A food grade medium molecular weight polyisobutylene and its preparation and application

Through the compounding of ferric chloride hexahydrate and anhydrous ferric chloride and the low-temperature aging complexation of ketones, ethers, and amides, a highly reactive catalytic system is formed, which solves the problem of difficulty in removing traditional catalysts. It achieves the preparation of narrow molecular weight distribution and high conversion rate of food-grade medium molecular weight polyisobutylene, which is suitable for the food field.

CN117362495BActive Publication Date: 2024-10-18ZHEJIANG CENWAY MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311489164.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-09
Publication Date
2024-10-18
Estimated Expiration
2043-11-09

AI Technical Summary

Technical Problem

In the synthesis process of medium molecular weight polyisobutylene, traditional catalysts are difficult to remove, resulting in metal residues and affecting the quality of food-grade products.

Method used

By compounding ferric chloride hexahydrate and anhydrous ferric chloride, combining ketones, ethers and amides as initiators, and performing low-temperature aging complexation, a catalytic system with high reactivity and no heavy metals is formed. Suppress the chain transfer phenomenon and achieve the preparation of medium molecular weight polyisobutylene with narrow molecular weight distribution.

Benefits of technology

It significantly reduces the amount of metal residues, improves the conversion rate and molecular weight distribution control of the product, simplifies the post-processing steps, and realizes the green preparation of food-grade medium molecular weight polyisobutylene, which is suitable for the food field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117362495B_ABST
    Figure CN117362495B_ABST
Patent Text Reader

Abstract

The embodiment of the present invention discloses a food-grade medium molecular weight polyisobutylene and its preparation and application. The chemical formula of the polyisobutylene is ‑[CH2‑C(CH3)2] n ‑. The preparation method comprises: preparing an initiator system; adding a third component to the initiator system to initiate monomer polymerization to prepare food-grade medium molecular weight polyisobutylene; the initiator system comprises ferric chloride hexahydrate and anhydrous ferric chloride, and also comprises a solvent; the third component comprises at least one of a ketone compound, an ether compound and an amide compound; the monomer is selected from isobutylene compounds; the temperature range of the monomer polymerization reaction is between ‑30°C and ‑80°C. The present invention uses ferric chloride hexahydrate and anhydrous ferric chloride as initiators, and a high reaction activity can be formed through low-temperature aging and complexation. Under the action of the third component, the phenomenon of chain transfer that is easy to occur in cationic polymerization is suppressed, and the narrow molecular weight distribution preparation of food-grade medium molecular weight polyisobutylene is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high molecular weight polymer preparation, and in particular to food-grade medium molecular weight polyisobutylene and preparation and application thereof. Background Art

[0002] Polyisobutylene is a product obtained by cationic polymerization of isobutylene monomer, and is a linear saturated polymer. Polyisobutylene has three molecular weight products: high, medium and low. High molecular weight polyisobutylene is a white solid, and medium molecular weight polyisobutylene is a semi-solid with a glass transition temperature of 198K-243K. It can still maintain elasticity at -50°C and has excellent weather resistance, insulation performance, cold flow, UV resistance and chemical inertness. Among them, medium molecular weight polyisobutylene is widely used in shock-absorbing and damping adhesives, pressure-sensitive adhesives, chewing gum and other fields. Food-grade medium molecular weight polyisobutylene is an important branch of downstream applications of polyisobutylene products, and the market demand is huge, but the product is required to be tasteless and non-biotoxic, free of any heavy metals, and will not pose a potential hazard to the human body.

[0003] In the synthesis process of medium molecular weight polyisobutylene, AlCl3, BF3, etc. are usually used as cationic polymerization initiators. These catalysts are highly toxic. The key is that the initiators are difficult to remove, resulting in a high residual metal content in the material, which will have a great impact on the quality of the product, especially the quality of materials used in the food field.

