A highly flame-retardant, foldable, heat-insulating double-sided spray-painted material and its preparation process and application

By using a base fabric layer and multi-layer coating structure blended with polyester chemical fiber and glass fiber in the spraying material, combined with silicone modified water-based polyurethane and nanomaterials, the existing spraying materials cannot meet both double-sided printing and high flame retardant at the same time. and the problem of heat insulation, the spray painted material with high flame retardancy, soft foldable and good thermal insulation effect is achieved.

CN117341374BActive Publication Date: 2024-12-03WEIFANG JIACHENG DIGITAL MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311095034.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-29
Publication Date
2024-12-03
Estimated Expiration
2043-08-29

AI Technical Summary

Technical Problem

Existing sprayed materials cannot meet both double-sided printing, high flame retardant performance and good thermal insulation performance, and traditional sprayed materials have poor flame retardant performance, which cannot meet the simultaneous needs of foldable and thermal insulation.

Method used

Using a combined structure of base fabric layer and composite coating, the base fabric layer is made of polyester chemical fiber and glass fiber, and is made of multi-layer coating (hand feel coating, adhesion enhancement coating, thermal insulation coating, waterproof coating ) The flame retardant, thermal insulation and printing properties of reinforced materials, including the use of silicone modified aqueous polyurethane, nanomaterials and microsphere foaming technology.

Benefits of technology

It achieves high flame retardancy, soft foldable, double-sided printing and good thermal insulation, while improving the wrinkle resistance and dimensional stability of the material, enhancing the prospects of industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117341374B_ABST
    Figure CN117341374B_ABST
Patent Text Reader

Abstract

The present invention discloses a highly flame-retardant, foldable, heat-insulating double-sided inkjet material and its preparation process, belonging to the technical field of inkjet materials. The inkjet material comprises two base fabric layers and a composite coating, and a single side of each base fabric layer is coated with a hand-feel coating, an adhesion enhancement coating, a heat-insulating coating I, a heat-insulating coating II, and a waterproof inkjet coating in sequence; the composite coating is used to composite the uncoated sides of the two base fabric layers. The highly flame-retardant, foldable, heat-insulating double-sided inkjet material of the present application has high flame retardancy, is soft and foldable, has good heat-insulating effect, and can be printed with UV, weak solvent, and Latex inks on both sides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inkjet printing materials, and in particular relates to a highly flame-retardant, foldable, heat-insulating double-sided inkjet printing material and a preparation process thereof. Background Art

[0002] Inkjet printing technology has been widely used in the advertising industry. Its rich color expression, fast production process, and long-lasting sun resistance have brought vitality to the entire industry. At present, the competition in the advertising industry is becoming more and more fierce, and higher and higher requirements are placed on inkjet printing material manufacturers.

[0003] Chinese patent number CN115220295A discloses a foldable optical curtain and its preparation method, comprising a chemical fiber cloth layer, a foaming anti-wrinkle layer, a silver stamping layer and an optical functional layer, wherein the foaming anti-wrinkle layer is arranged above the chemical fiber cloth layer, the silver stamping layer is arranged above the foaming anti-wrinkle layer, and the optical functional layer is arranged above the silver stamping layer; the foaming anti-wrinkle layer is prepared from the following raw materials by mass percentage: 40-45% textile emulsion, 2-5% foaming agent, 9-12% foam stabilizer, 10-15% kaolin, 10-15% titanium dioxide dispersion, and 20-25% composite flame retardant. The curtain is foldable, lightweight, environmentally friendly, and anti-oxidant, and increases the viewing angle and improves the viewing range of the optical curtain.

[0004] However, the above-mentioned foldable curtains have the following problems: (1) New chemical fiber cloth advertising cloths can generally only meet single-sided printing, and cannot simultaneously meet double-sided printing and customer requirements for different inks; (2) Existing inkjet printing materials have poor flame retardancy; (3) Existing inkjet printing materials cannot simultaneously meet the requirements of foldability and good thermal insulation performance. Therefore, in view of the above problems, it is necessary to develop a highly flame retardant, foldable, thermally insulating double-sided inkjet printing material, and at the same time establish a corresponding preparation process. Summary of the invention

[0005] In view of the defects existing in the prior art, the purpose of the present invention is to provide a highly flame-retardant, foldable, heat-insulating double-sided printing material and its preparation process. The printing material has high flame retardancy, is soft and foldable, has good heat insulation effect, and can be printed on both sides with UV, weak solvent, and Latex ink.

[0006] On the one hand, the present invention provides a highly flame-retardant, foldable, heat-insulating, double-sided spray-painted material, the spray-painted material comprising a base fabric layer and a composite coating, a single side of the base fabric layer being coated with a hand-feel coating, an adhesion enhancing coating, a heat-insulating coating I, a heat-insulating coating II, and a waterproof spray-painted coating in sequence; the composite coating composites the uncoated side of the base fabric layer.

[0007] Another aspect of the present invention provides a preparation process of a highly flame-retardant, foldable, heat-insulating, double-sided spray-painted material, the preparation process comprising the following steps:

[0008] (1) Preparation of base fabric layer

[0009] 40%-50% polyester chemical fiber yarn and 50%-60% glass fiber are mixed and spun, and then shaped;

[0010] (2) Preparation of hand-feel coating

[0011] 30-50 parts of silicone-modified waterborne polyurethane, 100 parts of water, and 3-10 parts of cellulose are mixed evenly by weight, coated on one side of the base fabric layer by screen coating, and then cross-linked and cured to form a hand-feel coating;

[0012] (3) Preparation of adhesion enhancing coating

[0013] 50-100 parts of an aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 6-10 parts of an alkali swelling and associative compound thickener, and 0.6-1 part of a defoamer are mixed uniformly according to weight parts, the viscosity is adjusted, and the mixture is applied on the surface of the hand-feel coating by a doctor blade coating method, dried and cured to form an adhesion-enhancing coating;

[0014] (4) Preparation of thermal insulation coating I

[0015] 200-300 parts of water-based acrylic self-crosslinking textile emulsion with a TG value of -30°C to -15°C, 200-300 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 40-60 parts of nano-silicon dioxide aerogel powder, 20-40 parts of nano-glass microbeads, 20-40 parts of core-shell titanium dioxide, and 12-20 parts of microsphere foaming agent are mixed uniformly according to weight parts, the pH is adjusted to 7-8, the viscosity is adjusted, and the coating is applied on the surface of the adhesion enhancing coating by an E-type knife gap coating method, dried and cured, and then foamed at 190-210°C to form a heat insulation coating I;

[0016] (5) Preparation of thermal insulation coating II

[0017] According to weight parts, 200-300 parts of water-based acrylic self-crosslinking textile emulsion with a TG value of -30°C to -15°C, 200-300 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 40-60 parts of nano-silicon dioxide aerogel powder, 20-40 parts of nano-glass microbeads, 20-40 parts of core-shell titanium dioxide, and 12-20 parts of microsphere foaming agent are mixed evenly, the pH is adjusted to 7-8, the viscosity is adjusted, and then the mixture is coated on the surface of the thermal insulation coating I by an E-type knife gap coating method, dried and cured, and then foamed at 190-210°C to form a thermal insulation coating II;

[0018] (6) Preparation of waterproof spray coating

[0019] 100-200 parts of organosilicon-modified waterborne polyurethane emulsion with a TG value of 5°C-20°C, 60-200 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 5-15 parts of nano-silicon dioxide, 5-10 parts of nano-modified wax powder, 3-6 parts of polyurethane thickener, and 0.6-1 part of defoamer are mixed evenly according to weight parts, and after adjusting the viscosity, the mixture is applied on the surface of the thermal insulation coating II by a doctor blade coating method, and then cured to form a waterproof spray coating;

[0020] (7) Preparation of composite coating

[0021] 100-200 parts of aqueous polyurethane emulsion with a TG value of 5°C-20°C and 10-30 parts of low melting point PA powder are mixed evenly according to weight, and the viscosity is adjusted. The uncoated sides of the two base fabric layers are laminated by roller heating using a laminating machine.

[0022] On the other hand, the present invention provides a highly flame-retardant, foldable, thermally insulating double-sided spray-painted material as described above and its preparation process, and / or the use of the highly flame-retardant, foldable, thermally insulating double-sided spray-painted material obtained by the highly flame-retardant, foldable, thermally insulating double-sided spray-painted material and its preparation process in thermal insulation materials for thermal insulation tents, simple steel structure houses, and indoor and outdoor advertising.

