A method and system for accelerated corrosion testing of steel wires inside cables

By adding a corrosion solution to the main test frame and combining it with non-destructive testing, the problem of accurately detecting the corrosion state of the steel wires inside the cable in the existing technology has been solved, and the accurate simulation of the corrosion morphology of the steel wires inside the cable and the reliability of the test results have been improved.

CN117347248BActive Publication Date: 2026-11-17HUAZHONG UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311130668.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-04
Publication Date
2026-11-17
Estimated Expiration
2043-09-04

AI Technical Summary

Technical Problem

Existing technologies are insufficient to accurately detect the corrosion state of the steel wires inside cables, especially in complex natural environments. Furthermore, the results of non-destructive testing methods depend on the professional competence of the testing personnel and are subject to randomness, making it impossible to effectively simulate the real corrosion scenario of cables.

Method used

By fabricating anchored and anchorless cables, different types of damage were simulated. Corrosion was accelerated by dripping a corrosion solution onto the main test frame. The relationship between the corrosion state of the steel wires inside the cables and the results of non-destructive testing was studied by combining non-destructive testing and observable dissection.

Benefits of technology

It achieves accurate simulation of the corrosion morphology of steel wires inside the cable, simplifies the detection process, improves the reliability and accuracy of the detection results, and enables the calibration of the corrosion state of steel wires inside the cable in non-destructive testing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117347248B_ABST
    Figure CN117347248B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of accelerated corrosion testing of cables, and specifically discloses a method and system for accelerated corrosion testing of steel wires inside cables. The method includes: cables to be tested, including long cables with anchor heads, long cables without anchor heads, and short cables without anchor heads; multiple cables of each type are prepared, and damage is created on their PE sheaths; the cables to be tested are placed on a main test frame, and a corrosive solution is continuously dripped onto the damaged areas of the cables. During the corrosion process: the signals of each long cable with and without anchor heads are monitored using non-destructive testing; simultaneously, the short cables without anchor heads are dissected at preset time intervals, and the corrosion state of their internal steel wires is recorded after dissection; after all the short cables without anchor heads have been dissected, the dripping of the corrosive solution is stopped; the corrosion state of the internal steel wires of the short cables without anchor heads is combined with the non-destructive testing results to study the correspondence between different corrosion states of the internal steel wires and the non-destructive testing results. This invention can provide a basis for the evaluation of non-destructive testing results of cable corrosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of accelerated corrosion testing of cables, and more specifically, relates to a method and system for accelerated corrosion testing of steel wires inside cables. Background Technology

[0002] Cables are an important component and main load-bearing structure of cable-stayed bridges, suspension bridges, and arch bridges, and their health directly affects the safe operation and service life of the bridge. Since cables are generally exposed to the natural environment, especially in areas with severe air pollution, severe water pollution, coastal and marine environments, the steel wires inside the cables are highly susceptible to environmental corrosion when their anti-corrosion system is damaged during construction or fatigue caused by alternating loads.

[0003] The degree of corrosion of the internal steel wires in a cable corresponds to different safety risk levels for the bridge structure. The development of corrosion within the internal steel wires of a cable is a complex and slow chemical reaction process, and the corrosion progress and morphological changes of cables in service bridges cannot be directly observed due to the PE sheath. Widely used non-destructive testing methods for cable corrosion, such as guided wave testing (for detecting corrosion damage in the cable anchorage zone) and magnetic flux leakage testing (for detecting corrosion damage in the free section of the cable), all encounter calibration difficulties when performing quantitative analysis of cable corrosion. Generally, the presence and severity of corrosion are determined based on experience or by methods such as opening windows in the PE sheath. Therefore, the test results heavily depend on the professional competence of the inspectors and are subject to randomness. Furthermore, opening windows in the cable for verification causes additional damage to the cable. In addition, although there are many studies on the corrosion of individual steel wires, bars, and strands, the corrosion development state of cables within the cable, due to the contact between the steel wires and the constraint of the PE sheath, differs significantly from that of individual steel wires, bars, and strands. The data collected by non-destructive testing methods is more complex and more difficult to analyze. Summary of the Invention

[0004] In view of the above-mentioned defects or improvement needs of the existing technology, the present invention provides a method and system for accelerated corrosion testing of steel wires inside cables. The purpose is to make the corrosion morphology of steel wires inside cables approximate the real corrosion scenario, and to achieve accurate corrosion detection of cables by combining non-destructive testing and observable dissection.