[0004] In the prior art, there is a method of preparing medium molecular weight polyisobutylene at a relatively high temperature by reacting FeCl3 with an oxygen-containing compound in a second organic solvent to form a FeCl3 complex, and then adding titanium tetrachloride to the mixture to obtain a composite initiator solution, but this method does not completely get rid of the use of heavy metal catalysts. There is also a method of preparing high-reactivity polyisobutylene and copolymers thereof with a number average molecular weight of 500 to 6000 g / mol by using an initiation system composed of FeCl3 and a complexing agent, but the core idea of ​​this method is to promote chain transfer to obtain a low molecular weight product, which does not provide a new method for preparing medium molecular weight polyisobutylene. Summary of the invention

[0005] The object of the present invention is to provide a food-grade medium molecular weight polyisobutylene and its preparation and application, so as to solve at least one of the above-mentioned technical problems. On the basis of being able to suppress the chain transfer phenomenon that is easy to occur in cationic polymerization, the green preparation of medium molecular weight polyisobutylene is achieved, while avoiding metal residues.

[0006] The embodiment of the present invention is achieved as follows:

[0007] A food grade medium molecular weight polyisobutylene, wherein the chemical formula of the polyisobutylene is -[CH2-C(CH3)2]n -, where n is in the range of 180 <n<1800;

[0008] The polyisobutylene contains Mn, and the content of Mn ranges from 10000 to 100000 g / mol;

[0009] Preferably, the content of Mn is 20000 g / mol, 30000 g / mol, or 40000 g / mol.

[0010] The molecular weight distribution of the polyisobutylene is between 1.0 and 1.5.

[0011] A method for preparing food-grade medium molecular weight polyisobutylene, comprising:

[0012] Configure the initiator system;

[0013] A third component is added to the initiator system to initiate monomer polymerization to prepare food-grade medium molecular weight polyisobutylene;

[0014] The initiator system includes ferric chloride hexahydrate and anhydrous ferric chloride, and also includes a solvent;

[0015] The third component includes at least one of a ketone compound, an ether compound and an amide compound;

[0016] The monomer is selected from isobutylene compounds;

[0017] The temperature range of the monomer polymerization reaction is -30°C to -80°C;

[0018] The polyisobutylene is the polyisobutylene described above.

[0019] Wherein, the monomer polymerization reaction is a cationic polymerization reaction of the monomer.

[0020] Among them, by adding the third component, the carbon cation active center is stabilized, the occurrence of chain transfer is inhibited, and narrow molecular weight distribution control can be achieved.

[0021] The product conversion rate of the medium molecular weight polyisobutylene prepared by the present invention is above 85%.

[0022] The residual metal ion content in the medium molecular weight polyisobutylene prepared by the present invention is only 10% of the residual content of other traditional catalysts. The residual metal ions in the polymer can be quickly removed in a simple post-treatment process, and the final ion removal rate can reach 100%.

[0023] In a preferred embodiment of the present invention, in the method for preparing the above-mentioned food-grade medium molecular weight polyisobutylene, the ferric chloride hexahydrate in the initiator system is ferric chloride saturated with crystal water, which is prepared by precipitation of ferric chloride from an aqueous solution, and has a chemical formula of FeCl3·6H2O;

[0024] The anhydrous ferric chloride in the initiator system is an ionic crystal, which is obtained by heating ferric chloride hexahydrate and removing the water in the ferric chloride saturated with water of crystallization, and has a chemical formula of FeCl3.

[0025] Ferric chloride is a new type of green initiator suitable for cationic polymerization. When ferric chloride is precipitated from aqueous solution, it carries six crystal waters, namely FeCl3·6H2O. Ferric chloride hexahydrate is orange-yellow crystals. After heating to remove the water in the crystals, black-brown ionic crystals of anhydrous ferric chloride are obtained.