[0023] The beneficial effects of the present invention include at least one of the following:

[0024] 1. The highly flame-retardant, foldable, heat-insulating, double-sided inkjet printing material provided by the present invention has a base fabric layer made of polyester chemical fiber and glass fiber blended in a customized manner, which enhances the fire resistance of the base material, improves the product's good folding resistance, and gives the product good dimensional stability through a 220°C high-temperature shaping method;

[0025] 2. The highly flame-retardant, foldable, heat-insulating double-sided spray-painted material provided by the present invention has a hand-feel coating layer comprising silicone-modified water-based polyurethane, which is coated on the surface of the base fabric layer by screen coating, thereby reducing the penetration of latex. Through cross-linking and curing treatment, the material is further provided with good flexibility and folding resistance, thereby achieving foldability of the material;

[0026] 3. The highly flame-retardant, foldable, heat-insulating double-sided spray-painted material provided by the present invention has an adhesion-enhancing coating that is coated with a high-viscosity aqueous polyurethane emulsion, which effectively prevents the latex from penetrating the yarn of the base fabric layer, and after the coating is cross-linked and cured, the coating has a strong adhesion to the yarn, further providing adhesion for the heat-insulating coating I;

[0027] 4. The highly flame-retardant foldable heat-insulating double-sided spray-painted material provided by the present invention, the heat-insulating coating I and the heat-insulating coating II form a microporous structure through the microsphere foaming technology, which increases the thickness of the material and has a better feel, and provides a good heat-insulating effect for the material. The coating further improves the heat-insulating effect of the product by compounding nano-silicon dioxide aerogel powder and nano-glass microbeads. At the same time, the coating provides a good flame-retardant effect for the product by compounding modified aluminum hydroxide, antimony trioxide, and decabromodiphenylethane flame retardant;

[0028] 5. The highly flame-retardant, foldable, heat-insulating double-sided inkjet printing material provided by the present invention has a waterproof inkjet printing coating, which gives the material a good water-repellent effect by adding modified polyurethane emulsion and nano wax powder, effectively preventing rainwater from infiltrating, and provides a printing coating for UV, weak solvent, and Latex ink, achieving the effects of isolating rainwater and being printable, thereby increasing the practicality of the material;

[0029] 6. The structure of the highly flame-retardant, foldable, heat-insulating, double-sided printing material provided by the present invention can provide better heat insulation and flame-retardant effects and realize double-sided printing without color difference by compounding the coated base fabric layer;

[0030] 7. The preparation process of the present invention adopts batch raw materials and industrial equipment, has strong versatility, is easy to mass produce, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The cross-sectional structure diagram of a highly flame-retardant, foldable, heat-insulating, double-sided spray-painted material of the present invention is shown.

[0032] List of parts and reference numerals:

[0033] 1-base fabric layer, 2-hand-feel coating, 3-adhesion enhancing coating, 4-thermal insulation coating I, 5-thermal insulation coating II, 6-waterproof spray coating, 7-composite coating. DETAILED DESCRIPTION

[0034] In order to more clearly illustrate the overall concept of the present invention, a detailed description is given below by way of examples.

[0035] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0036] In addition, in the description of the invention, it should be understood that the terms "top", "bottom", "inside", "outside", "axial", "radial", "circumferential", etc., indicating orientations or positional relationships, are for the convenience of describing the present invention, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0037] In the invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or a communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the invention can be understood according to specific circumstances.

[0038] In the present invention, unless otherwise clearly specified and limited, the first feature "on" or "under" the second feature may be that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in an appropriate manner in any one or more embodiments or examples.

[0039] Hereinafter, the highly flame-retardant, foldable, heat-insulating, double-sided spray-painted material and the preparation process thereof of the present invention will be described in detail in conjunction with exemplary embodiments.

[0040] In an exemplary embodiment of the present invention, a highly flame-retardant, foldable, heat-insulating, double-sided spray-painted material comprises a base fabric layer and a composite coating, wherein a single side of the base fabric layer is sequentially coated with a hand-feel coating, an adhesion enhancing coating, a heat-insulating coating I, a heat-insulating coating II, and a waterproof spray-painted coating; the composite coating composites the uncoated side of the base fabric layer.

[0041] The base fabric layer is composed of 40%-50% polyester fiber and 50%-60% glass fiber. The thickness of the polyester fiber can be selected from 75D-1000D composite yarn. The base fabric layer is made of a blend of chemical fiber and glass fiber to improve its flexibility, while the glass fiber increases the thermal insulation capacity of the product.

[0042] The coating for the hand-feel coating comprises the following components in parts by weight: 30-50 parts of organic silicon modified waterborne polyurethane, 100 parts of deionized water, and 3-10 parts of cellulose.

[0043] The coating for the adhesion enhancement layer includes the following components in parts by weight: 50-100 parts of an aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 6-10 parts of an alkali swelling and associative compound thickener, and 0.6-1 part of a defoaming agent.

[0044] The coatings used for both thermal insulation coating I and thermal insulation coating II include the following components by weight: 200-300 parts of water-based acrylic self-crosslinking textile emulsion with a TG value of -30℃ to -15℃, 200-300 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 40-60 parts of nano-silica aerogel powder, 20-40 parts of nano-glass microspheres, 20-40 parts of core-shell titanium dioxide, and 12-20 parts of microsphere foaming agent. The thermal conductivity of the product is reduced by compounding the low thermal conductivity materials of nano-silica aerogel powder and nano-glass microspheres, giving the product an excellent thermal insulation effect. The addition of bromine antimony flame retardant gives the product excellent flame retardancy.

[0045] The coating for the waterproof spray painting layer includes the following components in parts by weight: 100-200 parts of silicone modified waterborne polyurethane emulsion with a TG value of 5°C-20°C, 60-200 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 5-15 parts of nano silicon dioxide, 5-10 parts of nano modified wax powder, 3-6 parts of polyurethane thickener, and 0.6-1 part of defoaming agent.

[0046] The coating material for the composite coating comprises the following components in parts by weight: 100-200 parts of waterborne polyurethane emulsion with a TG value of 5-20°C and 10-30 parts of low melting point PA powder.

[0047] In another exemplary embodiment of the present invention, a preparation process of a highly flame-retardant, foldable, heat-insulating, double-sided spray-painted material can be achieved by the following steps:

[0048] (1) Preparation of base fabric layer

[0049] 40%-50% polyester chemical fiber yarn and 50%-60% glass fiber are mixed and spun, and then shaped.

[0050] Specifically, the base fabric layer is customized by blending polyester chemical fiber and glass fiber, which enhances the fire resistance of the base material and improves the product's good folding resistance. It can be shaped by a 10-section needle plate shaping machine, and the temperatures are set to 100℃, 180℃, 210℃, 220℃, 220℃, 220℃, 210℃, 190℃, 180℃ and 100℃ respectively. It can also be shaped by a high temperature of 220℃ to give the product good dimensional stability.

[0051] (2) Preparation of hand-feel coating

[0052] 30-50 parts of silicone-modified waterborne polyurethane, 100 parts of water and 3-10 parts of cellulose are mixed evenly by weight, coated on one side of the base fabric layer by screen coating, and then cross-linked and cured in a 10-section oven to form a hand-feel coating.

[0053] Specifically, the oven temperature is set to 90°C, 100°C, 120°C, 160°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C. The coating wet weight of the hand-feel coating is 60-100gsm, the coating speed is 35-45m / min, and the coating thickness is 5-20μm. It is coated on the surface of the base fabric layer by screen coating. By controlling the viscosity of the coating, the adhesion of the coating to the base fabric layer is increased, the penetration of latex is reduced, and the cross-linking and curing treatment further provides the material with good flexibility and folding resistance, making the material foldable.

[0054] (3) Preparation of adhesion enhancing coating

[0055] According to weight parts, 50-100 parts of aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 6-10 parts of alkali swelling and associative compound thickener, and 0.6-1 part of defoaming agent are mixed evenly, the pH is adjusted to 7-8, the viscosity is adjusted, and the coating is applied on the surface of the hand feel coating by a doctor blade coating method, and cured in a 10-section oven to form an adhesion enhanced coating.

