A three-dimensional wave absorbing frequency selective material and a manufacturing method thereof
By printing nanomaterial patterns on aramid paper and combining it with phenolic resin, a three-dimensional absorbing frequency-selective material is formed, which solves the problems of performance attenuation and high production cost of traditional absorbing materials at high temperatures, and achieves lightweight and high-temperature stability. Wave-absorbing performance simplifies the process.
Patent Information
- Application Number
- CN202311607918.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-11-29
AI Technical Summary
The performance of traditional absorbing honeycomb materials is attenuated in high-temperature environments, and the complex structure leads to high production costs. It cannot meet the lightweight and high-temperature stability needs of modern stealth fighters.
Multiple layers of aramid paper printed with two-dimensional metamaterial units are used to dislocate and bond each other. Patterns such as circular rings and elliptical rings are printed using nano carbon powder, nano graphene or nano metal powder, combined with a mixture of phenolic resin and organic solvents. , a three-dimensional wave-absorbing frequency-selective material is formed through hot pressing and stretching processes, simplifying the process and reducing costs.
It achieves stability and lightweight structure that maintains wave-absorbing performance in high-temperature environments, meets the mechanical and stealth requirements of modern stealth fighters, while simplifying the production process and reducing costs.
Smart Images

Figure CN117341288B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials, and in particular to a three-dimensional wave absorbing frequency selective material and a manufacturing method thereof. Background Art
[0002] Aramid paper honeycombs, as structural core materials with high specific strength and high specific stiffness, have been widely used in the aviation field. Now, facing increasingly demanding use environments, especially the high requirements for radar absorption and stealth capabilities, it is not enough for honeycomb core materials to have only excellent mechanical properties, but also to meet radar absorption and stealth performance indicators. However, as a functional material, traditional radar absorbing honeycombs have poor designability and high mass density, and cannot achieve lightweight and designability, a new performance design goal for aerospace vehicles, while meeting the requirements for structural and functional integration.
[0003] CN115603058A of the Institute of Aerospace Special Materials and Process Technology discloses a three-dimensional metamaterial based on a honeycomb structure and a preparation method thereof. The three-dimensional metamaterial based on a honeycomb structure includes an inner packaging layer, an outer packaging layer, a two-dimensional frequency-selective screen, and a honeycomb structure with microstructures in the wall; the two-dimensional frequency-selective screen is arranged above the inner packaging layer; the honeycomb structure is arranged above the two-dimensional frequency-selective screen, each cell in the honeycomb structure is a unit, and the wall of each unit contains multiple electromagnetic microstructures; the outer packaging layer is the outermost layer of the three-dimensional metamaterial. The inner packaging layer, the two-dimensional frequency-selective screen, the honeycomb structure with microstructures in the wall, and the outer packaging layer are laid layer by layer in order from the inside to the outside, and the three-dimensional metamaterial based on the honeycomb structure is obtained by compression molding using prepreg bags. The three-dimensional metamaterial structure of the present invention has the advantages of simple and efficient processing procedures, stable and controllable electromagnetic properties, good filtering performance, and can achieve wide-angle filtering effects. The invention uses a honeycomb core structure to set an electromagnetic microstructure on the inner wall of each cell unit. The electromagnetic microstructure is three hexagonal concentric rings. The material of the electromagnetic microstructure is conductive ink, and the conductive ink is conductive copper paste or conductive silver paste. The electromagnetic microstructure set on the inner wall of the cell provides electromagnetic resonance in the thickness direction, thereby improving the filtering performance and achieving a wide-angle filtering effect, and can maintain the filtering performance within an incident angle range of 70 degrees. The above invention has achieved certain effects in filtering performance, but its complex three-layer same-ring unit structure makes the packaging of the honeycomb core structure extremely difficult. The material of the electromagnetic microstructure is conductive ink, and the thermal stability temperature of the conductive ink is up to 200 degrees Celsius. The present invention is applied to high-speed aircraft and withstands instantaneous temperatures exceeding 350 degrees Celsius, which damages the stable structure of the conductive ink, causing the stealth wave absorption performance of the high-speed aircraft to decay or dissipate, and this damage is irreversible; in addition, the three-layer same-ring unit structure increases the mass of the honeycomb core structure, which cannot meet the lightweight requirements of modern stealth fighters. Therefore, how to provide a high-temperature resistant, structurally stable, and wave-absorbing stealth three-dimensional wave-absorbing frequency-selective material that meets mechanical properties has become a top priority in industry research. In addition, it is necessary to avoid complex preparation procedures and easy processing characteristics to reduce the production cost of three-dimensional wave-absorbing frequency-selective materials. Summary of the invention
[0004] To this end, the present invention provides a three-dimensional wave absorbing frequency selective material and a manufacturing method thereof to overcome the above-mentioned shortcomings.
[0005] To achieve the above-mentioned purpose, the present invention provides a three-dimensional wave absorbing frequency selective material, which comprises multiple layers of aramid paper printed with two-dimensional metamaterial units, which are mutually staggered and bonded together, and the aramid paper of two adjacent layers of two-dimensional metamaterial units is folded into a plurality of through holes arranged at intervals to have a regular hexagonal cross-section, and the aramid paper of the two-dimensional metamaterial unit is obtained by printing metamaterial structures of different units on paper made of aramid fiber, and each layer of the aramid paper of the two-dimensional metamaterial unit is impregnated with a mixture of phenolic resin and organic solvent, and the side length of the regular hexagonal through hole ranges from 3 to 10 mm.
[0006] Preferably, the organic solvent is one or more of ethanol, toluene, acetone and chloroform.
[0007] Preferably, the two-dimensional metamaterial unit prints a circular ring, an elliptical ring, or a regular polygonal pattern, and the unit printing material is nano-carbon powder, nano-graphene, or various nano-metal powders.
[0008] Preferably, in the aramid paper of the two-dimensional metamaterial unit provided, the thickness of the nano-carbon powder, nano-graphene or various nano-metal powders corresponding to the printed pattern is 0.05-0.5 mm.
[0009] Preferably, the arrangement direction of the pattern printed on the aramid paper of the two-dimensional metamaterial unit is consistent with the fiber distribution direction in the aramid paper, with an angle range of ±15°.
[0010] A method for manufacturing a three-dimensional wave absorbing frequency selective material comprises the following steps:
[0011] Material selection process: provide multi-layer aramid paper, which is not allowed to be damaged or have foreign matter that affects the electrical performance;
[0012] Printing process: Use nano-carbon powder, nano-graphene or nano-metal powder to print two-dimensional metamaterial units on multi-layer aramid paper. The printed patterns of the two-dimensional metamaterial units are circular rings, elliptical rings, and regular polygonal patterns. The thickness of the nano-carbon powder, nano-graphene or nano-metal powder corresponding to the printed pattern is 0.05~0.5mm. The arrangement direction of the printed pattern is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°
[0013] Gluing process: covering the front and back sides of the aramid paper of each layer of the two-dimensional metamaterial unit with a high-temperature resistant gel coat of equal thickness and uniformity; Curing process: performing high-temperature curing on the aramid paper of all the two-dimensional metamaterial units covered with the high-temperature resistant gel coat;
[0014] Gluing process: Gluing is performed at designated intervals on the aramid paper of each cured two-dimensional metamaterial unit, and the interval distance is determined by the side length of the honeycomb cells. On the aramid paper of the two-dimensional metamaterial unit, each strip of the glue is coated into a strip shape to form a glue strip, and in the direction perpendicular to the extension of the glue strip, the width of the glue strip is one third of the interval distance between two adjacent glue strips;
[0015] Paper stacking process: stacking each layer of the aramid paper of the two-dimensional metamaterial unit, wherein the spacing between two adjacent adhesive strips of the aramid paper of the stacked two-dimensional metamaterial unit is less than 10 mm; stacking the multiple layers of aramid paper of the two-dimensional metamaterial unit coated with adhesive strips in sequence, and staggering all the adhesive strips of the aramid paper of two adjacent layers of the two-dimensional metamaterial unit at equal distances;
[0016] Hot pressing step: hot pressing the aramid paper of the glued multi-layer two-dimensional metamaterial unit to obtain a honeycomb laminate;
[0017] Stretching process: stretching and shaping the honeycomb laminate, and from the beginning of stretching to the process of stretching and shaping, the honeycomb laminate is kept in a water-spraying state until the honeycomb laminate forms a honeycomb-shaped honeycomb core blank;
[0018] Providing a mixed liquid of reinforcing materials, and spraying the mixed liquid evenly on the honeycomb wall of the honeycomb core blank after stretching and shaping;
[0019] Shaping process: After the mixed liquid is sprayed all over the honeycomb wall of the honeycomb core blank, it is immediately placed in an oven for shaping before the mixed liquid dries.