[0005] To achieve the above objectives, according to one aspect of the present invention, a method for accelerating corrosion testing of steel wires inside a cable is provided, comprising the following steps:

[0006] Fabrication of test cables: The test cables include long cables with anchor heads, long cables without anchor heads, and short cables without anchor heads; multiple cables of each type are prepared, and damage is created on their PE sheaths;

[0007] The cables to be tested were placed on the main test frame, and a corrosive solution was continuously dripped onto the damaged areas of the cables to accelerate corrosion. During the accelerated corrosion process, the signals of each long cable with and without anchor heads were monitored using non-destructive testing. At the same time, the short cables without anchor heads were dissected in stages at preset time intervals, and the corrosion status of the internal steel wires of the short cables without anchor heads was recorded after dissection. After all the short cables without anchor heads were dissected, the dripping of the corrosive solution was stopped.

[0008] The corrosion state of the internal steel wires of the short cable without anchor head after different corrosion durations was equated with the corrosion state of the internal steel wires of the long cable with anchor head and the long cable without anchor head at the corresponding time. The correlation between the different corrosion states of the internal steel wires of the cable and the non-destructive testing results was studied by combining them with the non-destructive testing results.

[0009] As a further preferred option, each type of cable to be tested is provided in an array, with each array including one cable to be tested with PE sheath having circumferential cracks, axial cracks, and partial damage from a vehicle collision.

[0010] As a further preferred embodiment, the cable to be tested is placed at an angle, and any damage on the PE sheath is located at the lower part of the cable to be tested.

[0011] As a further preferred option, before starting to drip the corrosive solution, a liquid accumulation ring is placed at the circumferential crack damage site, a liquid accumulation strip is placed at the axial crack damage site, and a liquid accumulation bag is placed at the local damage site from the vehicle collision.

[0012] As a further preferred option, after corrosion is completed, the long cables with anchor heads and the long cables without anchor heads are dissected and the corrosion state of the internal steel wires is recorded after dissection, so as to compare and analyze the difference in corrosion state between the steel wires in the free section of the cable and the steel wires in the anchorage area under the same corrosion conditions.

[0013] As a further preferred method, the recorded internal steel wire corrosion status after dissection includes: photographing the steel wire inside the cable, collecting corrosion products, and recording the depth of corrosion pits, distribution of corrosion pits, and axial corrosion length of the steel wire, and weighing them.

[0014] According to another aspect of the present invention, a system for implementing the above-described accelerated corrosion test method for internal steel wires of a cable is provided, comprising a main test frame, a corrosion dripping device, and a non-destructive testing device, wherein:

[0015] The main test frame has a triangular structure, and the cable to be tested is placed on the inclined surface of the main test frame.

[0016] The corrosion dripping device is installed above the main test frame and is used to continuously drip corrosion solution onto the damaged area of ​​the cable to be tested.

[0017] The non-destructive testing device is used to monitor the signals of each anchored and unanchored long cable through non-destructive testing.

[0018] As a further preferred embodiment, the main test frame is provided with positioning plates and limiting plates. The limiting plates are used to prevent the cables to be tested from rolling and to determine the spacing between the cables to be tested. The positioning plates are used to prevent the cables to be tested from sliding axially.

[0019] As a further preferred embodiment, the main test frame is also provided with an adjustment plate, which is used to adjust the limiting piece so that the limiting piece can better fix the anchorless long cable.

[0020] As a further preferred embodiment, the corrosion dripping device includes a plastic bucket and an infusion tube. The plastic bucket is used to hold the corrosion solution and has graduations on its body and a side water outlet at the bottom. The thicker end of the infusion tube is connected to the side water outlet at the bottom of the plastic bucket, and the other end is fixed to the damaged part of the PE sheath of the cable to be tested. The infusion tube is equipped with a flow regulator.