[0056] Specifically, the viscosity is adjusted to 15000-20000cps / 4#, 30rpm, the solid content is 45%±5, and the adhesion enhancing coating is applied on the surface of the hand-feel coating by a 1mm scraper coating method. The 10-section oven temperature is set to 90℃, 100℃, 120℃, 160℃, 160℃, 160℃, 150℃, 150℃, 120℃ and 100℃ in sequence to form an adhesion enhancing coating. The coating wet weight of the adhesion enhancing coating is 20-100gsm, the coating speed is 10-20m / min, and the coating thickness is 5-20μm. Provide a connection between the hand-feel coating and the thermal insulation coating I, and enhance the adhesion of the thermal insulation coating I.

[0057] (4) Preparation of thermal insulation coating I

[0058] According to weight parts, 200-300 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30°C to -15°C, 200-300 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 40-60 parts of nano-silica aerogel powder, 20-40 parts of nano-glass microbeads, 20-40 parts of core-shell titanium dioxide, and 12-20 parts of microsphere foaming agent are uniformly mixed, the pH is adjusted to 7-8, the viscosity is adjusted, and the coating is applied on the surface of the adhesion enhancing coating by an E-type knife gap coating method, and then a 10-section oven curing treatment is performed, and then a foaming treatment is performed at 190-210°C to form a thermal insulation coating I.

[0059] Specifically, the coating with a viscosity of 5000-7000cps / 4#, 30rpm and a solid content of 45%±5 is adjusted with an alkali swelling thickener. A 5mm E-type knife is used to coat the surface of the adhesion enhancement coating in two intervals. The 10-section oven temperature is set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ in sequence. Then, it is heated by a 200℃ roller and a 300μm gap method, and the microsphere foaming agent is heated and expanded to form a porous structure. The coating wet weight of the thermal insulation coating I is 100-200gsm, the coating speed is 20-30m / min, and the coating thickness is 300μm.

[0060] (5) Preparation of thermal insulation coating II

[0061] According to weight parts, 200-300 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30°C to -15°C, 200-300 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 40-60 parts of nano-silica aerogel powder, 20-40 parts of nano-glass microbeads, 20-40 parts of core-shell titanium dioxide, and 12-20 parts of microsphere foaming agent are uniformly mixed, the pH is adjusted to 7-8, the viscosity is adjusted, and then the mixture is coated on the surface of the thermal insulation coating I by an E-type knife gap coating method, cured in a 10-section oven, and then foamed at 190-210°C to form a thermal insulation coating II.

[0062] Specifically, the viscosity of the coating is adjusted to 5000-7000cps / 4#, 30rpm with an alkali swelling thickener and a solid content of 45%±5. A 5mm E-type knife is used to coat the surface of the adhesion enhancement coating in two intervals. The 10-section oven temperature is set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ in sequence. Then, it is heated by a 200℃ roller and a 300μm gap method, and the microsphere foaming agent is heated and expanded to form a porous structure. The coating wet weight of the thermal insulation coating II is 100-200gsm, the coating speed is 20-30m / min, and the coating thickness is 300μm.

[0063] Thermal insulation coating I and thermal insulation coating II form a microporous structure through microsphere foaming technology, which increases the thickness of the material and provides a better feel, and provides a good thermal insulation effect for the material. The coating further improves the thermal insulation effect of the product by compounding nano-silicon dioxide aerogel powder and nano-glass beads. At the same time, the coating provides a good flame retardant effect for the product by compounding modified aluminum hydroxide, antimony trioxide, and decabromodiphenylethane flame retardant.

[0064] (6) Preparation of waterproof spray coating

[0065] According to weight parts, 100-200 parts of silicone-modified water-based polyurethane emulsion with a TG value of 5℃-20℃, 60-200 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 5-15 parts of nano-silicon dioxide, 5-10 parts of nano-modified wax powder, 3-6 parts of polyurethane thickener and 0.6-1 part of defoaming agent are mixed evenly, and after adjusting the viscosity, it is applied on the surface of the thermal insulation coating II by scraper coating, and dried and cured in a 10-section oven to form a waterproof spray coating.

[0066] Specifically, the oven temperatures are set to 90° C., 100° C., 120° C., 130° C., 130° C., 130° C., 130° C., 130° C., 110° C. and 100° C. The coating weight of the waterproof spray coating is 30-60 gsm, the coating speed is 10-20 m / min, and the coating thickness is 10-30 μm.

[0067] The waterproof spray coating gives the material a good water-repellent effect by adding modified polyurethane emulsion and nano wax powder, effectively preventing rainwater from infiltrating, and provides UV, weak solvent, and Latex ink printing coatings to achieve the effects of isolating rainwater and being printable, increasing the practicality of the material.

[0068] (7) Preparation of composite coating

[0069] 100-200 parts of aqueous polyurethane emulsion with a TG value of 5°C-20°C and 10-30 parts of low melting point PA powder are mixed evenly according to weight, and the viscosity is adjusted. The uncoated sides of the two base fabric layers are laminated by roller heating using a laminating machine.

[0070] Specifically, the coating with a viscosity of 5000-6000cps / 4#, 60rpm, and a solid content of 55%±5 is laminated by roller transfer coating on the uncoated side of the base fabric layer through a laminating machine and roller heating at 150℃. The wet weight of the composite coating is 15-20gsm, the coating speed is 8-12m / min, and the coating thickness is 5-10μm.

[0071] Example 1: A highly flame-retardant, foldable, heat-insulating, double-sided spray-painted material

[0072] Figure 1 The cross-sectional structure diagram of a highly flame-retardant, foldable, heat-insulating, double-sided spray-painted material of the present invention is shown.

[0073] like Figure 1 As shown, in an exemplary embodiment of the present invention, a highly flame-retardant, foldable, heat-insulating, double-sided spray-painted material comprises a base fabric layer 1, the upper surface of the base fabric layer is coated with a hand-feel coating 2, the upper surface of the hand-feel coating 2 is coated with an adhesion enhancing layer 3, the upper surface of the adhesion enhancing layer 3 is coated with a heat-insulating coating I4, the upper surface of the heat-insulating layer I4 is coated with a heat-insulating coating II5, the upper surface of the heat-insulating coating II5 is coated with a waterproof spray-painted layer 6, and the uncoated surface of the base fabric layer 1 is compounded together by a compound coating 7 to form a highly flame-retardant, foldable, heat-insulating, double-sided spray-painted material.

[0074] Example 2

[0075] This embodiment prepares a highly flame-retardant, foldable, heat-insulating, double-sided inkjet printing material 1#, which is prepared using the following method:

[0076] (1) Preparation of base fabric layer

[0077] 40% 75D*150D polyester chemical fiber yarn and 60% glass fiber are mixed and spun, and then formed by a 10-section needle plate forming machine with a speed of 40m / min. The temperatures are set to 100℃, 180℃, 210℃, 220℃, 220℃, 220℃, 210℃, 190℃, 180℃ and 100℃ in sequence to obtain a base fabric layer.

[0078] (2) Preparation of hand-feel coating

[0079] 30 parts of silicone modified waterborne polyurethane, 100 parts of water and 3 parts of cellulose were mixed evenly according to weight, and coated on one side of the base fabric layer by screen coating. The coating wet weight of the hand-feel coating was 60 gsm, the coating speed was 45 m / min, the coating thickness was 10 μm, and then the coating was cross-linked and cured in a 10-section oven. The oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C, respectively.

[0080] (3) Preparation of adhesion enhancing coating

[0081] According to weight parts, 50 parts of aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 10 parts of modified aluminum hydroxide, 10 parts of antimony trioxide, and 20 parts of decabromodiphenylethane were mixed evenly, the pH was adjusted to 7-8, and then 10 parts of alkali swelling and associative compound thickener and 0.6 parts of defoamer were slowly added and mixed evenly, the viscosity was adjusted to 15000-20000cps / 4#, 30rpm, 1mm scraper coating method was adopted, the coating wet weight was 20gsm, the coating speed was 20m / min, the coating thickness was 10μm, it was coated on the surface of the hand feel coating, and it was cured in 10 ovens, and the oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C in sequence to form an adhesion enhanced coating.

[0082] (4) Preparation of thermal insulation coating I

[0083] According to weight parts, 300 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 200 parts of water, 10 parts of modified aluminum hydroxide, 10 parts of antimony trioxide, 20 parts of decabromodiphenylethane, 40 parts of nano-silica aerogel powder, 20 parts of nano-glass microbeads, 20 parts of core-shell titanium dioxide, and 12 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5, using 5mm E-type knife, through gap coating method, coated on the surface of adhesion enhancing coating, coating wet weight is 100gsm, vehicle speed is 30m / min, dried in 10-section oven, oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃, then heated by 200℃ roller, 300μm gap method, through the microsphere foaming agent heat expansion, foaming treatment is carried out to form a porous structure thermal insulation coating I.