[0020] Preferably, the honeycomb core blank after being shaped in the oven in the shaping process is further subjected to the following steps to form the three-dimensional microwave absorbing frequency selective material honeycomb core:
[0021] Dipping and curing process: providing a dipping resin mixture, stirring it evenly, dipping the honeycomb core blank after being shaped in the oven, and curing the dipping honeycomb core blank after dipping;
[0022] Machining process: The solidified honeycomb core blank is processed into the three-dimensional wave-absorbing frequency-selective material with a designed structural shape on a honeycomb-specific five-axis machining center.
[0023] Preferably, in the coating process, both sides of the aramid paper of each layer of the two-dimensional metamaterial unit are covered with a high-temperature resistant gel coat of equal thickness and uniformity, which is at least one of cyanate ester, bismaleimide resin or polyimide resin, and the gel coat thickness is ≤0.5mm.
[0024] Preferably, a trimming step is included between the hot pressing step and the stretching step, and the trimming step is to trim the honeycomb laminate according to the designed width.
[0025] Preferably, the impregnation resin mixture in the impregnation curing step comprises phenolic resin and an organic solvent, industrial alcohol, and the mass of the phenolic resin is 50% to 60% of the total mass of the impregnation mixture.
[0026] Preferably, in the dipping and curing process, the dipping time is 10 minutes to 1 hour, the dipping times are 1-20 times, and after each dipping, it is preheated in a drying drum at 80 to 120 degrees for 30 to 60 minutes.
[0027] Preferably, in the dipping and curing process, after the last dipping, curing is performed at a temperature of 130 to 180 degrees for 90 to 240 minutes.
[0028] Preferably, the reinforcing material in the stretching process is a mixture of phenolic resin and an organic solvent, and the organic solvent is one or more of ethanol, toluene, acetone and chloroform.
[0029] The beneficial effects of the present invention are as follows: compared with the prior art, the three-dimensional wave absorbing frequency selective material manufactured by the present invention and the three-dimensional wave absorbing frequency selective material honeycomb core manufactured by the three-dimensional wave absorbing frequency selective material have the following advantages:
[0030] On the basis of meeting the mechanical properties of modern stealth fighters and aerospace vehicles, it is more lightweight; it overcomes the single function of the existing aramid paper honeycomb core, and on the basis of meeting the mechanical properties, the honeycomb core structure has wave-absorbing properties, even if modern stealth fighters and aerospace vehicles have stealth properties;
[0031] The present invention prints patterns such as circular rings and open rings on aramid paper by using nano-carbon powder, nano-graphene or various nano-metal powders, so that the paper has a wave-absorbing unit structure, and the wave-absorbing frequency band covers S, C, X, and Ku, which can meet the stealth performance requirements of modern stealth fighters and aerospace vehicles;
[0032] The present invention prints circular rings, released rings and other unit structures to enable the further processed three-dimensional absorbing frequency selective material honeycomb core to meet the lightweight requirements, and the processing procedures are simpler and more efficient than existing invisible absorbing materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a schematic structural diagram of a three-dimensional wave-absorbing frequency-selective material of the present invention;
[0034] Figure 2 A schematic diagram of a pattern printed on aramid paper of a two-dimensional metamaterial unit of the present invention;
[0035] Figure 3 A schematic diagram of an embodiment of a pattern printed on aramid paper of a two-dimensional metamaterial unit of the present invention;
[0036] Figure 4A schematic diagram of an embodiment of a pattern printed on aramid paper of a two-dimensional metamaterial unit of the present invention;
[0037] Figure 5 A schematic diagram of an embodiment of a pattern printed on aramid paper of a two-dimensional metamaterial unit of the present invention;
[0038] Figure 6 It is a schematic diagram of a method for manufacturing a three-dimensional wave absorbing frequency selective material of the present invention;
[0039] Figure 7 Schematic diagram of another embodiment of a method for manufacturing a three-dimensional wave absorbing frequency selective material according to the present invention
[0040] Figure 8 A schematic diagram of the additional steps required for the three-dimensional microwave absorbing frequency selective material honeycomb core of the present invention;
[0041] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0042] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0043] It should be noted that, in the description of the present invention, terms such as "up", "down", "left", "right", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.
[0044] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0045] Embodiment 1, as Figure 1 , Figure 2 , Figure 6-Figure 8As shown, a three-dimensional wave absorbing frequency selective material comprises multiple layers of aramid paper printed with two-dimensional metamaterial units, which are mutually staggered and bonded together, and the aramid paper of two adjacent layers of two-dimensional metamaterial units is folded into multiple through holes with regular hexagonal cross-sections arranged at intervals, and the aramid paper of the two-dimensional metamaterial unit is obtained by printing the metamaterial structure of different units on paper made of aramid fiber, and each layer of the aramid paper of the two-dimensional metamaterial unit is impregnated with a mixture of phenolic resin and organic solvent, and the side length of the regular hexagonal through hole ranges from 3 to 10 mm. The organic solution is one or more of ethanol, toluene, acetone, and chloroform. The two-dimensional metamaterial unit prints a circular pattern, and the unit printing material is nano-carbon powder, nano-graphene or nano-metal powder. The arrangement direction of the pattern printed on the aramid paper of the two-dimensional metamaterial unit is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°.
[0046] The manufacturing method thereof comprises the following steps:
[0047] S1 material selection process: provide multi-layer aramid paper, which is not allowed to be damaged or have foreign matter that affects the electrical performance;
[0048] S2 printing process: use nano-carbon powder, nano-graphene or various nano-metal powders to print two-dimensional metamaterial units on multi-layer aramid paper, and the printed pattern of the two-dimensional metamaterial unit is a circular pattern; the diameter of the circular pattern is 0.2-3 mm, and it is evenly arranged vertically and horizontally. The distance between each two adjacent groups of circular rings is 0.1-1.5 mm, which is the radius of the circular ring. The aramid paper of the provided two-dimensional metamaterial unit, wherein the thickness of the nano-carbon powder, nano-graphene or various nano-metal powders corresponding to the printed pattern is 0.05~0.5mm; the arrangement direction of the printed pattern is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°
[0049] S3 coating process: Cover the front and back sides of the aramid paper of each layer of the two-dimensional metamaterial unit with a high-temperature resistant gel coat of equal thickness and uniformity;
[0050] S4 curing process: high temperature curing of the aramid paper of all two-dimensional metamaterial units covered with high temperature resistant gel coat;
[0051] S5 glue coating process: coating the aramid paper of each cured two-dimensional metamaterial unit with glue at a specified interval, the interval distance being determined by the side length of the honeycomb cells, and coating each strip of glue on the aramid paper of the two-dimensional metamaterial unit into a strip shape, and in a direction perpendicular to the extension of the strip, the width of the strip is one third of the interval distance between two adjacent strips;
[0052] S6 paper stacking step: stacking each layer of the aramid paper of the two-dimensional metamaterial unit, wherein the spacing between two adjacent adhesive strips of the aramid paper of the stacked two-dimensional metamaterial unit is less than 10 mm; stacking the multiple layers of aramid paper of the two-dimensional metamaterial unit coated with adhesive strips in sequence, and staggering all the adhesive strips of the aramid paper of two adjacent layers of the two-dimensional metamaterial unit at equal distances;
[0053] S7 hot pressing step: hot pressing the aramid paper of the glued multi-layer two-dimensional metamaterial unit to obtain a honeycomb laminate;
[0054] S8 stretching process: stretching and shaping the honeycomb laminate, and from the beginning of stretching to the process of stretching and shaping, the honeycomb laminate is kept in a water-spraying state until the honeycomb laminate forms a honeycomb-shaped honeycomb core blank;
[0055] Providing a mixed liquid of reinforcing materials, and spraying the mixed liquid evenly on the honeycomb wall of the honeycomb core blank after stretching and shaping;
[0056] S9 shaping process: after the mixed liquid is sprayed all over the honeycomb wall of the honeycomb core blank, the mixed liquid is immediately placed in an oven for shaping before it dries.
