ; In formula (1), R1 and R2 are each independently an aliphatic substituent with 1-8 carbon atoms or an aromatic substituent with 6-12 carbon atoms; The polydicyclopentadiene engineering material includes the structure shown in formula (2): ; In equation (2), m, n, p, and q are all independent integers between 50 and 1500; R1 and R2 in equation (2) are the same as R1 and R2 in equation (1).
7. The multiply crosslinked intrinsically flame retardant polydicyclopentadiene engineering material of claim 6 containing phosphonate structural bisnorbornene flame retardant monomers, wherein, The mass percentage of the raw material is: Dicyclopentadiene 49.40 wt%–79.70 wt%; 10.00 wt%–40.00 wt% of dinorbornene flame retardant containing phenyl phosphate structure. (Z)-Cyclooct-4-ene-1-carboxylic acid 10.00 wt%.
8. A method for producing the multiply crosslinked intrinsically flame retardant polydicyclopentadiene engineering material containing a phosphonate structural bisnorbornene flame retardant monomer according to claim 6 or 7, wherein the sum of the mass percentages of each raw material for producing the polydicyclopentadiene engineering material is 100 wt%, characterized in that, The mass percentages of each raw material are as follows: ; The ruthenium-based catalyst is a second-generation Grubbs catalyst; The inhibitor is a phosphate ester; The preparation method of the multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing a phenyl phosphate-structured dinorbornene flame-retardant monomer includes: (1) Disperse the bisnorbornene flame retardant containing phenyl phosphate structure into a mixture containing dicyclopentadiene, (Z)-cyclooct-4-en-1-carboxylic acid, Grubbs second-generation catalyst and inhibitor in proportion, and ultrasonically mix under ice-water bath conditions to obtain a dispersion. (2) The dispersion is injected into the mold and local thermal initiation is carried out under heating conditions. Through its own thermal-driven self-propagating polymerization, the multi-crosslinked intrinsic flame-retardant polydicyclopentadiene engineering material containing the phenyl phosphate structure dinorbornene flame-retardant monomer is copolymerized to obtain the multi-crosslinked intrinsic flame-retardant polydicyclopentadiene engineering material.
9. Use of a multiply crosslinked intrinsically flame retardant polydicyclopentadiene engineering material containing phosphonate structured bisnorbornene flame retardant monomers according to any one of claims 6 to 7 or a multiply crosslinked intrinsically flame retardant polydicyclopentadiene engineering material containing phosphonate structured bisnorbornene flame retardant monomers prepared by the method of claim 8, characterized in that: The multi-crosslinked intrinsically flame-retardant polydicyclopentadiene engineering material containing phenyl phosphate-structured dinorbornene flame-retardant monomers is used in rocket casings, missile tail fins, vehicle tracks, or engine cover components.
Citation Information
Patent Citations
Composite flame-retardant agent, preparation method and flame-retardant poly-dicyclopentadiene material
CN104327205A
Halogen-free flame retardant and flame-retardant high polymer material comprising same
CN105085984A
High-heat-resistance halogen-free intrinsic flame-retardant polydicyclopentadiene engineering material and preparation method thereof
CN116396468A
Self-crosslinking charring intrinsic flame-retardant polydicyclopentadiene engineering material and preparation method thereof
CN114316215A
High-modulus, high-impact, wear-resistant and heat-resistant intrinsic flame-retardant polydicyclopentadiene engineering material and preparation method thereof
CN114790260A