[0026] However, in ferric chloride hexahydrate, the molar ratio of crystal water is excessive and cannot be directly used as a polymerization initiator. Therefore, we innovatively compounded ferric chloride hexahydrate with anhydrous ferric chloride, so that the reaction system no longer needs to add additional initiators, simplifying the experimental steps.

[0027] This compound catalyst system is a green catalytic system, does not contain heavy metals, and can produce high reaction activity with a very small amount of addition through low-temperature aging and complexation, which is much higher than traditional Lewis acids such as TiCl4 and BF3.

[0028] The new efficient catalytic system formed by the combination of ferric chloride saturated with crystal water and anhydrous ferric chloride can not only solve the drawbacks of the traditional catalytic system, such as large dosage and metal ions that are difficult to remove, but also can stabilize the active center under the action of the third component, realize fast initiation and growth in the polymerization process, and achieve narrow molecular weight distribution control of the product.

[0029] The technical effect is that by selecting different forms of ferric chloride and using hexahydrate ferric chloride and anhydrous ferric chloride in the preparation process, the initiator system is optimized, which helps to control and improve the preparation process of food-grade medium molecular weight polyisobutylene.

[0030] In a preferred embodiment of the present invention, in the method for preparing the above-mentioned food-grade medium molecular weight polyisobutylene, in the initiator system, the molar ratio of the ferric chloride hexahydrate to the anhydrous ferric chloride is 1:(5-29).

[0031] Preferably, the molar ratio of the ferric chloride hexahydrate to the anhydrous ferric chloride is 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:20, or 1:25.

[0032] In a preferred embodiment of the present invention, in the method for preparing the food-grade medium molecular weight polyisobutylene, after the initiator system is prepared, the initiator system is aged at low temperature to activate the initiator system;

[0033] The temperature range of low temperature aging of the initiator system is -30°C to -80°C;

[0034] The low-temperature aging time of the initiator system ranges from 2 minutes to 20 minutes.

[0035] The initiator complex is a green catalytic system and does not contain any heavy metals;

[0036] The initiator complex system does not need to add other auxiliary initiators and can generate higher reaction activity after low-temperature aging and complexation.

[0037] After compounding, the high-activity initiator system with low-temperature aging and complexing can achieve fast initiation and growth in the solvent. However, too fast a reaction speed will lead to large heat release per unit time, and chain transfer and termination are prone to occur, resulting in low conversion rate and wide molecular weight distribution.

[0038] In a preferred embodiment of the present invention, in the method for preparing the food-grade medium molecular weight polyisobutylene, the ketone compound is benzophenone;

[0039] The ether compound is p-tert-butylphenyl ethyl ether;

[0040] The amide compound adopts food grade N-ethylmenthane amide.

[0041] In a preferred embodiment of the present invention, in the method for preparing the above-mentioned food-grade medium molecular weight polyisobutylene, the molar ratio of the ferric chloride hexahydrate to the third component is 1:(0.1~10).

[0042] In a preferred embodiment of the present invention, in the method for preparing the above-mentioned food-grade medium molecular weight polyisobutylene, the solvent is a polar solvent and / or a non-polar solvent.

[0043] In a preferred embodiment of the present invention, in the method for preparing the above-mentioned food-grade medium molecular weight polyisobutylene, the polar solvent is a chlorinated alkane compound;

[0044] Preferably, the chlorinated alkane compound is selected from at least one of monochloromethane and dichloromethane.

[0045] The non-polar solvent is at least one of a hexane compound, a methylcyclohexane compound and a cyclohexane compound;

[0046] The volume ratio of the polar solvent to the non-polar solvent is (0-5):(5-10).

[0047] Preferably, the volume ratio of the polar solvent to the non-polar solvent is (0-2):(2-10).

[0048] The invention discloses an application of food-grade medium molecular weight polyisobutylene in chewing gum base, food adhesive, food packaging, food-grade hot melt adhesive and medical plaster, wherein the polyisobutylene is the polyisobutylene as described above.