[0057] Between the S7 hot pressing process and the S8 stretching process, there is also an S71 trimming process, which is to trim the honeycomb laminate according to the designed width. The dipping resin mixture in the dipping and curing process includes phenolic resin and organic solvent industrial alcohol, and the mass of the phenolic resin is 50% to 60% of the total mass of the dipping mixture. In the dipping and curing process, the dipping time is 10 minutes to 1 hour, the number of dippings is 1-20 times, and after each dipping, it is preheated in a drying drum at 80 to 120 degrees for 30 to 60 minutes. In the dipping and curing process, after the last dipping is completed, it is cured at a temperature of 130 to 180 degrees for 90 to 240 minutes. The reinforcing material in the stretching process is a mixture of phenolic resin and an organic solvent, and the organic solvent is one or more of ethanol, toluene, acetone, and chloroform.
[0058] The ring printed with nano-carbon powder is recorded as sample 1, and its absorption frequency range is 2-8GHz, and the average vertical incidence reflectivity is 10dB; the ring printed with nano-graphene is recorded as sample 2, and its absorption frequency range is 2-18GHz, and the average vertical incidence reflectivity is 20dB;
[0059] The ring printed with nano-metal powder is marked as sample 3. This embodiment uses Fe, Co, and Ni alloy powders with an absorption frequency of 3-16 GHz and an average vertical incidence reflectivity of 13 dB.
[0060] Embodiment 2, as Figure 1 , Figure 2 , Figure 6-Figure 8 As shown, a three-dimensional wave absorbing frequency selective material comprises multiple layers of aramid paper printed with two-dimensional metamaterial units, which are mutually staggered and bonded together, and the aramid paper of two adjacent layers of two-dimensional metamaterial units is folded into multiple through holes with regular hexagonal cross-sections arranged at intervals, and the aramid paper of the two-dimensional metamaterial unit is obtained by printing the metamaterial structure of different units on paper made of aramid fiber, and each layer of the aramid paper of the two-dimensional metamaterial unit is impregnated with a mixture of phenolic resin and organic solvent, and the side length of the regular hexagonal through hole ranges from 3 to 10 mm. The organic solution is one or more of ethanol, toluene, acetone, and chloroform. The two-dimensional metamaterial unit prints a circular pattern, and the unit printing material is nano-carbon powder, nano-graphene or nano-metal powder. The arrangement direction of the pattern printed on the aramid paper of the two-dimensional metamaterial unit is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°.
[0061] The manufacturing method thereof comprises the following steps:
[0062] S1 material selection process: provide multi-layer aramid paper, which is not allowed to be damaged or have foreign matter that affects the electrical performance;
[0063] S2 printing process: use nano-carbon powder, nano-graphene or nano-metal powder to print two-dimensional metamaterial units on multi-layer aramid paper, and the printed pattern of the two-dimensional metamaterial unit is a circular pattern; the diameter of the circular pattern is 0.2-3 mm, and it is evenly arranged vertically and horizontally. The distance between each two adjacent groups of circular rings is 0.1-1.5 mm, which is the radius of the circular ring. The aramid paper of the provided two-dimensional metamaterial unit, wherein the thickness of the nano-carbon powder, nano-graphene or various nano-metal powders corresponding to the printed pattern is 0.05~0.5mm; the arrangement direction of the printed pattern is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°
[0064] S3 coating process: Cover the front and back sides of the aramid paper of each layer of the two-dimensional metamaterial unit with a high-temperature resistant gel coat of equal thickness and uniformity;
[0065] S4 curing process: high temperature curing of the aramid paper of all two-dimensional metamaterial units covered with high temperature resistant gel coat;
[0066] S5 glue coating process: coating the aramid paper of each cured two-dimensional metamaterial unit with glue at a specified interval, the interval distance being determined by the side length of the honeycomb cells, and coating each strip of glue on the aramid paper of the two-dimensional metamaterial unit into a strip shape, and in a direction perpendicular to the extension of the strip, the width of the strip is one third of the interval distance between two adjacent strips;
[0067] S6 paper stacking step: stacking each layer of the aramid paper of the two-dimensional metamaterial unit, wherein the spacing between two adjacent adhesive strips of the aramid paper of the stacked two-dimensional metamaterial unit is less than 10 mm; stacking the multiple layers of aramid paper of the two-dimensional metamaterial unit coated with adhesive strips in sequence, and staggering all the adhesive strips of the aramid paper of two adjacent layers of the two-dimensional metamaterial unit at equal distances;
[0068] S7 hot pressing step: hot pressing the aramid paper of the glued multi-layer two-dimensional metamaterial unit to obtain a honeycomb laminate;
[0069] S8 stretching process: stretching and shaping the honeycomb laminate, and from the beginning of stretching to the process of stretching and shaping, the honeycomb laminate is kept in a water-spraying state until the honeycomb laminate forms a honeycomb-shaped honeycomb core blank;
[0070] Providing a mixed liquid of reinforcing materials, and spraying the mixed liquid evenly on the honeycomb wall of the honeycomb core blank after stretching and shaping;
[0071] S9 shaping process: after the mixed liquid is sprayed all over the honeycomb wall of the honeycomb core blank, the mixed liquid is immediately placed in an oven for shaping before it dries.
[0072] Between the S7 hot pressing process and the S8 stretching process, there is also an S71 trimming process, which is to trim the honeycomb laminate according to the designed width. The dipping resin mixture in the dipping and curing process includes phenolic resin and organic solvent industrial alcohol, and the mass of the phenolic resin is 50% to 60% of the total mass of the dipping mixture. In the dipping and curing process, the dipping time is 10 minutes to 1 hour, the number of dippings is 1-20 times, and after each dipping, it is preheated in a drying drum at 80 to 120 degrees for 30 to 60 minutes. In the dipping and curing process, after the last dipping is completed, it is cured at a temperature of 130 to 180 degrees for 90 to 240 minutes. The reinforcing material in the stretching process is a mixture of phenolic resin and an organic solvent, and the organic solvent is one or more of ethanol, toluene, acetone, and chloroform.
[0073] The honeycomb core blank after shaping in the oven is further subjected to the following steps to form the three-dimensional microwave absorbing frequency selective material honeycomb core:
[0074] S10 dipping and curing process: providing a dipping resin mixture, stirring it evenly, dipping the honeycomb core blank after being shaped in the oven, and curing the dipping honeycomb core blank after dipping;
[0075] S11 machining process: processing the solidified honeycomb core blank into the three-dimensional wave-absorbing frequency-selective material with the designed structural shape on a honeycomb-specific five-axis machining center.