[0084] (5) Preparation of thermal insulation coating II

[0085] According to weight parts, 300 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 200 parts of water, 10 parts of modified aluminum hydroxide, 10 parts of antimony trioxide, 20 parts of decabromodiphenylethane, 40 parts of nano-silica aerogel powder, 20 parts of nano-glass microbeads, 20 parts of core-shell titanium dioxide, and 12 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5, using 5mm The E-type knife is applied on the surface of the thermal insulation coating I by gap coating, the wet coating weight is 100gsm, the vehicle speed is 30m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to form a thermal insulation coating II with a porous structure.

[0086] (6) Preparation of waterproof spray coating

[0087] According to weight parts, 100 parts of silicone modified waterborne polyurethane emulsion with a TG value of 5°C-20°C, 60 parts of water, 10 parts of modified aluminum hydroxide, 10 parts of antimony trioxide, 20 parts of decabromodiphenylethane, 5 parts of nano-silicon dioxide, 5 parts of nano-modified wax powder, 3 parts of polyurethane thickener and 0.6 parts of defoamer are mixed evenly, and the viscosity is adjusted to 15000-20000cps / 4#, 30rpm, and the solid content of the top coating is 35%±5. A 1mm scraper coating method is adopted, the wet coating amount is 30gsm, the vehicle speed is 20m / min, and the coating thickness is 10μm. It is coated on the surface layer of the thermal insulation coating II, and is cured in a 10-section oven. The oven temperatures are set to 90°C, 100°C, 120°C, 130°C, 130°C, 130°C, 130°C, 130°C, 110°C and 100°C in sequence to form a waterproof spray coating.

[0088] (7) Preparation of composite coating

[0089] According to weight portions, 100 portions of aqueous polyurethane emulsion with a TG value of 5°C-20°C and 10 portions of low melting point PA powder were mixed evenly, and the viscosity was adjusted to 5000-6000cps / 4#, 60rpm, and the solid content of the coating was 55%±5. The laminating speed was 12m / min, and the uncoated side of the base fabric layer was coated by roller transfer coating with a glue amount of 15gsm and a thickness of 5μm. The coating was heated by roller at 150°C and compounded together to obtain a highly flame-retardant, foldable, and heat-insulating double-sided inkjet material 1#.

[0090] Example 3

[0091] This embodiment prepares another highly flame-retardant, foldable, heat-insulating, double-sided inkjet printing material 2#, which is prepared using the following method:

[0092] (1) Preparation of base fabric layer

[0093] 45% 300D*500D polyester chemical fiber yarn and 55% glass fiber are mixed and spun, and then formed by a 10-section needle plate forming machine with a speed of 35m / min. The temperatures are set to 100℃, 180℃, 210℃, 220℃, 220℃, 220℃, 210℃, 190℃, 180℃ and 100℃ in sequence to obtain a base fabric layer.

[0094] (2) Preparation of hand-feel coating

[0095] 38 parts of silicone modified waterborne polyurethane, 100 parts of water and 6 parts of cellulose were mixed evenly according to weight, and coated on one side of the base fabric layer by screen coating. The coating wet weight of the hand-feel coating was 75 gsm, the coating speed was 40 m / min, the coating thickness was 10 μm, and then the coating was cross-linked and cured in a 10-section oven. The oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C, respectively.

[0096] (3) Preparation of adhesion enhancing coating

[0097] According to weight parts, 65 parts of aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 13 parts of modified aluminum hydroxide, 13 parts of antimony trioxide, and 26 parts of decabromodiphenylethane were mixed evenly, the pH was adjusted to 7-8, and then 9 parts of alkali swelling and associative compound thickener and 0.7 parts of defoamer were slowly added and mixed evenly, and the viscosity was adjusted to 15000-20000cps / 4#, 30rpm, 1mm scraper coating method was adopted, the coating wet weight was 40gsm, the coating speed was 18m / min, the coating thickness was 10μm, and it was coated on the surface of the hand feel coating, and it was cured in a 10-section oven. The oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C in sequence to form an adhesion enhanced coating.

[0098] (4) Preparation of thermal insulation coating I

[0099] According to weight parts, 260 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 230 parts of water, 13 parts of modified aluminum hydroxide, 13 parts of antimony trioxide, 26 parts of decabromodiphenylethane, 45 parts of nano-silica aerogel powder, 25 parts of nano-glass microbeads, 25 parts of core-shell titanium dioxide, and 15 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5. 5mm The E-type knife is applied on the surface of the adhesion enhancing coating by gap coating, the wet coating weight is 120gsm, the vehicle speed is 28m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to form a porous structure thermal insulation coating I.

[0100] (5) Preparation of thermal insulation coating II

[0101] According to weight parts, 260 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 230 parts of water, 13 parts of modified aluminum hydroxide, 13 parts of antimony trioxide, 26 parts of decabromodiphenylethane, 45 parts of nano-silica aerogel powder, 25 parts of nano-glass microbeads, 25 parts of core-shell titanium dioxide, and 15 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5. 5mm The E-type knife is applied on the surface of the thermal insulation coating I by gap coating, the wet coating weight is 120gsm, the vehicle speed is 28m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to form a thermal insulation coating II with a porous structure.

[0102] (6) Preparation of waterproof spray coating

[0103] According to weight parts, 130 parts of silicone modified waterborne polyurethane emulsion with a TG value of 5°C-20°C, 100 parts of water, 13 parts of modified aluminum hydroxide, 13 parts of antimony trioxide, 26 parts of decabromodiphenylethane, 8 parts of nano silicon dioxide, 7 parts of nano modified wax powder, 4 parts of polyurethane thickener and 0.7 parts of defoamer are mixed evenly, and the viscosity is adjusted to 15000-20000cps / 4#, 30rpm, and the solid content of the top coating is 35%±5. A 1mm scraper coating method is adopted, a wet coating amount of 40gsm, a vehicle speed of 18m / min, a coating thickness of 10μm, and it is coated on the surface layer of thermal insulation coating II, and cured in a 10-section oven. The oven temperatures are set to 90°C, 100°C, 120°C, 130°C, 130°C, 130°C, 130°C, 130°C, 110°C and 100°C in sequence to form a waterproof spray coating.

[0104] (7) Preparation of composite coating

[0105] 120 parts of water-based polyurethane emulsion with a TG value of 5℃-20℃ and 13 parts of low-melting point PA powder are mixed according to weight parts, and the viscosity is adjusted to 5000-6000cps / 4#, 60rpm, and the solid content of the coating is 55%±5. The laminating locomotive speed is 11m / min. The uncoated side of the base fabric layer is coated with 17gsm of glue and 5μm of thickness by roller transfer coating, and the roller heating method is 150℃. The materials are compounded together to obtain a highly flame-retardant, foldable, and heat-insulating double-sided inkjet material 2#.

[0106] Example 4

[0107] This embodiment prepares another highly flame-retardant, foldable, heat-insulating, double-sided inkjet printing material 3#, which is prepared using the following method:

[0108] (1) Preparation of base fabric layer

[0109] 50% 600D*600D polyester chemical fiber yarn and 50% glass fiber are mixed and spun, and then formed by a 10-section needle plate forming machine with a speed of 30m / min. The temperatures are set to 100℃, 180℃, 210℃, 220℃, 220℃, 220℃, 210℃, 190℃, 180℃ and 100℃ in sequence to obtain a base fabric layer.

[0110] (2) Preparation of hand-feel coating

[0111] 45 parts of silicone modified waterborne polyurethane, 100 parts of water and 8 parts of cellulose were mixed evenly according to weight, and coated on one side of the base fabric layer by screen coating. The coating wet weight of the hand-feel coating was 35 gsm, the coating speed was 85 m / min, the coating thickness was 10 μm, and then the coating was cross-linked and cured in a 10-section oven. The oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C, respectively.

[0112] (3) Preparation of adhesion enhancing coating

[0113] According to weight parts, 80 parts of aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 16 parts of modified aluminum hydroxide, 16 parts of antimony trioxide, and 32 parts of decabromodiphenylethane were mixed evenly, the pH was adjusted to 7-8, and then 8 parts of alkali swelling and associative compound thickener and 0.85 parts of defoamer were slowly added and mixed evenly, the viscosity was adjusted to 15000-20000cps / 4#, 30rpm, 1mm scraper coating method was adopted, the coating wet weight was 60gsm, the coating speed was 15m / min, the coating thickness was 10μm, and it was coated on the surface of the hand feel coating, and it was cured in a 10-section oven. The oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C in sequence to form an adhesion enhanced coating.