[0021] In summary, compared with the prior art, the above-described technical solutions conceived by this invention mainly possess the following technical advantages:

[0022] 1. This invention provides a method for simulating the accelerated corrosion of steel wires inside the free section and anchorage zone of a cable in a natural environment. The test operation is simple and safe, the corrosion rate is controllable, and the corrosion morphology of the steel wires inside the cable can be made close to the real corrosion scenario. Combined with non-destructive testing and observable dissection, accurate corrosion detection of the cable can be achieved.

[0023] 2. This invention uses anchored long cables, anchorless long cables, and anchorless short cables for comparison. Specifically, by dissecting the short cables at regular intervals, the corrosion of the internal steel wires of the short cables under different corrosion durations is observed. The corrosion state of the internal steel wires of the short cables is equated to the corrosion state of the internal steel wires of anchored and anchorless long cables under the same corrosion conditions (corrosion duration and corrosion environment). At the same time, non-destructive testing is continuously performed on both anchored and anchorless long cables. After corrosion is completed, by comparing the dissection observation results of different batches of short cables with the corresponding non-destructive testing results of anchored and anchorless long cables, the corrosion state of the internal steel wires of the cables can be calibrated.

[0024] 3. By comparing long cables with anchor heads and long cables without anchor heads, the differences in corrosion state between the free section wires and the wires in the anchorage zone of the cable under the same corrosion conditions (corrosion duration and corrosion environment) can be analyzed.

[0025] 4. Common PE sheath damage to bridge cables includes circumferential cracking, axial cracking, and localized damage caused by vehicle collisions. Harmful substances in the natural environment can enter the cable body through the PE sheath damage and corrode the internal steel wires. This invention accurately simulates the cable corrosion caused by these three types of PE sheath damage. At the same time, the cable tilt more realistically simulates the state of cables in service bridges, and the PE sheath damage is located at the lower part of the cable, which matches the actual damage situation of cables in service bridges and facilitates non-destructive testing. Attached Figure Description

[0026] Figure 1 This is a schematic diagram of the main test frame structure according to an embodiment of the present invention, wherein (a)-(c) are the main test frames applicable to long cables with anchor heads, long cables without anchor heads, and short cables without anchor heads, respectively;

[0027] Figure 2 This is a schematic diagram of the corrosion dripping device according to an embodiment of the present invention;

[0028] Figure 3 This is a schematic diagram of the test frame and corrosion dripping device according to an embodiment of the present invention;

[0029] Figure 4 This is a schematic cross-sectional view of the corrosion state of the steel wires inside the cable according to an embodiment of the present invention;

[0030] Figure 5 This is a diagram showing the arrangement of the guided wave nondestructive testing transducer according to an embodiment of the present invention;

[0031] Figure 6 This is a schematic diagram of the internal steel wires of the short cable body after 30 days of corrosion, according to an embodiment of the present invention.

[0032] Figure 7 This is a comparison diagram of the reference signal obtained by the guided wave nondestructive testing method in this embodiment of the invention and the signal after 30 days of corrosion.

[0033] In all the accompanying drawings, the same reference numerals are used to denote the same elements or structures, wherein: 1-plastic bucket, 2-infusion tube. Detailed Implementation

[0034] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.

[0035] This invention provides an accelerated corrosion testing system for the internal steel wires of a cable, comprising a main test frame, a corrosion dripping device, and a non-destructive testing device, wherein:

[0036] The main test frame has a triangular structure, which makes it more stable. The cable to be tested is placed on the inclined surface of the main test frame, so that the cable is placed at an angle. The corrosion dripping device is installed above the main test frame to continuously drip corrosion solution onto the damaged area of ​​the cable to be tested. The non-destructive testing device is used to monitor the signal of each cable to be tested through non-destructive testing.

[0037] Specifically, such as Figure 1 As shown, the test system consists of three main test frames:

[0038] The main test frame Y1 is used for corrosion tests on long cables with anchor heads, and it is equipped with positioning plates and limiting plates; the main test frame Y2 is used for corrosion tests on long cables without anchor heads, and it is equipped with positioning plates, limiting plates and adjusting plates; the test frame Y3 is used for corrosion tests on short cables without anchor heads, and it is equipped with positioning plates and limiting plates.