[0076] Embodiment 3, as Figure 1 , Figure 3 , Figure 6-Figure 8 As shown, a three-dimensional wave absorbing frequency selective material comprises multiple layers of aramid paper printed with two-dimensional metamaterial units, which are mutually staggered and bonded together, and the adjacent two layers of aramid paper of the two-dimensional metamaterial unit are folded into multiple through holes with regular hexagonal cross-sections arranged at intervals, and the aramid paper of the two-dimensional metamaterial unit is obtained by printing the metamaterial structure of different units on paper made of aramid fiber, and each layer of the aramid paper of the two-dimensional metamaterial unit is impregnated with a mixture of phenolic resin and organic solvent, and the side length of the regular hexagonal through hole ranges from 3 to 10 mm. The organic solution is one or more of ethanol, toluene, acetone, and chloroform. The two-dimensional metamaterial unit is printed with an elliptical ring pattern, and the unit printing material is nano-carbon powder, nano-graphene or nano-metal powder. The arrangement direction of the pattern printed on the aramid paper of the two-dimensional metamaterial unit is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°.
[0077] The manufacturing method thereof comprises the following steps:
[0078] S1 material selection process: provide multi-layer aramid paper, which is not allowed to be damaged or have foreign matter that affects the electrical performance;
[0079] S2 printing process: use nano-carbon powder, nano-graphene or various nano-metal powders to print two-dimensional metamaterial units on multi-layer aramid paper, and the printed pattern of the two-dimensional metamaterial unit is an elliptical ring pattern; the long radius of the elliptical ring pattern is 0.1-1.5 mm, the short radius is 0.05-1 mm, and it is evenly arranged vertically and horizontally. The distance between each adjacent group of elliptical rings is 0.1-1.5 mm, which is the long radius of the elliptical ring. The aramid paper of the provided two-dimensional metamaterial unit, wherein the thickness of the nano-carbon powder, nano-graphene or various nano-metal powders corresponding to the printed pattern is 0.05~0.5mm; the arrangement direction of the printed pattern is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15° S3 coating process: cover the front and back sides of each layer of the two-dimensional metamaterial unit aramid paper with a high-temperature resistant gel coat of equal thickness and uniformity;
[0080] S4 curing process: high temperature curing of the aramid paper of all two-dimensional metamaterial units covered with high temperature resistant gel coat;
[0081] S5 glue coating process: coating the aramid paper of each cured two-dimensional metamaterial unit with glue at a specified interval, the interval distance being determined by the side length of the honeycomb cells, and coating each strip of glue on the aramid paper of the two-dimensional metamaterial unit into a strip shape, and in a direction perpendicular to the extension of the strip, the width of the strip is one third of the interval distance between two adjacent strips;
[0082] S6 paper stacking step: stacking each layer of the aramid paper of the two-dimensional metamaterial unit, wherein the spacing between two adjacent adhesive strips of the aramid paper of the stacked two-dimensional metamaterial unit is less than 10 mm; stacking the multiple layers of aramid paper of the two-dimensional metamaterial unit coated with adhesive strips in sequence, and staggering all the adhesive strips of the aramid paper of two adjacent layers of the two-dimensional metamaterial unit at equal distances;
[0083] S7 hot pressing step: hot pressing the aramid paper of the glued multi-layer two-dimensional metamaterial unit to obtain a honeycomb laminate;
[0084] S8 stretching process: stretching and shaping the honeycomb laminate, and from the beginning of stretching to the process of stretching and shaping, the honeycomb laminate is kept in a water-spraying state until the honeycomb laminate forms a honeycomb-shaped honeycomb core blank;
[0085] Providing a mixed liquid of reinforcing materials, and spraying the mixed liquid evenly on the honeycomb wall of the honeycomb core blank after stretching and shaping;
[0086] S9 shaping process: after the mixed liquid is sprayed all over the honeycomb wall of the honeycomb core blank, the mixed liquid is immediately placed in an oven for shaping before it dries.
[0087] Between the S7 hot pressing process and the S8 stretching process, there is also an S71 trimming process, which is to trim the honeycomb laminate according to the designed width. The dipping resin mixture in the dipping and curing process includes phenolic resin and organic solvent industrial alcohol, and the mass of the phenolic resin is 50% to 60% of the total mass of the dipping mixture. In the dipping and curing process, the dipping time is 10 minutes to 1 hour, the number of dippings is 1-20 times, and after each dipping, it is preheated in a drying drum at 80 to 120 degrees for 30 to 60 minutes. In the dipping and curing process, after the last dipping is completed, it is cured at a temperature of 130 to 180 degrees for 90 to 240 minutes. The reinforcing material in the stretching process is a mixture of phenolic resin and an organic solvent, and the organic solvent is one or more of ethanol, toluene, acetone, and chloroform.
[0088] The elliptical ring printed with nano-carbon powder is recorded as sample 4, and its absorption frequency range is 2-8GHz, and the average vertical incidence reflectivity is 8dB; the elliptical ring printed with nano-graphene is recorded as sample 5, and its absorption frequency range is 2-18GHz, and the average vertical incidence reflectivity is 16dB;
[0089] The elliptical ring printed with nano-metal powder is marked as sample 6. This embodiment uses Fe, Co, and Ni alloy powders with an absorption frequency of 3-16 GHz and an average vertical incidence reflectivity of 10 dB.
[0090] Embodiment 4, as Figure 1 , Figure 3 , Figure 6-Figure 8 As shown, a three-dimensional wave absorbing frequency selective material comprises multiple layers of aramid paper printed with two-dimensional metamaterial units, which are mutually staggered and bonded together, and the aramid paper of two adjacent layers of two-dimensional metamaterial units is folded into multiple through holes with regular hexagonal cross-sections arranged at intervals, and the aramid paper of the two-dimensional metamaterial unit is obtained by printing the metamaterial structure of different units on paper made of aramid fiber, and each layer of the aramid paper of the two-dimensional metamaterial unit is impregnated with a mixture of phenolic resin and organic solvent, and the side length of the regular hexagonal through hole ranges from 3 to 10 mm. The organic solution is one or more of ethanol, toluene, acetone, and chloroform. The two-dimensional metamaterial unit prints an elliptical ring pattern, and the unit printing material is nano-carbon powder, nano-graphene or various nano-metal powders. The arrangement direction of the pattern printed on the aramid paper of the two-dimensional metamaterial unit is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°.
[0091] The manufacturing method thereof comprises the following steps:
[0092] S1 material selection process: provide multi-layer aramid paper, which is not allowed to be damaged or have foreign matter that affects the electrical performance;
[0093] S2 printing process: use nano-carbon powder, nano-graphene or nano-metal powder to print two-dimensional metamaterial units on multi-layer aramid paper, and the printed pattern of the two-dimensional metamaterial unit is an elliptical ring pattern; the elliptical ring pattern has a long radius of 0.1-1.5 mm and a short radius of 0.05-1 mm, and is evenly arranged vertically and horizontally. The distance between each two adjacent groups of elliptical rings is 0.1-1.5 mm, which is the long radius of the elliptical ring. The aramid paper of the provided two-dimensional metamaterial unit, wherein the thickness of the nano-carbon powder, nano-graphene or various nano-metal powders corresponding to the printed pattern is 0.05~0.5mm; the arrangement direction of the printed pattern is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°
[0094] S3 coating process: coating the front and back sides of the aramid paper of each layer of the two-dimensional metamaterial unit with a high-temperature resistant gel coat of equal thickness and uniformity; S4 curing process: performing high-temperature curing on the aramid paper of all the two-dimensional metamaterial units covered with the high-temperature resistant gel coat;
[0095] S5 glue coating process: coating the aramid paper of each cured two-dimensional metamaterial unit with glue at a specified interval, the interval distance being determined by the side length of the honeycomb cells, and coating each strip of glue on the aramid paper of the two-dimensional metamaterial unit into a strip shape, and in a direction perpendicular to the extension of the strip, the width of the strip is one third of the interval distance between two adjacent strips;
[0096] S6 paper stacking step: stacking each layer of the aramid paper of the two-dimensional metamaterial unit, wherein the spacing between two adjacent adhesive strips of the aramid paper of the stacked two-dimensional metamaterial unit is less than 10 mm; stacking the multiple layers of aramid paper of the two-dimensional metamaterial unit coated with adhesive strips in sequence, and staggering all the adhesive strips of the aramid paper of two adjacent layers of the two-dimensional metamaterial unit at equal distances;
[0097] S7 hot pressing step: hot pressing the aramid paper of the glued multi-layer two-dimensional metamaterial unit to obtain a honeycomb laminate;
[0098] S8 stretching process: stretching and shaping the honeycomb laminate, and from the beginning of stretching to the process of stretching and shaping, the honeycomb laminate is kept in a water-spraying state until the honeycomb laminate forms a honeycomb-shaped honeycomb core blank;
[0099] Providing a mixed liquid of reinforcing materials, and spraying the mixed liquid evenly on the honeycomb wall of the honeycomb core blank after stretching and shaping;
[0100] S9 shaping process: after the mixed liquid is sprayed all over the honeycomb wall of the honeycomb core blank, the mixed liquid is immediately placed in an oven for shaping before it dries.