[0114] (4) Preparation of thermal insulation coating I

[0115] According to weight parts, 230 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 260 parts of water, 17 parts of modified aluminum hydroxide, 17 parts of antimony trioxide, 34 parts of decabromodiphenylethane, 55 parts of nano-silica aerogel powder, 35 parts of nano-glass microbeads, 17 parts of core-shell titanium dioxide, and 17 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5. 5mm The E-type knife is applied on the surface of the adhesion enhancing coating by gap coating, the wet coating weight is 150gsm, the vehicle speed is 25m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to form a porous structure thermal insulation coating I.

[0116] (5) Preparation of thermal insulation coating II

[0117] According to weight parts, 260 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 230 parts of water, 13 parts of modified aluminum hydroxide, 13 parts of antimony trioxide, 26 parts of decabromodiphenylethane, 45 parts of nano-silica aerogel powder, 25 parts of nano-glass microbeads, 25 parts of core-shell titanium dioxide, and 15 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5. 5mm The E-type knife is applied on the surface of the thermal insulation coating I by gap coating, the wet coating weight is 150gsm, the vehicle speed is 25m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to form a thermal insulation coating II with a porous structure.

[0118] (6) Preparation of waterproof spray coating

[0119] According to weight parts, 150 parts of silicone modified waterborne polyurethane emulsion with a TG value of 5°C-20°C, 150 parts of water, 15 parts of modified aluminum hydroxide, 15 parts of antimony trioxide, 30 parts of decabromodiphenylethane, 12 parts of nano silicon dioxide, 9 parts of nano modified wax powder, 5 parts of polyurethane thickener and 0.9 parts of defoamer are mixed evenly, and the viscosity is adjusted to 15000-20000cps / 4#, 30rpm, and the solid content of the top coating is 35%±5. A 1mm scraper coating method is adopted, a wet coating amount of 50gsm, a vehicle speed of 15m / min, a coating thickness of 10μm, and it is coated on the surface layer of the thermal insulation coating II, and cured in a 10-section oven. The oven temperatures are set to 90°C, 100°C, 120°C, 130°C, 130°C, 130°C, 130°C, 130°C, 110°C and 100°C in sequence to form a waterproof spray coating.

[0120] (7) Preparation of composite coating

[0121] 150 parts of water-based polyurethane emulsion with a TG value of 5℃-20℃ and 17 parts of low-melting point PA powder are mixed according to weight, and the viscosity is adjusted to 5000-6000cps / 4#, 60rpm, and the solid content of the coating is 55%±5. The laminating locomotive speed is 9m / min. The uncoated side of the base fabric layer is coated with 18gsm of glue and 5μm of thickness by roller transfer coating, and the roller heating method is 150℃. The materials are compounded together to obtain a highly flame-retardant, foldable, and heat-insulating double-sided inkjet material 3#.

[0122] Example 5

[0123] This embodiment prepares another highly flame-retardant, foldable, heat-insulating, double-sided inkjet printing material 4#, which is prepared using the following method:

[0124] (1) Preparation of base fabric layer

[0125] 45% 1000D*1000D polyester chemical fiber yarn and 55% glass fiber are mixed and spun, and then formed by a 10-section needle plate forming machine with a speed of 25m / min. The temperatures are set to 100℃, 180℃, 210℃, 220℃, 220℃, 220℃, 210℃, 190℃, 180℃ and 100℃ in sequence to obtain a base fabric layer.

[0126] (2) Preparation of hand-feel coating

[0127] 50 parts of silicone modified waterborne polyurethane, 100 parts of water and 10 parts of cellulose were mixed evenly according to weight, and coated on one side of the base fabric layer by screen coating. The coating wet weight of the hand-feel coating was 35 gsm, the coating speed was 100 m / min, the coating thickness was 10 μm, and then the coating was cross-linked and cured in 10 ovens. The oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C respectively.

[0128] (3) Preparation of adhesion enhancing coating

[0129] According to weight parts, 100 parts of aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, and 40 parts of decabromodiphenylethane were mixed evenly, the pH was adjusted to 7-8, and then 6 parts of alkali swelling and associative compound thickener and 1 part of defoamer were slowly added and mixed evenly, and the viscosity was adjusted to 15000-20000cps / 4#, 30rpm, and a 1mm scraper coating method was adopted. The coating wet weight was 100gsm, the coating speed was 10m / min, the coating thickness was 10μm, and it was coated on the surface of the hand feel coating. It was cured in a 10-section oven, and the oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C in sequence to form an adhesion enhanced coating.

[0130] (4) Preparation of thermal insulation coating I

[0131] According to weight parts, 200 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 300 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 60 parts of nano-silica aerogel powder, 40 parts of nano-glass microbeads, 40 parts of core-shell titanium dioxide, and 20 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5, using 5mm The E-type knife is applied on the surface of the adhesion enhancing coating by gap coating, the wet coating weight is 200gsm, the vehicle speed is 20m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to form a porous structure thermal insulation coating I.

[0132] (5) Preparation of thermal insulation coating II

[0133] According to weight parts, 200 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 300 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 60 parts of nano-silica aerogel powder, 40 parts of nano-glass microbeads, 40 parts of core-shell titanium dioxide, and 20 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5, using 5mm The E-type knife is applied on the surface of the thermal insulation coating I by gap coating, the wet coating weight is 200gsm, the vehicle speed is 20m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to carry out foaming treatment to form a thermal insulation coating II with a porous structure.

[0134] (6) Preparation of waterproof spray coating

[0135] According to weight parts, 200 parts of silicone modified waterborne polyurethane emulsion with a TG value of 5°C-20°C, 200 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 15 parts of nano silicon dioxide, 10 parts of nano modified wax powder, 6 parts of polyurethane thickener and 1 part of defoamer are mixed evenly, and the viscosity is adjusted to 15000-20000cps / 4#, 30rpm, and the solid content of the top coating is 35%±5. A 1mm scraper coating method is adopted, the wet coating amount is 60gsm, the vehicle speed is 10m / min, and the coating thickness is 10μm. It is coated on the surface layer of the thermal insulation coating II, and is cured in a 10-section oven. The oven temperatures are set to 90°C, 100°C, 120°C, 130°C, 130°C, 130°C, 130°C, 130°C, 110°C and 100°C in sequence to form a waterproof spray coating.

[0136] (7) Preparation of composite coating

[0137] According to weight portions, 200 portions of aqueous polyurethane emulsion with a TG value of 5°C-20°C and 30 portions of low melting point PA powder are mixed, and the viscosity is adjusted to 5000-6000cps / 4#, 60rpm, and the solid content of the coating is 55%±5. The laminating locomotive speed is 8m / min. The uncoated side of the base fabric layer is coated with 20gsm of glue and 5μm of thickness by roller transfer coating, and the roller heating method is 150°C. The materials are compounded together to obtain a highly flame-retardant, foldable, and heat-insulating double-sided inkjet material 4#.

[0138] Comparative Example 1

[0139] This comparative example prepared a comparative double-sided inkjet printing material D1#, which was prepared using the following method:

[0140] (1) Preparation of base fabric layer

[0141] The base fabric layer is polyester chemical fiber.

[0142] (2) Preparation of hand-feel coating

[0143] 5 parts of polyurethane, 100 parts of water and 2 parts of cellulose were mixed evenly according to weight, and coated on one side of the base fabric layer by screen coating. The coating wet weight of the hand-feel coating was 50 gsm, the coating speed was 35 m / min, the coating thickness was 10 μm, and then cross-linked and cured at 160°C.

[0144] (3) Preparation of adhesion enhancing coating

[0145] According to weight parts, 100 parts of aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, and 40 parts of decabromodiphenylethane were mixed evenly, the pH was adjusted to 7-8, and then 6 parts of alkali swelling and associative compound thickener and 1 part of defoamer were slowly added and mixed evenly, and the viscosity was adjusted to 15000-20000cps / 4#, 30rpm, and a 1mm scraper coating method was adopted. The coating wet weight was 100gsm, the coating speed was 10m / min, the coating thickness was 10μm, and it was coated on the surface of the hand feel coating. It was cured in a 10-section oven, and the oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C in sequence to form an adhesion enhanced coating.