[0039] The main test frame is constructed entirely of welded angle steel and is used to determine the cable inclination angle and bear the cable's weight. Limiting and positioning plates are used to define the cable's position on the main test frame. Positioning plates prevent axial slippage of the cable, while limiting plates prevent cable rolling and limit the spacing between cables on the test frame. Because long, anchorless cables are difficult to fix due to the lack of anchors and their considerable length, an adjusting plate is also installed on the main test frame Y2. The limiting plates are connected to the adjusting plate via bolts, allowing the cable to be fixed by adjusting the limiting plates on the upper part of the test frame Y2.

[0040] The corrosion dripping device consists of a plastic bucket and an infusion tube. The plastic bucket has a lid, graduations on its body, and a side outlet at the bottom for holding the corrosion solution. The thicker end of the infusion tube is connected to the side outlet at the bottom of the plastic bucket, and the other end is fixed to the notch in the PE sheath of the cable. The dripping rate of the corrosion solution is adjusted by a flow regulator on the infusion tube.

[0041] Non-destructive testing devices include, but are not limited to, guided wave non-destructive testing instruments and magnetic flux leakage testing instruments mounted on climbing robots.

[0042] The method for accelerated corrosion testing of the internal steel wires of the cable based on the above system includes the following steps:

[0043] S1. Prepare the cables to be tested: The cables to be tested include long cables with anchor heads, long cables without anchor heads, and short cables without anchor heads; multiple cables of each type are prepared, and damage is made on their PE sheaths.

[0044] Generally, common PE sheath damage to bridge cables includes circumferential cracking, axial cracking, and localized damage caused by vehicle collisions. Harmful substances from the natural environment can enter the cable body through PE sheath damage, corroding the internal steel wires. Cable corrosion experiments simulated cable corrosion caused by these three types of PE sheath damage. Therefore, the number of anchored cables, the number of long cable bodies, and the number of short cable bodies were all set to multiples of 3, i.e., i%3 = 0, j%3 = 0, k%3 = 0 (% is the remainder). Furthermore, the corrosion state of short cable bodies was analogous to that of anchored and long cable bodies. Therefore, short cable bodies were dissected after different corrosion durations to observe and record the corrosion of their internal steel wires. Thus, the number of short cable bodies was determined based on the corrosion duration and the number of observation nodes.

[0045] In some embodiments, the anchored long cable is divided into 3 groups. A 20mm wide annular notch is made on each cable of the first group to simulate circumferential cracking of the PE sheath of the cable. A 300mm long and 20mm wide strip notch is made on each cable of the second group to simulate axial cracking of the PE sheath of the cable. A 20mm diameter circular notch is made on each cable of the third group to simulate vehicle collision damage to the PE sheath of the cable. The depth of all notches is the thickness of the PE sheath, and the steel wire inside the cable is exposed at the notches.

[0046] The anchorless long cable body is divided into 3 groups. On each cable of the first group, a 20mm wide annular notch is made to simulate circumferential cracking of the PE sheath. On each cable of the second group, a long strip notch with an axial length of 300mm and a width of 20mm is made to simulate axial cracking of the PE sheath. On each cable of the third group, a 20mm diameter circular notch is made to simulate vehicle collision damage to the PE sheath. The depth of all notches is the thickness of the PE sheath, and the steel wire inside the cable is exposed at the notches.

[0047] The anchorless short cable body is divided into 3 groups. On each cable of the first group, a 20mm wide annular notch is made to simulate circumferential cracking of the PE sheath. On each cable of the second group, a 300mm long and 20mm wide strip notch is made to simulate axial cracking of the PE sheath. On each cable of the third group, a 20mm diameter circular notch is made to simulate vehicle collision damage to the PE sheath. The depth of all notches is the thickness of the PE sheath, and the steel wire inside the cable is exposed at the notches.

[0048] Simultaneously, liquid accumulation rings are placed at the annular notches of all cables, liquid accumulation strips are placed at the axial elongated notches of all cables, and liquid accumulation bags are placed at the circular notches of all cables. The liquid accumulation rings are made by wrapping cotton in gauze and then connecting and tying the two ends of the gauze together; the liquid accumulation strips are made by wrapping cotton in gauze and then tying the two ends together; and the liquid accumulation bags are made by wrapping cotton in gauze to form a spherical shape.