[0101] Between the S7 hot pressing process and the S8 stretching process, there is also an S71 trimming process, which is to trim the honeycomb laminate according to the designed width. The dipping resin mixture in the dipping and curing process includes phenolic resin and organic solvent industrial alcohol, and the mass of the phenolic resin is 50% to 60% of the total mass of the dipping mixture. In the dipping and curing process, the dipping time is 10 minutes to 1 hour, the number of dippings is 1-20 times, and after each dipping, it is preheated in a drying drum at 80 to 120 degrees for 30 to 60 minutes. In the dipping and curing process, after the last dipping is completed, it is cured at a temperature of 130 to 180 degrees for 90 to 240 minutes. The reinforcing material in the stretching process is a mixture of phenolic resin and an organic solvent, and the organic solvent is one or more of ethanol, toluene, acetone, and chloroform.
[0102] The honeycomb core blank after shaping in the oven is further subjected to the following steps to form the three-dimensional microwave absorbing frequency selective material honeycomb core:
[0103] S10 dipping and curing process: providing a dipping resin mixture, stirring it evenly, dipping the honeycomb core blank after being shaped in the oven, and curing the dipping honeycomb core blank after dipping;
[0104] S11 machining process: processing the solidified honeycomb core blank into the three-dimensional wave-absorbing frequency-selective material with the designed structural shape on a honeycomb-specific five-axis machining center.
[0105] Embodiment 5, as Figure 1 , Figure 4 , Figure 6-Figure 8 As shown, a three-dimensional wave absorbing frequency selective material comprises multiple layers of aramid paper printed with two-dimensional metamaterial units, which are mutually staggered and bonded together, and the adjacent two layers of aramid paper of the two-dimensional metamaterial unit are folded into multiple through holes with regular hexagonal cross-sections arranged at intervals, and the aramid paper of the two-dimensional metamaterial unit is obtained by printing the metamaterial structure of different units on paper made of aramid fiber, and each layer of the aramid paper of the two-dimensional metamaterial unit is impregnated with a mixture of phenolic resin and organic solvent, and the side length of the regular hexagonal through hole ranges from 3 to 10 mm. The organic solution is one or more of ethanol, toluene, acetone, and chloroform. The two-dimensional metamaterial unit prints a regular hexagonal pattern, and the unit printing material is nano-carbon powder, nano-graphene or nano-metal powder. The arrangement direction of the pattern printed on the aramid paper of the two-dimensional metamaterial unit is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°.
[0106] The manufacturing method thereof comprises the following steps:
[0107] S1 material selection process: provide multi-layer aramid paper, which is not allowed to be damaged or have foreign matter that affects the electrical performance;
[0108] S2 printing process: use nano-carbon powder, nano-graphene or various nano-metal powders to print two-dimensional metamaterial units on multi-layer aramid paper, and the printed pattern of the two-dimensional metamaterial unit is a regular hexagonal pattern; the regular hexagonal pattern has a side length of 0.2-3 mm, and is evenly arranged vertically and horizontally. The spacing between each two adjacent groups of regular hexagons is 0.1-1.5 mm, which is half the side length. The aramid paper of the provided two-dimensional metamaterial unit, wherein the thickness of the nano-carbon powder, nano-graphene or various nano-metal powders corresponding to the printed pattern is 0.05~0.5mm; the arrangement direction of the printed pattern is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°
[0109] S3 coating process: Cover the front and back sides of the aramid paper of each layer of the two-dimensional metamaterial unit with a high-temperature resistant gel coat of equal thickness and uniformity;
[0110] S4 curing process: high temperature curing of all aramid papers of the two-dimensional metamaterial units covered with high temperature resistant gel coats; S5 gluing process: gluing of each layer of the aramid paper of the two-dimensional metamaterial unit after curing at a specified interval, the interval distance being determined by the side length of the honeycomb cells, on the aramid paper of the two-dimensional metamaterial unit, each strip of the glue is coated into a strip shape to form a glue strip, and in the extension direction perpendicular to the glue strip, the width of the glue strip is one third of the interval distance between two adjacent glue strips;
[0111] S6 paper stacking step: stacking each layer of the aramid paper of the two-dimensional metamaterial unit, wherein the spacing between two adjacent adhesive strips of the aramid paper of the stacked two-dimensional metamaterial unit is less than 10 mm; stacking the multiple layers of aramid paper of the two-dimensional metamaterial unit coated with adhesive strips in sequence, and staggering all the adhesive strips of the aramid paper of two adjacent layers of the two-dimensional metamaterial unit at equal distances;
[0112] S7 hot pressing step: hot pressing the aramid paper of the glued multi-layer two-dimensional metamaterial unit to obtain a honeycomb laminate;
[0113] S8 stretching process: stretching and shaping the honeycomb laminate, and from the beginning of stretching to the process of stretching and shaping, the honeycomb laminate is kept in a water-spraying state until the honeycomb laminate forms a honeycomb-shaped honeycomb core blank;
[0114] Providing a mixed liquid of reinforcing materials, and spraying the mixed liquid evenly on the honeycomb wall of the honeycomb core blank after stretching and shaping;
[0115] S9 shaping process: after the mixed liquid is sprayed all over the honeycomb wall of the honeycomb core blank, the mixed liquid is immediately placed in an oven for shaping before it dries.
[0116] Between the S7 hot pressing process and the S8 stretching process, there is also an S71 trimming process, which is to trim the honeycomb laminate according to the designed width. The dipping resin mixture in the dipping and curing process includes phenolic resin and organic solvent industrial alcohol, and the mass of the phenolic resin is 50% to 60% of the total mass of the dipping mixture. In the dipping and curing process, the dipping time is 10 minutes to 1 hour, the number of dippings is 1-20 times, and after each dipping, it is preheated in a drying drum at 80 to 120 degrees for 30 to 60 minutes. In the dipping and curing process, after the last dipping is completed, it is cured at a temperature of 130 to 180 degrees for 90 to 240 minutes. The reinforcing material in the stretching process is a mixture of phenolic resin and an organic solvent, and the organic solvent is one or more of ethanol, toluene, acetone, and chloroform.
[0117] Among them, the hexagon printed with nano-carbon powder is recorded as sample 7, and its absorption frequency range is 2-8GHz, and the average vertical incidence reflectivity is 16dB; the hexagon printed with nano-graphene is recorded as sample 8, and its absorption frequency is 2-18GHz, and the average vertical incidence reflectivity is 22dB;
[0118] The regular hexagon printed with nano-metal powder is recorded as sample 9. This embodiment uses Fe, Co, and Ni alloy powders with an absorption frequency of 3-16 GHz and an average vertical incidence reflectivity of 15 dB.