[0146] (4) Preparation of thermal insulation coating I

[0147] According to weight parts, 200 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 300 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 60 parts of nano-silica aerogel powder, 40 parts of nano-glass microbeads, 40 parts of core-shell titanium dioxide, and 20 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5, using 5mm The E-type knife is applied on the surface of the adhesion enhancing coating by gap coating, the wet coating weight is 200gsm, the vehicle speed is 20m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to form a porous structure thermal insulation coating I.

[0148] (5) Preparation of thermal insulation coating II

[0149] According to weight parts, 200 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 300 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 60 parts of nano-silica aerogel powder, 40 parts of nano-glass microbeads, 40 parts of core-shell titanium dioxide, and 20 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5, using 5mm The E-type knife is applied on the surface of the thermal insulation coating I by gap coating, the wet coating weight is 200gsm, the vehicle speed is 20m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to carry out foaming treatment to form a thermal insulation coating II with a porous structure.

[0150] (6) Preparation of waterproof spray coating

[0151] According to weight parts, 200 parts of silicone modified waterborne polyurethane emulsion with a TG value of 5°C-20°C, 200 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 15 parts of nano silicon dioxide, 10 parts of nano modified wax powder, 6 parts of polyurethane thickener and 1 part of defoamer are mixed evenly, and the viscosity is adjusted to 15000-20000cps / 4#, 30rpm, and the solid content of the top coating is 35%±5. A 1mm scraper coating method is adopted, the wet coating amount is 60gsm, the vehicle speed is 10m / min, and the coating thickness is 10μm. It is coated on the surface layer of the thermal insulation coating II, and is cured in a 10-section oven. The oven temperatures are set to 90°C, 100°C, 120°C, 130°C, 130°C, 130°C, 130°C, 130°C, 110°C and 100°C in sequence to form a waterproof spray coating.

[0152] (7) Preparation of composite coating

[0153] 200 parts of water-based polyurethane emulsion with a TG value of 5°C-20°C and 30 parts of low-melting-point PA powder were mixed according to weight, and the viscosity was adjusted to 5000-6000cps / 4#. The coating with a solid content of 55%±5 was prepared at 60rpm and a laminating speed of 8m / min. The uncoated side of the base fabric layer was coated with 20gsm of glue and 5μm of thickness by roller transfer coating and 150°C roller heating. The materials were compounded together to obtain a highly flame-retardant, foldable, and heat-insulating double-sided inkjet material D1#.

[0154] Comparative Example 2

[0155] This comparative example prepared another comparative double-sided inkjet printing material D2#, which was prepared using the following method:

[0156] (1) Preparation of base fabric layer

[0157] 45% 1000D*1000D polyester chemical fiber yarn and 55% glass fiber are mixed and spun, and then formed by a 10-section needle plate forming machine with a speed of 25m / min. The temperatures are set to 100℃, 180℃, 210℃, 220℃, 220℃, 220℃, 210℃, 190℃, 180℃ and 100℃ in sequence to obtain a base fabric layer.

[0158] (2) Preparation of hand-feel coating

[0159] 50 parts of silicone modified waterborne polyurethane, 100 parts of water and 10 parts of cellulose were mixed evenly according to weight, and coated on one side of the base fabric layer by screen coating. The coating wet weight of the hand-feel coating was 35 gsm, the coating speed was 100 m / min, the coating thickness was 10 μm, and then the coating was cross-linked and cured in 10 ovens. The oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C respectively.

[0160] (3) Preparation of adhesion enhancing coating

[0161] According to weight parts, 100 parts of aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, and 40 parts of decabromodiphenylethane were mixed evenly, the pH was adjusted to 7-8, and then 6 parts of alkali swelling and associative compound thickener and 1 part of defoamer were slowly added and mixed evenly, and the viscosity was adjusted to 15000-20000cps / 4#, 30rpm, and a 1mm scraper coating method was adopted. The coating wet weight was 100gsm, the coating speed was 10m / min, the coating thickness was 10μm, and it was coated on the surface of the hand feel coating. It was cured in a 10-section oven, and the oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C in sequence to form an adhesion enhanced coating.

[0162] (4) Preparation of thermal insulation coating I

[0163] According to weight parts, 200 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 300 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 60 parts of nano-silica aerogel powder, 40 parts of nano-glass microbeads, 40 parts of core-shell titanium dioxide, and 20 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5, using 5mm The E-type knife is applied on the surface of the adhesion enhancing coating by gap coating, the wet coating weight is 200gsm, the vehicle speed is 20m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to form a porous structure thermal insulation coating I.

[0164] (5) Preparation of thermal insulation coating II

[0165] According to weight parts, 200 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 300 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 60 parts of nano-silica aerogel powder, 40 parts of nano-glass microbeads, 40 parts of core-shell titanium dioxide, and 20 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5, using 5mm The E-type knife is applied on the surface of the thermal insulation coating I by gap coating, the wet coating weight is 200gsm, the vehicle speed is 20m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to carry out foaming treatment to form a thermal insulation coating II with a porous structure.

[0166] (6) Preparation of waterproof spray coating

[0167] According to weight parts, 200 parts of unmodified common polyurethane emulsion with a TG value of 5°C-20°C, 200 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 15 parts of nano silicon dioxide, 10 parts of nano modified wax powder, 6 parts of polyurethane thickener and 1 part of defoamer are mixed evenly, and the viscosity is adjusted to 15000-20000cps / 4#, 30rpm, and the solid content of the top coating is 35%±5. A 1mm scraper coating method is adopted, the wet coating amount is 60gsm, the vehicle speed is 10m / min, and the coating thickness is 10μm. It is coated on the surface layer of the thermal insulation coating II, and is cured in a 10-section oven. The oven temperatures are set to 90°C, 100°C, 120°C, 130°C, 130°C, 130°C, 130°C, 130°C, 110°C and 100°C in sequence to form a waterproof spray coating.

[0168] (7) Preparation of composite coating

[0169] 200 parts of water-based polyurethane emulsion with a TG value of 5°C-20°C and 30 parts of low-melting-point PA powder were mixed according to weight, and the viscosity was adjusted to 5000-6000cps / 4#. The coating with a solid content of 55%±5 was prepared at 60rpm and a laminating speed of 8m / min. The uncoated side of the base fabric layer was coated with 20gsm of glue and 5μm of thickness by roller transfer coating and 150°C roller heating. The materials were compounded together to obtain a highly flame-retardant, foldable, and heat-insulating double-sided inkjet material D2#.

[0170] Comparative Example 3

[0171] This comparative example prepared another comparative double-sided inkjet printing material D3#, which was prepared using the following method:

[0172] (1) Preparation of base fabric layer

[0173] 45% 1000D*1000D polyester chemical fiber yarn and 55% glass fiber are mixed and spun, and then formed by a 10-section needle plate forming machine with a speed of 25m / min. The temperatures are set to 100℃, 180℃, 210℃, 220℃, 220℃, 220℃, 210℃, 190℃, 180℃ and 100℃ in sequence to obtain a base fabric layer.

[0174] (2) Preparation of hand-feel coating

[0175] 50 parts of silicone modified waterborne polyurethane, 100 parts of water and 10 parts of cellulose were mixed evenly according to weight, and coated on one side of the base fabric layer by screen coating. The coating wet weight of the hand-feel coating was 35 gsm, the coating speed was 100 m / min, the coating thickness was 10 μm, and then the coating was cross-linked and cured in 10 ovens. The oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C respectively.

[0176] (3) Preparation of adhesion enhancing coating

[0177] According to weight parts, 100 parts of aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, and 40 parts of decabromodiphenylethane were mixed evenly, the pH was adjusted to 7-8, and then 6 parts of alkali swelling and associative compound thickener and 1 part of defoamer were slowly added and mixed evenly, and the viscosity was adjusted to 15000-20000cps / 4#, 30rpm, and a 1mm scraper coating method was adopted. The coating wet weight was 100gsm, the coating speed was 10m / min, the coating thickness was 10μm, and it was coated on the surface of the hand feel coating. It was cured in a 10-section oven, and the oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C in sequence to form an adhesion enhanced coating.

[0178] (4) Preparation of thermal insulation coating I

[0179] According to weight parts, 200 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 300 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 60 parts of nano-silica aerogel powder, 40 parts of nano-glass microbeads, 40 parts of core-shell titanium dioxide, and 20 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5, using 5mm The E-type knife is applied on the surface of the adhesion enhancing coating by gap coating, the wet coating weight is 200gsm, the vehicle speed is 20m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to form a porous structure thermal insulation coating I.