[0049] S2. Place the cables to be tested on the main test frame and prepare the corrosion solution.

[0050] The anchor cables M1, M2, ..., M i The cable bodies T1, T2, ..., T are fixed to the test frame Y1 using positioning and limiting plates; j The short cables D1, D2, ..., D are fixed to the test frame Y2 using positioning and limiting plates; k It is fixed on test frame Y3 of No. 3 by positioning plates and limiting plates.

[0051] The corrosive solution is prepared from chemically pure sodium chloride (5%), copper chloride dihydrate (0.03%), glacial acetic acid (0.6%), and distilled water (94.37%), with the pH value controlled between 3.1 and 3.5. The thicker end of the infusion tube is connected to the outlet on the bottom side of the plastic bucket, and the other end is fixed to the notch of the PE sheath of the cable. The drip rate of the corrosive solution is adjusted by the flow regulator on the infusion tube.

[0052] S3. Continuously drip a corrosive solution onto the damaged area of ​​the cable to be tested and monitor the signal of each cable to be tested using non-destructive testing methods; dissect the short cable without anchor head in stages according to the preset time interval and record the internal corrosion of the short cable without anchor head after dissection.

[0053] Before corrosion begins, initial signals of the anchored cable, long cable body, and short cable body are collected using non-destructive testing instruments as reference signals. During the corrosion process, the anchored cable, long cable body, and short cable body are tested with non-destructive testing instruments every N (N>=1) days to collect the required data.

[0054] At different corrosion stages of the cables, at least three short cable sections were dissected, including at least one cable with a circumferential notch, one cable with an axial notch, and one cable with a perforated notch. The internal corrosion of the cables was observed, and photographs of the internal steel wires were taken and recorded, including the depth of the corrosion pits, the length of the axial corrosion, and weighing data.

[0055] In some embodiments, the specific method is as follows:

[0056] (1) Ten days after the corrosion experiment was completed, at least three short cables were dissected, and the steel wires inside the short cables after the PE was removed were photographed. Corrosion products were collected, and the depth of corrosion pits, distribution of corrosion pits, and axial corrosion length of steel wires were recorded and weighed.

[0057] (2) After 25 days of corrosion experiment, dissect at least 3 short cables, take pictures of the steel wires inside the short cables after PE is removed, collect corrosion products, record the depth of corrosion pits, distribution of corrosion pits, and axial corrosion length of steel wires, and weigh them.

[0058] (3) 45 days after the corrosion experiment, dissect at least 3 short cables, take pictures of the steel wires inside the short cables after the PE is removed, collect corrosion products, record the depth of corrosion pits, distribution of corrosion pits, and axial corrosion length of steel wires, and weigh them.

[0059] (4) After 70 days of corrosion experiment, dissect at least 3 short cables, take pictures of the steel wires inside the short cables after PE is removed, collect corrosion products, record the depth of corrosion pits, distribution of corrosion pits, and axial corrosion length of steel wires, and weigh them.

[0060] (5) After 100 days of corrosion experiment, dissect at least 3 short cables, take pictures of the steel wires inside the short cables after PE removal, collect corrosion products, record the depth of corrosion pits, distribution of corrosion pits, and axial corrosion length of steel wires, and weigh them.

[0061] (6) The corrosion experiment continued until all the short cables were dissected.

[0062] S4. Equate the corrosion state of the steel wires inside short cables with different corrosion durations (including corrosion products, corrosion pit depth, corrosion pit distribution, axial corrosion length of steel wires, etc.) to the corrosion state of the steel wires inside long cables with and without anchor heads under the same corrosion conditions (corrosion duration and corrosion environment). Combine this with the results of non-destructive testing, extract feature quantities from the non-destructive testing signals to characterize the corrosion development process of the steel wires inside the cables, and realize the calibration of the corrosion state of the cables.

[0063] In addition, after the corrosion was completed, the long cables with anchor heads and the long cables without anchor heads were dissected and the corrosion state of the internal steel wires was recorded. This allowed for the analysis and comparison of the differences in corrosion state between the steel wires in the free section of the cable and the steel wires in the anchorage area under the same corrosion conditions (corrosion time and corrosion environment).