[0119] Embodiment 6, as Figure 1 , Figure 4 , Figure 6-Figure 8 As shown, a three-dimensional wave absorbing frequency selective material comprises multiple layers of aramid paper printed with two-dimensional metamaterial units, which are mutually staggered and bonded together, and the adjacent two layers of aramid paper of the two-dimensional metamaterial unit are folded into multiple through holes with regular hexagonal cross-sections arranged at intervals, and the aramid paper of the two-dimensional metamaterial unit is obtained by printing the metamaterial structure of different units on paper made of aramid fiber, and each layer of the aramid paper of the two-dimensional metamaterial unit is impregnated with a mixture of phenolic resin and organic solvent, and the side length of the regular hexagonal through hole ranges from 3 to 10 mm. The organic solution is one or more of ethanol, toluene, acetone, and chloroform. The two-dimensional metamaterial unit prints a regular hexagonal pattern, and the unit printing material is nano-carbon powder, nano-graphene or nano-metal powder. The arrangement direction of the pattern printed on the aramid paper of the two-dimensional metamaterial unit is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°.
[0120] The manufacturing method thereof comprises the following steps:
[0121] S1 material selection process: provide multi-layer aramid paper, which is not allowed to be damaged or have foreign matter that affects the electrical performance;
[0122] S2 printing process: use nano-carbon powder, nano-graphene or various nano-metal powders to print two-dimensional metamaterial units on multi-layer aramid paper, and the printed pattern of the two-dimensional metamaterial unit is a regular hexagonal pattern; the regular hexagonal pattern has a side length of 0.2-3 mm, and is evenly arranged vertically and horizontally. The spacing between each two adjacent groups of regular hexagons is 0.1-1.5 mm, which is half the side length. The aramid paper of the provided two-dimensional metamaterial unit, wherein the thickness of the nano-carbon powder, nano-graphene or various nano-metal powders corresponding to the printed pattern is 0.05~0.5mm; the arrangement direction of the printed pattern is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°
[0123] S3 coating process: Cover the front and back sides of the aramid paper of each layer of the two-dimensional metamaterial unit with a high-temperature resistant gel coat of equal thickness and uniformity;
[0124] S4 curing process: high temperature curing of the aramid paper of all two-dimensional metamaterial units covered with high temperature resistant gel coat;
[0125] S5 glue coating process: coating the aramid paper of each cured two-dimensional metamaterial unit with glue at a specified interval, the interval distance being determined by the side length of the honeycomb cells, and coating each strip of glue on the aramid paper of the two-dimensional metamaterial unit into a strip shape, and in a direction perpendicular to the extension of the strip, the width of the strip is one third of the interval distance between two adjacent strips;
[0126] S6 paper stacking step: stacking each layer of the aramid paper of the two-dimensional metamaterial unit, wherein the spacing between two adjacent adhesive strips of the aramid paper of the stacked two-dimensional metamaterial unit is less than 10 mm; stacking the multiple layers of aramid paper of the two-dimensional metamaterial unit coated with adhesive strips in sequence, and staggering all the adhesive strips of the aramid paper of two adjacent layers of the two-dimensional metamaterial unit at equal distances;
[0127] S7 hot pressing step: hot pressing the aramid paper of the glued multi-layer two-dimensional metamaterial unit to obtain a honeycomb laminate;
[0128] S8 stretching process: stretching and shaping the honeycomb laminate, and from the beginning of stretching to the process of stretching and shaping, the honeycomb laminate is kept in a water-spraying state until the honeycomb laminate forms a honeycomb-shaped honeycomb core blank;
[0129] Providing a mixed liquid of reinforcing materials, and spraying the mixed liquid evenly on the honeycomb wall of the honeycomb core blank after stretching and shaping;
[0130] S9 shaping process: after the mixed liquid is sprayed all over the honeycomb wall of the honeycomb core blank, the mixed liquid is immediately placed in an oven for shaping before it dries.
[0131] Between the S7 hot pressing process and the S8 stretching process, there is also an S71 trimming process, which is to trim the honeycomb laminate according to the designed width. The dipping resin mixture in the dipping and curing process includes phenolic resin and organic solvent industrial alcohol, and the mass of the phenolic resin is 50% to 60% of the total mass of the dipping mixture. In the dipping and curing process, the dipping time is 10 minutes to 1 hour, the number of dippings is 1-20 times, and after each dipping, it is preheated in a drying drum at 80 to 120 degrees for 30 to 60 minutes. In the dipping and curing process, after the last dipping is completed, it is cured at a temperature of 130 to 180 degrees for 90 to 240 minutes. The reinforcing material in the stretching process is a mixture of phenolic resin and an organic solvent, and the organic solvent is one or more of ethanol, toluene, acetone, and chloroform.
[0132] The honeycomb core blank after shaping in the oven is further subjected to the following steps to form the three-dimensional microwave absorbing frequency selective material honeycomb core:
[0133] S10 dipping and curing process: providing a dipping resin mixture, stirring it evenly, dipping the honeycomb core blank after being shaped in the oven, and curing the dipping honeycomb core blank after dipping;
[0134] S11 machining process: processing the solidified honeycomb core blank into the three-dimensional wave-absorbing frequency-selective material with the designed structural shape on a honeycomb-specific five-axis machining center.
[0135] Embodiment 7, as Figure 1 , Figure 5 , Figure 6-Figure 8 As shown, a three-dimensional wave absorbing frequency selective material comprises multiple layers of aramid paper printed with two-dimensional metamaterial units, which are mutually staggered and bonded together, and the adjacent two layers of aramid paper of the two-dimensional metamaterial unit are folded into multiple through holes with regular hexagonal cross-sections arranged at intervals, and the aramid paper of the two-dimensional metamaterial unit is obtained by printing the metamaterial structure of different units on paper made of aramid fiber, and each layer of the aramid paper of the two-dimensional metamaterial unit is impregnated with a mixture of phenolic resin and organic solvent, and the side length of the regular hexagonal through hole ranges from 3 to 10 mm. The organic solution is one or more of ethanol, toluene, acetone, and chloroform. The two-dimensional metamaterial unit is printed with a regular triangle pattern, and the unit printing material is nano-carbon powder, nano-graphene or various nano-metal powders. The arrangement direction of the pattern printed on the aramid paper of the two-dimensional metamaterial unit is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°.