[0180] (5) Preparation of thermal insulation coating II

[0181] According to weight parts, 200 parts of water-based acrylic self-crosslinking textile emulsion with TG value of -30℃~-15℃, 300 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 60 parts of nano-silica aerogel powder, 40 parts of nano-glass microbeads, 40 parts of core-shell titanium dioxide, and 20 parts of microsphere foaming agent were mixed evenly, and the pH was adjusted to 7-8. The viscosity was adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating was 45%±5, using 5mm The E-type knife is applied on the surface of the thermal insulation coating I by gap coating, the wet coating weight is 200gsm, the vehicle speed is 20m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90℃, 100℃, 120℃, 130℃, 130℃, 130℃, 130℃, 130℃, 110℃ and 100℃ respectively, and then heated by a 200℃ roller and a 300μm gap. The microsphere foaming agent is heated and expanded to carry out foaming treatment to form a thermal insulation coating II with a porous structure.

[0182] (6) Preparation of waterproof spray coating

[0183] According to weight parts, 200 parts of silicone modified waterborne polyurethane emulsion with a TG value of 5°C-20°C, 200 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 15 parts of nano-silicon dioxide, 6 parts of polyurethane thickener and 1 part of defoamer are mixed evenly, and the viscosity is adjusted to 15000-20000cps / 4#, 30rpm, and the solid content of the top coating is 35%±5. A 1mm scraper coating method is adopted, the wet coating amount is 60gsm, the vehicle speed is 10m / min, the coating thickness is 10μm, and it is coated on the surface layer of the thermal insulation coating II. It is cured in a 10-section oven, and the oven temperatures are set to 90°C, 100°C, 120°C, 130°C, 130°C, 130°C, 130°C, 130°C, 110°C and 100°C in sequence to form a waterproof spray coating.

[0184] (7) Preparation of composite coating

[0185] 200 parts of water-based polyurethane emulsion with a TG value of 5℃-20℃ and 30 parts of low-melting point PA powder are mixed according to weight parts, and the viscosity is adjusted to 5000-6000cps / 4#, 60rpm, and the solid content of the coating is 55%±5. The laminating locomotive speed is 8m / min. The uncoated side of the base fabric layer is coated with 20gsm of glue and 5μm of thickness by roller transfer coating, and the roller heating method is 150℃. The highly flame-retardant, foldable and heat-insulating double-sided inkjet material D3# is obtained.

[0186] Comparative Example 4

[0187] This comparative example prepared a comparative double-sided inkjet printing material D4#, which was prepared using the following method:

[0188] (1) Preparation of base fabric layer

[0189] 45% 1000D*1000D polyester chemical fiber yarn and 55% glass fiber are mixed and spun, and then formed by a 10-section needle plate forming machine with a speed of 25m / min. The temperatures are set to 100℃, 180℃, 210℃, 220℃, 220℃, 220℃, 210℃, 190℃, 180℃ and 100℃ in sequence to obtain a base fabric layer.

[0190] (2) Preparation of hand-feel coating

[0191] 50 parts of silicone modified waterborne polyurethane, 100 parts of water and 10 parts of cellulose were mixed evenly according to weight, and coated on one side of the base fabric layer by screen coating. The coating wet weight of the hand-feel coating was 35 gsm, the coating speed was 100 m / min, the coating thickness was 10 μm, and then the coating was cross-linked and cured in 10 ovens. The oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C respectively.

[0192] (3) Preparation of adhesion enhancing coating

[0193] According to weight parts, 100 parts of aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, and 40 parts of decabromodiphenylethane were mixed evenly, the pH was adjusted to 7-8, and then 6 parts of alkali swelling and associative compound thickener and 1 part of defoamer were slowly added and mixed evenly, and the viscosity was adjusted to 15000-20000cps / 4#, 30rpm, and a 1mm scraper coating method was adopted. The coating wet weight was 100gsm, the coating speed was 10m / min, the coating thickness was 10μm, and it was coated on the surface of the hand feel coating. It was cured in a 10-section oven, and the oven temperatures were set to 90°C, 100°C, 120°C, 160°C, 160°C, 150°C, 150°C, 120°C and 100°C in sequence to form an adhesion enhanced coating.

[0194] (4) Preparation of thermal insulation coating I

[0195] According to weight parts, 100 parts of water-based acrylic self-crosslinking textile emulsion with a TG value of -30°C to -15°C, 100 parts of water, 5 parts of modified aluminum hydroxide, 5 parts of antimony trioxide, 5 parts of decabromodiphenylethane, and 3 parts of core-shell titanium dioxide are mixed evenly, the pH is adjusted to 7-8, the viscosity is adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content is 45%±5. A 5mm E-type knife is used to apply it on the surface of the adhesion enhancing coating through gap coating. The wet coating amount is 200gsm, the vehicle speed is 20m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90°C, 100°C, 120°C, 130°C, 130°C, 130°C, 130°C, 130°C, 110°C and 100°C in sequence to form a thermal insulation coating I.

[0196] (5) Preparation of thermal insulation coating II

[0197] According to weight parts, 100 parts of water-based acrylic self-crosslinking textile emulsion with a TG value of -30°C to -15°C, 100 parts of water, 5 parts of modified aluminum hydroxide, 5 parts of antimony trioxide, 5 parts of decabromodiphenylethane, and 3 parts of core-shell titanium dioxide are mixed evenly, the pH is adjusted to 7-8, the viscosity is adjusted to 5000-7000cps / 4# with an alkali swelling thickener, 30rpm, and the solid content of the coating is 45%±5. A 5mm E-type knife is used to apply it on the surface of the thermal insulation coating I through a gap coating method. The wet coating amount is 200gsm, the vehicle speed is 20m / min, and it is dried in a 10-section oven. The oven temperatures are set to 90°C, 100°C, 120°C, 130°C, 130°C, 130°C, 130°C, 130°C, 110°C and 100°C in sequence to form a thermal insulation coating II.

[0198] (6) Preparation of waterproof spray coating

[0199] According to weight parts, 200 parts of silicone modified waterborne polyurethane emulsion with a TG value of 5°C-20°C, 200 parts of water, 20 parts of modified aluminum hydroxide, 20 parts of antimony trioxide, 40 parts of decabromodiphenylethane, 15 parts of nano silicon dioxide, 10 parts of nano modified wax powder, 6 parts of polyurethane thickener and 1 part of defoamer are mixed evenly, and the viscosity is adjusted to 15000-20000cps / 4#, 30rpm, and the solid content of the top coating is 35%±5. A 1mm scraper coating method is adopted, the wet coating amount is 60gsm, the vehicle speed is 10m / min, and the coating thickness is 10μm. It is coated on the surface layer of the thermal insulation coating II, and is cured in a 10-section oven. The oven temperatures are set to 90°C, 100°C, 120°C, 130°C, 130°C, 130°C, 130°C, 130°C, 110°C and 100°C in sequence to form a waterproof spray coating.

[0200] (7) Preparation of composite coating

[0201] 200 parts of water-based polyurethane emulsion with a TG value of 5°C-20°C and 30 parts of low-melting-point PA powder were mixed according to weight, and the viscosity was adjusted to 5000-6000cps / 4#. The coating with a solid content of 55%±5 was prepared at 60rpm and a laminating speed of 8m / min. The uncoated side of the base fabric layer was coated with 20gsm of glue and 5μm of thickness by roller transfer coating and 150°C roller heating. The materials were compounded together to obtain a highly flame-retardant, foldable, and heat-insulating double-sided inkjet material D4#.

[0202] The performance tests were performed on the inkjet materials prepared by the preparation processes of Examples 2-5 and Comparative Examples D1-D4. The flame retardant properties of the inkjet materials were evaluated according to German DIN 4102 and American NFPA 701. The wrinkle resistance of the inkjet materials was evaluated according to GB / T 29257-2012. The thermal insulation properties of the inkjet materials were evaluated based on the comparative thermal insulation effects. The specific thermal insulation effect test method is as follows:

[0203] Test samples 1-7 are 20-foot standard container-converted simple houses, and the surroundings and tops of the simple houses are sprayed with the spraying materials of Examples 2-5 and Comparative Examples D1-D4, respectively. The standard sample is a 20-foot standard container-converted simple house, and the external environment is: sunny summer, noon, the external temperature is 37-39°C, and the insulation level is marked by comparing the indoor temperature difference between test samples 1-7 and the standard sample. The test results are shown in Table 1.