[0049] The beneficial effects of the embodiments of the present invention are:

[0050] The invention uses ferric chloride hexahydrate and anhydrous ferric chloride as initiators, and can form a high reaction activity through low-temperature aging and complexation. Under the action of the third component, the phenomenon of chain transfer that is easy to occur in cationic polymerization is suppressed, and the narrow molecular weight distribution preparation of food-grade medium molecular weight polyisobutylene is achieved.

[0051] The catalyst system of the present invention is a green catalytic system that does not contain heavy metals. It can produce high reaction activity in a non-polar solvent with a very small compound addition amount, avoiding the serious damage to the environment caused by highly polar chlorinated solvents due to their toxicity, volatility and strong corrosiveness.

[0052] The food-grade medium molecular weight polyisobutylene prepared by the present invention does not need to add other auxiliary initiators, simplifies the experimental steps, and the reaction activity generated by low-temperature aging and complexation is much higher than that of traditional Lewis acids such as TiCl4 and BF3.

[0053] The food-grade medium molecular weight polyisobutylene prepared by the present invention can reduce the residual amount of initiator in the polymer and simplify the purification step. It can even be completely removed by a simple dissolution-alcohol washing method, thereby reducing the post-processing cost. The prepared polymer has an extremely low ion content, can reach a higher food grade, and reduces the industrialization cost.

[0054] The present invention uses the third component to complex with the active center, which reduces the probability of chain transfer, so that the molecular weight distribution of the prepared polymer is narrow and the conversion rate is high.

[0055] The unique composite ferric chloride high-activity initiation system of the present invention can prepare polymers without the need for ultra-low temperature, thereby reducing the production energy consumption of deep refrigeration. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0057] Figure 1 Schematic diagram of the molecular structure of food-grade medium molecular weight polyisobutylene of the present invention;

[0058] Figure 2 The schematic diagram of the preparation structure of food-grade medium molecular weight polyisobutylene of the present invention is shown in FIG. DETAILED DESCRIPTION

[0059] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0060] Please refer to Figure 1 The embodiment of the present invention provides a food grade medium molecular weight polyisobutylene, wherein the chemical formula of the polyisobutylene is -[CH2-C(CH3)2] n -, where n is in the range of 180 <n<1800;

[0061] The polyisobutylene contains Mn, and the content of Mn ranges from 10000 to 100000 g / mol;

[0062] Preferably, the content of Mn is 20000 g / mol, 30000 g / mol, or 40000 g / mol.

[0063] The molecular weight distribution of the polyisobutylene is between 1.0 and 1.5.

[0064] Please refer to Figure 2 The embodiment of the present invention also provides a method for preparing food-grade medium molecular weight polyisobutylene, comprising:

[0065] Configure the initiator system;

[0066] A third component is added to the initiator system to initiate monomer polymerization to prepare food-grade medium molecular weight polyisobutylene;

[0067] The initiator system includes ferric chloride hexahydrate and anhydrous ferric chloride, and also includes a solvent;

[0068] The third component includes at least one of a ketone compound, an ether compound and an amide compound;

[0069] The monomer is selected from isobutylene compounds;

[0070] The temperature range of the monomer polymerization reaction is -30°C to -80°C;

[0071] The polyisobutylene is the polyisobutylene described above.

[0072] Wherein, the monomer polymerization reaction is a cationic polymerization reaction of the monomer.

[0073] Among them, by adding the third component, the carbon cation active center is stabilized, the occurrence of chain transfer is inhibited, and narrow molecular weight distribution control can be achieved.

[0074] The product conversion rate of the medium molecular weight polyisobutylene prepared by the present invention is above 85%.

[0075] The residual metal ion content in the medium molecular weight polyisobutylene prepared by the present invention is only 10% of the residual content of other traditional catalysts. The residual metal ions in the polymer can be quickly removed in a simple post-treatment process, and the final ion removal rate can reach 100%.