[0136] The manufacturing method thereof comprises the following steps:
[0137] S1 material selection process: provide multi-layer aramid paper, which is not allowed to be damaged or have foreign matter that affects the electrical performance;
[0138] S2 printing process: use nano-carbon powder, nano-graphene or nano-metal powder to print two-dimensional metamaterial units on multi-layer aramid paper, and the printed pattern of the two-dimensional metamaterial unit is an equilateral triangle pattern; the side length of the equilateral triangle pattern is 0.2-3 mm, and it is evenly arranged vertically and horizontally. The distance between each adjacent two groups of equilateral triangles is 0.1-1.5 mm, which is half of the side length. The aramid paper of the provided two-dimensional metamaterial unit, wherein the thickness of the nano-carbon powder, nano-graphene or various nano-metal powders corresponding to the printed pattern is 0.05~0.5mm; the arrangement direction of the printed pattern is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°
[0139] S3 coating process: Cover the front and back sides of the aramid paper of each layer of the two-dimensional metamaterial unit with a high-temperature resistant gel coat of equal thickness and uniformity;
[0140] S4 curing process: high temperature curing of the aramid paper of all two-dimensional metamaterial units covered with high temperature resistant gel coat;
[0141] S5 glue coating process: coating the aramid paper of each cured two-dimensional metamaterial unit with glue at a specified interval, the interval distance being determined by the side length of the honeycomb cells, and coating each strip of glue on the aramid paper of the two-dimensional metamaterial unit into a strip shape, and in a direction perpendicular to the extension of the strip, the width of the strip is one third of the interval distance between two adjacent strips;
[0142] S6 paper stacking step: stacking each layer of the aramid paper of the two-dimensional metamaterial unit, wherein the spacing between two adjacent adhesive strips of the aramid paper of the stacked two-dimensional metamaterial unit is less than 10 mm; stacking the multiple layers of aramid paper of the two-dimensional metamaterial unit coated with adhesive strips in sequence, and staggering all the adhesive strips of the aramid paper of two adjacent layers of the two-dimensional metamaterial unit at equal distances;
[0143] S7 hot pressing step: hot pressing the aramid paper of the glued multi-layer two-dimensional metamaterial unit to obtain a honeycomb laminate;
[0144] S8 stretching process: stretching and shaping the honeycomb laminate, and from the beginning of stretching to the process of stretching and shaping, the honeycomb laminate is kept in a water-spraying state until the honeycomb laminate forms a honeycomb-shaped honeycomb core blank;
[0145] Providing a mixed liquid of reinforcing materials, and spraying the mixed liquid evenly on the honeycomb wall of the honeycomb core blank after stretching and shaping;
[0146] S9 shaping process: after the mixed liquid is sprayed all over the honeycomb wall of the honeycomb core blank, the mixed liquid is immediately placed in an oven for shaping before it dries.
[0147] Between the S7 hot pressing process and the S8 stretching process, there is also an S71 trimming process, which is to trim the honeycomb laminate according to the designed width. The dipping resin mixture in the dipping and curing process includes phenolic resin and organic solvent industrial alcohol, and the mass of the phenolic resin is 50% to 60% of the total mass of the dipping mixture. In the dipping and curing process, the dipping time is 10 minutes to 1 hour, the number of dippings is 1-20 times, and after each dipping, it is preheated in a drying drum at 80 to 120 degrees for 30 to 60 minutes. In the dipping and curing process, after the last dipping is completed, it is cured at a temperature of 130 to 180 degrees for 90 to 240 minutes. The reinforcing material in the stretching process is a mixture of phenolic resin and an organic solvent, and the organic solvent is one or more of ethanol, toluene, acetone, and chloroform.
[0148] The equilateral triangle printed with nano-carbon powder is sample 10, and its absorption frequency range is 2-8GHz, and its average vertical incidence reflectivity is 14dB; the equilateral triangle printed with nano-graphene is sample 11, and its absorption frequency range is 2-18GHz, and its average vertical incidence reflectivity is 18dB;
[0149] The equilateral triangle printed with nano-metal powder is recorded as sample 12. This embodiment uses Fe, Co, and Ni alloy powders with an absorption frequency of 3-16 GHz and an average vertical incidence reflectivity of 12 dB.
[0150] Embodiment 8, as Figure 1 , Figure 5, Figure 6-Figure 8 As shown, a three-dimensional wave absorbing frequency selective material comprises multiple layers of aramid paper printed with two-dimensional metamaterial units, which are mutually staggered and bonded together, and the aramid paper of two adjacent layers of two-dimensional metamaterial units is folded into multiple through holes with regular hexagonal cross-sections arranged at intervals, and the aramid paper of the two-dimensional metamaterial unit is obtained by printing the metamaterial structure of different units on paper made of aramid fiber, and each layer of the aramid paper of the two-dimensional metamaterial unit is impregnated with a mixture of phenolic resin and organic solvent, and the side length of the regular hexagonal through hole ranges from 3 to 10 mm. The organic solution is one or more of ethanol, toluene, acetone, and chloroform. The two-dimensional metamaterial unit is printed with a regular triangle pattern, and the unit printing material is nano-carbon powder, nano-graphene or nano-metal powder. The arrangement direction of the pattern printed on the aramid paper of the two-dimensional metamaterial unit is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°.
[0151] The manufacturing method thereof comprises the following steps:
[0152] S1 material selection process: provide multi-layer aramid paper, which is not allowed to be damaged or have foreign matter that affects the electrical performance;
[0153] S2 printing process: use nano-carbon powder, nano-graphene or various nano-metal powders to print two-dimensional metamaterial units on multi-layer aramid paper, and the printed pattern of the two-dimensional metamaterial unit is an equilateral triangle pattern; the side length of the equilateral triangle pattern is 0.2-3 mm, and it is evenly arranged vertically and horizontally. The distance between each adjacent two groups of equilateral triangles is 0.1-1.5 mm, which is half of the side length. The aramid paper of the provided two-dimensional metamaterial unit, wherein the thickness of the nano-carbon powder, nano-graphene or various nano-metal powders corresponding to the printed pattern is 0.05~0.5mm; the arrangement direction of the printed pattern is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°
[0154] S3 coating process: Cover the front and back sides of the aramid paper of each layer of the two-dimensional metamaterial unit with a high-temperature resistant gel coat of equal thickness and uniformity;
[0155] S4 curing process: high temperature curing of the aramid paper of all two-dimensional metamaterial units covered with high temperature resistant gel coat;
[0156] S5 glue coating process: coating the aramid paper of each cured two-dimensional metamaterial unit with glue at a specified interval, the interval distance being determined by the side length of the honeycomb cells, and coating each strip of glue on the aramid paper of the two-dimensional metamaterial unit into a strip shape, and in a direction perpendicular to the extension of the strip, the width of the strip is one third of the interval distance between two adjacent strips;
[0157] S6 paper stacking step: stacking each layer of the aramid paper of the two-dimensional metamaterial unit, wherein the spacing between two adjacent adhesive strips of the aramid paper of the stacked two-dimensional metamaterial unit is less than 10 mm; stacking the multiple layers of aramid paper of the two-dimensional metamaterial unit coated with adhesive strips in sequence, and staggering all the adhesive strips of the aramid paper of two adjacent layers of the two-dimensional metamaterial unit at equal distances;
[0158] S7 hot pressing step: hot pressing the aramid paper of the glued multi-layer two-dimensional metamaterial unit to obtain a honeycomb laminate;
[0159] S8 stretching process: stretching and shaping the honeycomb laminate, and from the beginning of stretching to the process of stretching and shaping, the honeycomb laminate is kept in a water-spraying state until the honeycomb laminate forms a honeycomb-shaped honeycomb core blank;
[0160] Providing a mixed liquid of reinforcing materials, and spraying the mixed liquid evenly on the honeycomb wall of the honeycomb core blank after stretching and shaping;
[0161] S9 shaping process: after the mixed liquid is sprayed all over the honeycomb wall of the honeycomb core blank, the mixed liquid is immediately placed in an oven for shaping before it dries.
[0162] Between the S7 hot pressing process and the S8 stretching process, there is also an S71 trimming process, which is to trim the honeycomb laminate according to the designed width. The dipping resin mixture in the dipping and curing process includes phenolic resin and organic solvent industrial alcohol, and the mass of the phenolic resin is 50% to 60% of the total mass of the dipping mixture. In the dipping and curing process, the dipping time is 10 minutes to 1 hour, the number of dippings is 1-20 times, and after each dipping, it is preheated in a drying drum at 80 to 120 degrees for 30 to 60 minutes. In the dipping and curing process, after the last dipping is completed, it is cured at a temperature of 130 to 180 degrees for 90 to 240 minutes. The reinforcing material in the stretching process is a mixture of phenolic resin and an organic solvent, and the organic solvent is one or more of ethanol, toluene, acetone, and chloroform.
[0163] The honeycomb core blank after shaping in the oven is further subjected to the following steps to form the three-dimensional microwave absorbing frequency selective material honeycomb core:
[0164] S10 dipping and curing process: providing a dipping resin mixture, stirring it evenly, dipping the honeycomb core blank after being shaped in the oven, and curing the dipping honeycomb core blank after dipping;
[0165] S11 machining process: processing the solidified honeycomb core blank into the three-dimensional wave-absorbing frequency-selective material with the designed structural shape on a honeycomb-specific five-axis machining center.