[0204] Table 1

[0205]

[0206] It can be seen from Table 1 that the inkjet materials obtained in Examples 2-5 have excellent flame retardancy, wrinkle resistance, thermal insulation and printing performance, especially the wall cloth prepared by the preparation process of Example 5 has the best comprehensive performance, while the inkjet materials obtained in Comparative Examples D1-D4 have significantly lower flame retardancy, wrinkle resistance, thermal insulation and printing performance than those in Examples 2-5.

[0207] In the preparation process of comparative example D1, the base fabric layer was not subjected to high temperature setting, and the proportion of the coating of the hand-feel layer was not within the scope of protection of this application, resulting in a significant decrease in the wrinkle resistance of the obtained inkjet material. Therefore, the base fabric layer was customized by blending polyester chemical fiber and glass fiber, which enhanced the fireproof level of the substrate, improved the good folding resistance of the product, and gave the product good dimensional stability through high temperature setting at 220°C. The hand-feel coating contained silicone-modified waterborne polyurethane and was coated on the surface of the base fabric layer by screen coating, which reduced the penetration of latex. Through cross-linking and curing treatment, the material was further provided with good flexibility and folding resistance, and the material was foldable.

[0208] In the preparation process of Comparative Example D2, the modified polyurethane emulsion in the waterproof spray coating was replaced with an ordinary unmodified polyurethane emulsion, and in Comparative Example D3, no nano wax powder was added to the waterproof spray coating, which resulted in reduced printing performance of the prepared spray material. Therefore, the waterproof spray coating gives the spray material a good water-repellent effect, effectively prevents rainwater from infiltrating, and provides a printing coating for UV, weak solvent, and Latex ink, achieving the compatibility of isolating rainwater and being printable, thereby increasing the practicality of the material.

[0209] In the preparation process of comparative example D4, no compounded nano-silica aerogel powder and nano-glass microbeads were added to the coatings in thermal insulation coating I and thermal insulation coating II, and the proportion in the coatings was not within the protection scope of this application, and no microsphere foaming was performed, and the flame retardant and heat insulation effects were greatly reduced. Therefore, thermal insulation coating I and thermal insulation coating II form a microporous structure through microsphere foaming technology, which increases the thickness of the material and a better feel, and provides a good heat insulation effect for the material. The coating further improves the heat insulation effect of the product by compounding nano-silica aerogel powder and nano-glass microbeads. At the same time, the coating provides a good flame retardant effect for the product by compounding modified aluminum hydroxide, antimony trioxide, and decabromodiphenylethane flame retardant.

[0210] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A highly flame-retardant, foldable, heat-insulating, double-sided inkjet printing material, characterized in that: The inkjet printing material comprises two base fabric layers and a composite coating, and a single side of each base fabric layer is coated with a hand-feel coating, an adhesion enhancing coating, a heat-insulating coating I, a heat-insulating coating II, and a waterproof inkjet printing coating in sequence; The composite coating is to composite the uncoated sides of the two base fabric layers; the base fabric layer is composed of 40%-50% polyester fiber and 50%-60% glass fiber; the coating for the hand-feel coating includes the following components in parts by weight: 30-50 parts of silicone-modified water-based polyurethane, 100 parts of deionized water, and 3-10 parts of cellulose; the coating for the thermal insulation coating I and the thermal insulation coating II includes the following components in parts by weight: 200-300 parts of water-based acrylic self-crosslinking textile emulsion with a TG value of -30°C to -15°C, 200-300 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 40-60 parts of nano-silicon dioxide aerogel powder, 20-40 parts of nano-glass microspheres, 20-40 parts of core-shell titanium dioxide, and 12-20 parts of microsphere foaming agent; the coating for waterproof spray coating comprises the following components in parts by weight: 100-200 parts of silicone-modified waterborne polyurethane emulsion with a TG value of 5°C-20°C, 60-200 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 5-15 parts of nano-silicon dioxide, 5-10 parts of nano-modified wax powder, 3-6 parts of polyurethane thickener, and 0.6-1 part of defoaming agent.

2. The highly flame-retardant, foldable, heat-insulating, double-sided spray-painted material according to claim 1, characterized in that: The coating for adhesion enhancement coating comprises the following components in parts by weight: 50-100 parts of aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 6-10 parts of alkali swelling and associative composite thickener, and 0.6-1 part of defoamer.

3. The highly flame-retardant, foldable, heat-insulating, double-sided inkjet printing material according to claim 1, characterized in that: The composite coating paint comprises the following components in parts by weight: 100-200 parts of waterborne polyurethane emulsion with a TG value of 5° C.-20° C. and 10-30 parts of low melting point PA powder.

4. The preparation process of the highly flame-retardant, foldable, heat-insulating double-sided inkjet printing material according to any one of claims 1 to 3, characterized in that: The preparation process comprises the following steps: (1) Preparation of base fabric layer 40%-50% polyester chemical fiber yarn and 50%-60% glass fiber are mixed and spun, and then shaped; (2) Preparation of hand-feel coating 30-50 parts of silicone-modified waterborne polyurethane, 100 parts of water, and 3-10 parts of cellulose are mixed evenly by weight, coated on one side of the base fabric layer by screen coating, and then cross-linked and cured to form a hand-feel coating; (3) Preparation of adhesion enhancing coating 50-100 parts of an aqueous polyurethane emulsion with a TG value of -35°C-0°C, 100 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 6-10 parts of an alkali swelling and associative compound thickener, and 0.6-1 part of a defoamer are mixed uniformly according to weight parts, the viscosity is adjusted, and the mixture is applied on the surface of the hand-feel coating by a doctor blade coating method, dried and cured to form an adhesion-enhancing coating; (4) Preparation of thermal insulation coating I 200-300 parts of water-based acrylic self-crosslinking textile emulsion with a TG value of -30°C to -15°C, 200-300 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 40-60 parts of nano-silicon dioxide aerogel powder, 20-40 parts of nano-glass microbeads, 20-40 parts of core-shell titanium dioxide, and 12-20 parts of microsphere foaming agent are mixed uniformly according to weight parts, the pH is adjusted to 7-8, the viscosity is adjusted, and the coating is applied on the surface of the adhesion enhancing coating by an E-type knife gap coating method, dried and cured, and then foamed at 190-210°C to form a heat insulation coating I; (5) Preparation of thermal insulation coating II According to weight parts, 200-300 parts of water-based acrylic self-crosslinking textile emulsion with a TG value of -30°C to -15°C, 200-300 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 40-60 parts of nano-silicon dioxide aerogel powder, 20-40 parts of nano-glass microbeads, 20-40 parts of core-shell titanium dioxide, and 12-20 parts of microsphere foaming agent are mixed evenly, the pH is adjusted to 7-8, the viscosity is adjusted, and then the mixture is coated on the surface of the thermal insulation coating I by an E-type knife gap coating method, dried and cured, and then foamed at 190-210°C to form a thermal insulation coating II; (6) Preparation of waterproof spray coating 100-200 parts of organosilicon-modified waterborne polyurethane emulsion with a TG value of 5°C-20°C, 60-200 parts of water, 10-20 parts of modified aluminum hydroxide, 10-20 parts of antimony trioxide, 20-40 parts of decabromodiphenylethane, 5-15 parts of nano-silicon dioxide, 5-10 parts of nano-modified wax powder, 3-6 parts of polyurethane thickener, and 0.6-1 part of defoamer are mixed evenly according to weight parts, and after adjusting the viscosity, the mixture is applied on the surface of the thermal insulation coating II by a doctor blade coating method, and then cured to form a waterproof spray coating; (7) Preparation of composite coating 100-200 parts of aqueous polyurethane emulsion with a TG value of 5°C-20°C and 10-30 parts of low melting point PA powder are mixed evenly according to weight, and the viscosity is adjusted. The uncoated sides of the two base fabric layers are laminated by a laminating machine through roller heating.

5. The preparation process of the highly flame-retardant, foldable, heat-insulating double-sided inkjet printing material according to claim 4, characterized in that: The steps (1) to (6) are all dried and cured in a 10-section oven.

6. An application of the highly flame retardant, foldable, heat-insulating double-sided inkjet printing material as described in any one of claims 1 to 3, and / or the highly flame retardant, foldable, heat-insulating double-sided inkjet printing material prepared by the preparation process of the highly flame retardant, foldable, heat-insulating double-sided inkjet printing material as described in any one of claims 4 to 5 in insulation materials for heat-insulating tents, simple steel structure houses, and indoor and outdoor advertising.