[0076] In a preferred embodiment of the present invention, in the method for preparing the above-mentioned food-grade medium molecular weight polyisobutylene, the ferric chloride hexahydrate in the initiator system is ferric chloride saturated with crystal water, which is prepared by precipitation of ferric chloride from an aqueous solution, and has a chemical formula of FeCl3·6H2O;

[0077] The anhydrous ferric chloride in the initiator system is an ionic crystal, which is obtained by heating ferric chloride hexahydrate and removing the water in the ferric chloride saturated with water of crystallization, and has a chemical formula of FeCl3.

[0078] The technical effect is that by selecting different forms of ferric chloride and using hexahydrate ferric chloride and anhydrous ferric chloride in the preparation process, the initiator system is optimized, which helps to control and improve the preparation process of food-grade medium molecular weight polyisobutylene.

[0079] In a preferred embodiment of the present invention, in the method for preparing the above-mentioned food-grade medium molecular weight polyisobutylene, in the initiator system, the molar ratio of the ferric chloride hexahydrate to the anhydrous ferric chloride is 1:(5-29).

[0080] Preferably, the molar ratio of the ferric chloride hexahydrate to the anhydrous ferric chloride is 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:20, or 1:25.

[0081] In a preferred embodiment of the present invention, in the method for preparing the food-grade medium molecular weight polyisobutylene, after the initiator system is prepared, the initiator system is aged at low temperature to activate the initiator system;

[0082] The temperature range of low temperature aging of the initiator system is -30°C to -80°C;

[0083] The low-temperature aging time of the initiator system ranges from 2 minutes to 20 minutes.

[0084] The initiator complex is a green catalytic system and does not contain any heavy metals;

[0085] The initiator complex system does not need to add other auxiliary initiators and can generate higher reaction activity after low-temperature aging and complexation.

[0086] In a preferred embodiment of the present invention, in the method for preparing the food-grade medium molecular weight polyisobutylene, the ketone compound is benzophenone;

[0087] The ether compound is p-tert-butylphenyl ethyl ether;

[0088] The amide compound adopts food grade N-ethylmenthane amide.

[0089] In a preferred embodiment of the present invention, in the method for preparing the above-mentioned food-grade medium molecular weight polyisobutylene, the molar ratio of the ferric chloride hexahydrate to the third component is 1:(0.1~10).

[0090] In a preferred embodiment of the present invention, in the method for preparing the above-mentioned food-grade medium molecular weight polyisobutylene, the solvent is a polar solvent and / or a non-polar solvent.

[0091] In a preferred embodiment of the present invention, in the method for preparing the above-mentioned food-grade medium molecular weight polyisobutylene, the polar solvent is a chlorinated alkane compound;

[0092] Preferably, the chlorinated alkane compound is selected from at least one of monochloromethane and dichloromethane.

[0093] The non-polar solvent is at least one of a hexane compound, a methylcyclohexane compound and a cyclohexane compound;

[0094] The volume ratio of the polar solvent to the non-polar solvent is (0-5):(5-10).

[0095] Preferably, the volume ratio of the polar solvent to the non-polar solvent is (0-2):(2-10).

[0096] The embodiments of the present invention also provide a use of a food-grade medium molecular weight polyisobutylene in a chewing gum base, a food adhesive, a food packaging material, a food-grade hot melt adhesive and a medical plaster, wherein the polyisobutylene is the polyisobutylene described above.