[0166] The wave absorption properties of samples 1-12 in the above embodiments and samples prepared in CN115603058A as comparative example 1 are shown in Table 1:
[0167] Absorption frequency(GHz) Average vertical incidence reflectivity (db) Sample 1 2-8 10.2 Sample 2 2-18 20.6 Sample 3 3-16 13.5 Sample 4 2-8 8.8 Sample 5 2-18 16.5 Sample 6 3-16 10.6 Sample 7 2-8 16.2 Sample 8 2-18 22.6 Sample 9 3-16 15.7 Sample 10 2-8 14.2 Sample 11 2-18 18.3 Sample 12 3-16 12.5 Comparative Example 1 2-6.4 9.8
[0168] Table 1
[0169] It can be seen from Table 1 that samples 1-12 prepared by the present invention have a wider absorption frequency than the samples prepared by CN CN115603058A, and the absorption performance is stronger than that of the comparative example except sample 4; from the present invention 1-12, the absorption frequency is related to the material used for printing, and in terms of materials, nanographene>nanometal powder>nanocarbon powder; from the attenuation performance, the printed pattern shape is regular hexagon>equilateral triangle>circle>ellipse.
[0170] The thickness of the printed pattern of the two-dimensional metamaterial unit of the present invention is 0.05~0.5mm. The printing thickness of sample 8 is 0.1, 0.2, 0.5, and 1mm, respectively. The average vertical incidence reflectivity is 20.1db, 21.2db, 22.6db, and 19.8db, respectively. It can be seen from the above that the average vertical incidence reflectivity is related to the printing material as well as the printing thickness, and printing 0.05~0.5mm is the best.
[0171] Plane compressive strength at 300℃ (MPa) L-axis shear strength at 300°C (MPa) W-axis shear strength at 300°C (MPa) Sample 1 3.16 2.15 0.98 Sample 2 3.29 2.23 0.97 Sample 3 3.18 2.16 1.08 Sample 4 3.21 2.24 1.03 Sample 5 3.22 2.15 1.06 Sample 6 3.20 2.08 1.03 Sample 7 3.13 2.15 1.01 Sample 8 3.14 2.20 1.03 Sample 9 3.22 2.28 0.97 Sample 10 3.08 2.12 1.03 Sample 11 3.16 2.09 1.02 Sample 12 3.22 2.15 1.05 Comparative Example 1 3.08 1.96 0.89
[0172] Table 2
[0173] It can be seen from Table 2 that samples 1-12 prepared by the present invention have better high temperature resistance and mechanical properties than comparative example 1.
[0174] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
Claims
1. A method for manufacturing a three-dimensional wave absorbing frequency selective material, characterized in that: The steps include: Material selection process: provide multi-layer aramid paper, which is not allowed to be damaged or have foreign matter that affects the electrical performance; Printing process: using nano-carbon powder, nano-graphene or nano-metal powder to print two-dimensional metamaterial units on multi-layer aramid paper, the printed pattern of the two-dimensional metamaterial unit is a circular ring, an elliptical ring or a regular polygonal pattern; The thickness of the nano-carbon powder, nano-graphene or nano-metal powder corresponding to the printed pattern is 0.05-0.5 mm; the arrangement direction of the printed pattern is consistent with the fiber distribution direction in the aramid paper, and the angle range is ±15°; Glue coating process: the front and back sides of the aramid paper of each layer of the two-dimensional metamaterial unit are covered with a high-temperature resistant gel coat of equal thickness and uniformity; in the glue coating process, the front and back sides of the aramid paper of each layer of the two-dimensional metamaterial unit are covered with a high-temperature resistant gel coat of equal thickness and uniformity, which is at least one of cyanate ester, bismaleimide resin or polyimide resin, and the gel coat thickness is ≤0.5mm; Curing process: high temperature curing of the aramid paper of all two-dimensional metamaterial units covered with high temperature resistant gel coat; Gluing process: Gluing is performed at designated intervals on the aramid paper of each cured two-dimensional metamaterial unit, and the interval distance is determined by the side length of the honeycomb cells. On the aramid paper of the two-dimensional metamaterial unit, each strip of the glue is coated into a strip shape to form a glue strip, and in the direction perpendicular to the extension of the glue strip, the width of the glue strip is one third of the interval distance between two adjacent glue strips; Paper stacking process: stacking each layer of the aramid paper of the two-dimensional metamaterial unit, wherein the spacing between two adjacent adhesive strips of the aramid paper of the stacked two-dimensional metamaterial unit is less than 10 mm; stacking the multiple layers of aramid paper of the two-dimensional metamaterial unit coated with adhesive strips in sequence, and staggering all the adhesive strips of the aramid paper of two adjacent layers of the two-dimensional metamaterial unit at equal distances; Hot pressing process: hot pressing the glued multi-layer two-dimensional metamaterial unit aramid paper to obtain a honeycomb laminate; Stretching process: stretching and shaping the honeycomb laminate, and from the beginning of stretching to the process of stretching and shaping, the honeycomb laminate is kept in a water-spraying state until the honeycomb laminate forms a honeycomb-shaped honeycomb core blank; Providing a mixed liquid of reinforcing materials, and spraying the mixed liquid evenly on the honeycomb wall of the honeycomb core blank after stretching and shaping; Shaping process: after the mixed liquid is sprayed all over the honeycomb wall of the honeycomb core blank, the mixed liquid is immediately placed in an oven for shaping before it dries; The honeycomb core blank after shaping in the oven is further subjected to the following steps to form the three-dimensional microwave absorbing frequency selective material honeycomb core: Dipping and curing process: providing a dipping resin mixture, stirring it evenly, dipping the honeycomb core blank after being shaped in the oven, and curing the dipping honeycomb core blank after dipping; Machining process: The solidified honeycomb core blank is processed into the three-dimensional wave-absorbing frequency-selective material with a designed structural shape on a honeycomb-specific five-axis machining center.
2. The method for manufacturing a three-dimensional wave absorbing frequency selective material according to claim 1, characterized in that: Between the hot pressing process and the stretching process, there is also a trimming process, in which the honeycomb laminate is trimmed according to the designed width.
3. The method for manufacturing a three-dimensional wave absorbing frequency selective material according to claim 1, characterized in that: In the dipping and curing process, the dipping resin mixed liquid comprises phenolic resin and organic solvent industrial alcohol, and the mass of the phenolic resin accounts for 50% to 60% of the total mass of the dipping mixed liquid.
4. The method for manufacturing a three-dimensional wave absorbing frequency selective material according to claim 1, characterized in that: In the dipping and curing process, the dipping time is 10 minutes to 1 hour, the dipping times are 1-20 times, and after each dipping, it is preheated in a drying drum at 80 to 120 degrees for 30 to 60 minutes.
5. The method for manufacturing a three-dimensional wave absorbing frequency selective material according to claim 1 or 4, characterized in that: In the dipping and curing process, after the last dipping, curing is carried out at a temperature of 130 to 180 degrees for 90 to 240 minutes.
6. The method for manufacturing a three-dimensional wave absorbing frequency selective material according to claim 1, characterized in that: The reinforcing material in the stretching process is a mixture of phenolic resin and an organic solvent, and the organic solvent is one or more of ethanol, toluene, acetone and chloroform.
Citation Information
Patent Citations
Three-dimensional metamaterial based on honeycomb structure and preparation method thereof
CN115603058A
Low-cost paper honeycomb core and manufacturing method thereof
CN108177393A
Manufacturing method of honeycomb composite structure for absorbing electromagnetic waves using screen printing and honeycomb composite structure manufactured by the manufacturing method
KR102562499B1