[0064] The following are specific examples:

[0065] An experimental apparatus for testing corrosion of steel wires inside cables, such as Figure 1 and Figure 3 As shown, the apparatus includes test frames Y1 to Y3 and a corrosion dripping device. Test frame Y1 is used to fix three long cables with anchor heads, M1, M2, and M3; test frame Y2 is used to fix three long cables without anchor heads, T1, T2, and T3; and test frame Y3 is used to fix 15 short cables without anchor heads, D1 to D3. 15 Among them, M1, T1, and D1-D5 have a 20mm wide annular notch on their PE sheaths, while M2, T2, and D6-D5 have a notch on their PE sheaths. 10 A long strip notch with an axial length of 300mm and a width of 20mm is made on the PE sheath, in M3, T3 and D. 11 ~D 15A 20mm diameter circular notch is made on the PE sheath. All cables are Φ7-61 parallel steel wire cables. Anchored cables M1, M2, and M3 are 6800mm long. Longer cables T1, T2, and T3 are also 6800mm long. Shorter cables D1 to D... 15 1000mm in length.

[0066] A liquid-collecting ring is wrapped around the annular notch of the PE sheath, a liquid-collecting strip is placed at the axial notch of the PE sheath, and a liquid-collecting bag is placed at the perforated notch of the PE sheath. The liquid-collecting ring is made by wrapping cotton in gauze and then connecting and tying the two ends of the gauze together; the liquid-collecting strip is made by wrapping cotton in gauze and then tying the two ends together; and the liquid-collecting bag is made by wrapping cotton in gauze into a spherical shape. Depending on the number of cables, seven liquid-collecting rings, seven liquid-collecting strips, and seven liquid-collecting bags are needed.

[0067] The corrosion dripping device is used to quantitatively control the dripping of corrosion solution into the accumulation ring, accumulation strip, and accumulation bag, as shown in the schematic diagram. Figure 2 As shown. The specific operation is as follows: Add acid solution to plastic bucket 1, and record the amount of acid added each time using the scale inside the bucket; connect the thicker end of the infusion tube 2 to the water outlet at the bottom of the plastic bucket, and fix the thinner end to the PE notch of the cable; adjust the drip rate of the acid solution using the flow regulator on the infusion tube, controlling the drip rate to about 35 drops per second. The acid solution is first dripped into the accumulating ring, accumulating strip, and accumulating bag, and then slowly seeps into the interior of the cable.

[0068] Cable body D1~D 15 After different corrosion times, the PE sheath was dissected in batches to observe and record the corrosion status of the internal steel wires. Figure 4 The diagram shows the corrosion state of the internal steel wires of a cable with a PE sheath and an annular notch after a period of corrosion. The outermost layer of steel wires is the most severely corroded, followed by the next outermost layer, with the degree of corrosion decreasing from the outside in. Figure 6 This diagram illustrates the corrosion state of the internal steel wires in a cable with a ring-shaped notch in the PE sheath after 25 days of corrosion. It shows that the outer steel wires are severely corroded, with a large amount of corrosion products adhering to them; obvious corrosion pits are visible at the PE notch; the internal steel wires only show discoloration of the galvanized layer, without significant rust. Cable body D1~D 15 The specific corrosion times are shown in Table 1:

[0069] Table 1 Corrosion Duration of Cables

[0070]

[0071] The corrosion level of the cable wire is assessed based on the maximum depth of corrosion pits in the wire, as shown in Table 2.

[0072] Table 2 Corrosion Level Assessment Standards

[0073]

[0074] During the corrosion experiment, magnetostrictive guided wave detection was performed on cables M1, M2, M3 and T1, T2, T3 at regular intervals. Figure 5 This is a diagram showing the layout of a magnetostrictive guided wave transducer for nondestructive testing. Figure 7 The initial signal (reference signal) of cable T1 before corrosion is compared with the signal after 25 days of corrosion. It can be seen that the echo at the lower end of cable T1 is attenuated due to internal corrosion of the cable.