[0097] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0098] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0099] (I) Example 1:

[0100] Before the reaction, the 4-liter low-temperature polymerization kettle should be heated and "baked". A fully enclosed temperature controller should be used to ensure that the internal temperature of the polymerization kettle reaches above 75°C. Then, the residual solvent and water should be removed by decompression. At the same time, nitrogen should be continuously pumped out for about 20 times to ensure that the polymerization kettle is in a nitrogen atmosphere. The feeding tank used should be cleaned, baked and nitrogen-exhausted to the same standard. Then the temperature is set to drop, and when the temperature in the polymerization kettle reaches below the boiling point of methyl chloride and isobutylene monomer, the feeding is ready to start. Add 1000g hexane, 540g isobutylene, and 0.1M food-grade N-ethylmenthanamide. Add 0.5M ferric chloride, 0.1M ferric chloride hexahydrate, and 10g hexane to mix and configure the initiation system. After aging for 5 minutes, nitrogen is pressed into the reactor to initiate polymerization. Finally, a large amount of methanol is added to terminate the reaction, and the product is desolventized and dried.

[0101] (II) Example 2:

[0102] Before the reaction, the 4-liter low-temperature polymerization kettle should be heated and "baked". A fully enclosed temperature controller should be used to ensure that the internal temperature of the polymerization kettle reaches above 75°C. Then, the residual solvent and water should be removed by decompression. At the same time, nitrogen should be continuously pumped out for about 20 times to ensure that the polymerization kettle is in a nitrogen atmosphere. The feeding tank used should be cleaned, baked and nitrogen pumped out to the same standard. Then the temperature should be lowered. When the temperature in the polymerization kettle reaches below the boiling point of methyl chloride and isobutylene monomers, the feeding should be started. 100g of methyl chloride, 1000g of hexane, 540g of isobutylene, and 0.1M of tert-butylbenzene ethyl ether were added. 2.9M ferric chloride was added as a co-initiator, 0.1M ferric chloride hexahydrate, and 20g of dichloromethane were added to mix and configure the initiation system. After aging for 5 minutes, nitrogen was pressed into the reactor to initiate polymerization. Finally, a large amount of methanol was added to terminate the reaction. The product was desolventized and dried.

[0103] (III) Example 3:

[0104] Before the reaction, the 4-liter low-temperature polymerization kettle should be heated and "baked". A fully enclosed temperature controller should be used to ensure that the internal temperature of the polymerization kettle reaches above 75°C. Then, the residual solvent and water should be removed by decompression. At the same time, nitrogen should be continuously pumped out for about 20 times to ensure that the polymerization kettle is in a nitrogen atmosphere. The feeding tank used should be cleaned, baked and nitrogen pumped out to the same standard. Then the temperature is set to drop, and when the temperature in the polymerization kettle reaches below the boiling point of methyl chloride and isobutylene monomer, the feeding is ready to start. Add 200g of dichloromethane, 1000g of hexane, 540g of isobutylene, and 0.15M of food-grade N-ethylmenthanamide. Add 1.7M ferric chloride, 0.1M ferric chloride hexahydrate, and 15g of dichloromethane to mix and configure the initiation system. After aging for 5 minutes, nitrogen is pressed into the reactor to initiate polymerization. Finally, a large amount of methanol is added to terminate the reaction, and the product is desolventized and dried.

[0105] (IV) Example 4:

[0106] Before the reaction, the 4-liter low-temperature polymerization kettle should be heated and "baked". A fully enclosed temperature controller should be used to ensure that the internal temperature of the polymerization kettle reaches above 75°C. Then, the residual solvent and water should be removed by decompression. At the same time, nitrogen should be continuously pumped out for about 20 times to ensure that the polymerization kettle is in a nitrogen atmosphere. The feeding tank used should be cleaned, baked and nitrogen pumped out to the same standard. Then the temperature is set to drop, and when the temperature in the polymerization kettle reaches below the boiling point of methyl chloride and isobutylene monomer, the feeding is ready to start. Add 200g of dichloromethane, 1000g of cyclohexane, 540g of isobutylene, and 0.2M of tert-butylbenzene ethyl ether. Add 2.3M ferric chloride, 0.1M ferric chloride hexahydrate, and 15g of dichloromethane to mix and configure the initiation system. After aging for 5 minutes, nitrogen is pressed into the reactor to initiate polymerization. Finally, a large amount of methanol is added to terminate the reaction, and the product is desolventized and dried.

[0107] (V) Example 5:

[0108] Before the reaction, the 4-liter low-temperature polymerization kettle should be heated and "baked". A fully enclosed temperature controller should be used to ensure that the internal temperature of the polymerization kettle reaches above 75°C. Then, the residual solvent and water should be removed by decompression. At the same time, nitrogen should be continuously pumped out for about 20 times to ensure that the polymerization kettle is in a nitrogen atmosphere. The feeding tank used should be cleaned, baked and nitrogen-exhausted to the same standard. Then the temperature is set to drop, and when the temperature in the polymerization kettle reaches below the boiling point of methyl chloride and isobutylene monomers, the feeding is ready to start. Add 100g of methyl chloride, 1000g of hexane, 540g of isobutylene, and 0.1M of food-grade N-ethylmenthanamide. Add 2.9M ferric chloride, 0.1M ferric chloride hexahydrate, and 15g of dichloromethane to mix and configure the initiation system. After aging for 5 minutes, nitrogen is pressed into the reactor to initiate polymerization. Finally, a large amount of methanol is added to terminate the reaction, and the product is desolventized and dried.

[0109] (VI) Example 6:

[0110] Before the reaction, the 4-liter low-temperature polymerization kettle should be heated and "baked". A fully enclosed temperature controller should be used to ensure that the internal temperature of the polymerization kettle reaches above 75°C. Then, the residual solvent and water should be removed by decompression. At the same time, nitrogen should be continuously pumped out for about 20 times to ensure that the polymerization kettle is in a nitrogen atmosphere. The feeding tank used should be cleaned, baked and nitrogen-exhausted to the same standard. Then the temperature should be lowered. When the temperature in the polymerization kettle reaches below the boiling point of methyl chloride and isobutylene monomer, the feeding should be started. Add 1000g of methylcyclohexane, 540g of isobutylene, and 0.1M of food-grade N-ethylmenthanamide. Add 1.7M ferric chloride, 0.1M ferric chloride hexahydrate, and 10g of dichloromethane to mix and configure the initiation system. After aging for 10 minutes, nitrogen is pressed into the reactor to initiate polymerization. Finally, a large amount of methanol is added to terminate the reaction. The product is desolventized and dried.

[0111] (VII) Example 7:

[0112] Before the reaction, the 4-liter low-temperature polymerization kettle should be heated and "baked". A fully enclosed temperature controller should be used to ensure that the internal temperature of the polymerization kettle reaches above 75°C. Then, the residual solvent and water should be removed by decompression. At the same time, nitrogen should be continuously pumped out for about 20 times to ensure that the polymerization kettle is in a nitrogen atmosphere. The feeding tank used should be cleaned, baked and nitrogen-exhausted to the same standard. Then the temperature is set to drop, and when the temperature in the polymerization kettle reaches below the boiling point of methyl chloride and isobutylene monomer, the feeding is ready to start. Add 1000g of hexane, 540g of isobutylene, and 0.1M of food-grade N-ethylmenthanamide. Add 1.1M ferric chloride, 0.1M ferric chloride hexahydrate, and 10g of dichloromethane to mix and configure the initiation system. After aging for 15 minutes, nitrogen is pressed into the reactor to initiate polymerization. Finally, a large amount of methanol is added to terminate the reaction, and the product is desolventized and dried.