[0075] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method of accelerated corrosion testing of the internal wires of a cable, characterized in that, Includes the following steps: Fabrication of test cables: The test cables include long cables with anchor heads, long cables without anchor heads, and short cables without anchor heads; multiple cables of each type are prepared, and damage is created on their PE sheaths; The cables to be tested were placed on the main test frame, and a corrosive solution was continuously dripped onto the damaged areas of the cables to accelerate corrosion. During the accelerated corrosion process, the signals of each long cable with and without anchor heads were monitored using non-destructive testing. At the same time, the short cables without anchor heads were dissected in stages at preset time intervals, and the corrosion status of the internal steel wires of the short cables without anchor heads was recorded after dissection. After all the short cables without anchor heads were dissected, the dripping of the corrosive solution was stopped. The corrosion state of the internal steel wires of the short cable without anchor head after different corrosion durations was equated with the corrosion state of the internal steel wires of the long cable with anchor head and the long cable without anchor head at the corresponding time. The correlation between the different corrosion states of the internal steel wires of the cable and the non-destructive testing results was studied by combining them with the non-destructive testing results.

2. The accelerated corrosion test method for the internal steel wires of a tensile cable according to claim 1, wherein Each type of cable to be tested is set up in an array, and each array includes one cable to be tested with PE sheath having circumferential cracks, axial cracks, and partial damage from a vehicle collision.

3. The accelerated corrosion test method for the internal steel wires of a tensile cable according to claim 2, characterized in that, The cable to be tested was placed at an angle, and all damage on the PE sheath was located at the lower part of the cable to be tested.

4. The accelerated corrosion test method for the internal steel wires of a tensile cable according to claim 2, characterized in that, Before starting to add the corrosive solution, place a liquid accumulation ring at the circumferential crack damage site, a liquid accumulation strip at the axial crack damage site, and a liquid accumulation bag at the local damage site from the vehicle collision.

5. The accelerated corrosion test method for the internal steel wires of a tensile cable according to claim 1, characterized in that, After corrosion was completed, the long cables with and without anchor heads were dissected and the corrosion state of the internal steel wires was recorded. This allowed for a comparative analysis of the differences in corrosion state between the steel wires in the free section and the steel wires in the anchorage zone under the same corrosion conditions.

6. The accelerated corrosion test method for the internal wire of a tensile cable according to any one of claims 1 to 5, characterized in that, The recorded internal steel wire corrosion status after dissection included: photographing the steel wire inside the cable, collecting corrosion products, and recording the depth, distribution, and axial corrosion length of the steel wire corrosion pits, as well as measuring and weighing them.

7. The accelerated corrosion test method for the internal steel wires of the cable as described in any one of claims 1-5, characterized in that, An accelerated corrosion test method for the internal steel wires of the cable was conducted based on a test system, which includes a main test frame, a corrosion dripping device, and a non-destructive testing device, wherein: The main test frame has a triangular structure, and the cable to be tested is placed on the inclined surface of the main test frame. The corrosion dripping device is installed above the main test frame and is used to continuously drip corrosion solution onto the damaged area of ​​the cable to be tested. The non-destructive testing device is used to monitor the signals of each anchored and unanchored long cable through non-destructive testing.

8. The accelerated corrosion test method for the internal steel wires of the cable as described in claim 7, characterized in that, The main test frame is equipped with positioning plates and limiting plates. The limiting plates are used to prevent the cables to be tested from rolling and to determine the spacing between the cables to be tested. The positioning plates are used to prevent the cables to be tested from sliding axially.

9. The accelerated corrosion test method for the internal steel wires of the cable as described in claim 8, characterized in that, The main test frame is also equipped with an adjustment plate, which is used to adjust the limiting plate so that the limiting plate can better fix the anchorless long cable.

10. The accelerated corrosion test method for the internal steel wires of the cable as described in claim 7, characterized in that, The corrosion dripping device includes a plastic bucket and an infusion tube. The plastic bucket is used to hold the corrosion solution. The plastic bucket has graduations and a side water outlet at the bottom. The thicker end of the infusion tube is connected to the side water outlet at the bottom of the plastic bucket, and the other end is fixed to the damaged part of the PE sheath of the cable to be tested. The infusion tube is equipped with a flow regulator.

Citation Information

Patent Citations

  • Detection for corrosion of stayed cable and evaluation method thereof

    CN102313680A

  • Many parameter adjustment's disconnected silk test system of bridge cable pole corrosion