[0113] (VIII) Embodiment 8:

[0114] Before the reaction, the 4-liter low-temperature polymerization kettle should be heated and "baked". A fully enclosed temperature controller should be used to ensure that the internal temperature of the polymerization kettle reaches above 75°C. Then, the residual solvent and water should be removed by decompression. At the same time, nitrogen should be continuously pumped out for about 20 times to ensure that the polymerization kettle is in a nitrogen atmosphere. The feeding tank used should be cleaned, baked and nitrogen-exhausted to the same standard. Then the temperature is set to drop, and when the temperature in the polymerization kettle reaches below the boiling point of methyl chloride and isobutylene monomers, the feeding is ready to start. Add 200g of dichloromethane, 1000g of cyclohexane, 540g of isobutylene, and 0.2M of food-grade N-ethylmenthanamide. Add 1.7M ferric chloride, 0.1M ferric chloride hexahydrate, and 15g of dichloromethane to mix and configure the initiation system. After aging for 20 minutes, nitrogen is pressed into the reactor to initiate polymerization. Finally, a large amount of methanol is added to terminate the reaction, and the product is desolventized and dried.

[0115] (IX) Comparative Example 1:

[0116] Before the reaction, the 4-liter low-temperature polymerization kettle should be heated and "baked". A fully enclosed temperature controller should be used to ensure that the internal temperature of the polymerization kettle reaches above 75°C. Then, the residual solvent and water should be removed by decompression. At the same time, nitrogen should be continuously pumped out for about 20 times to ensure that the polymerization kettle is in a nitrogen atmosphere. The feeding tank used should be cleaned, baked and nitrogen pumped out according to the same standards. Then the temperature is set to drop, and when the temperature in the polymerization kettle reaches below the boiling point of monochloromethane and isobutylene monomer, the feeding is ready to start. Add 1000g of hexane and 540g of isobutylene. Add 1.1M ferric chloride, 0.1M ferric chloride hexahydrate, and 10g of hexane to mix and configure the initiation system. After aging for 5 minutes, nitrogen is pressed into the reactor to initiate polymerization. Finally, a large amount of methanol is added to terminate the reaction, and the product is desolventized and dried.

[0117] (X) Comparative Example 2:

[0118] Before the reaction, the 4-liter low-temperature polymerization kettle should be heated and "baked". A fully enclosed temperature controller should be used to ensure that the internal temperature of the polymerization kettle reaches above 75°C. Then, the residual solvent and water should be removed by decompression. At the same time, nitrogen should be continuously pumped out for about 20 times to ensure that the polymerization kettle is in a nitrogen atmosphere. The feeding tank used should be cleaned, baked and nitrogen-exhausted to the same standard. Then the temperature is set to drop, and when the temperature in the polymerization kettle reaches below the boiling point of methyl chloride and isobutylene monomer, the feeding is ready to start. 1000g of hexane, 540g of isobutylene, and 0.1M of food-grade N-ethylmenthanamide are added. 0.6M titanium tetrachloride is added as a co-initiator and 0.6M water is added as the main initiator. The mixture is configured into an initiation system. After aging for 5 minutes, nitrogen is pressed into the reactor to initiate polymerization. Finally, a large amount of methanol is added to terminate the reaction. The product is desolventized and dried.

[0119] (XI) Comparative Example 3:

[0120] Before the reaction, the 4-liter low-temperature polymerization kettle should be heated and "baked". A fully enclosed temperature controller should be used to ensure that the internal temperature of the polymerization kettle reaches above 75°C. Then, the residual solvent and water should be removed by decompression. At the same time, nitrogen should be continuously pumped out for about 20 times to ensure that the polymerization kettle is in a nitrogen atmosphere. The feeding tank used should be cleaned, baked and nitrogen-exhausted to the same standard. Then the temperature is set to drop, and when the temperature in the polymerization kettle reaches below the boiling point of methyl chloride and isobutylene monomer, the feeding is ready to start. 1000g of hexane, 540g of isobutylene, and 0.1M of food-grade N-ethylmenthanamide are added. 9.0M titanium tetrachloride is added as a co-initiator and 0.6M water as the main initiator, and the mixture is configured into an initiation system. After aging for 5 minutes, nitrogen is pressed into the reactor to initiate polymerization. Finally, a large amount of methanol is added to terminate the reaction, and the product is desolventized and dried.

[0121] 12. Performance testing

[0122] In the examples of the present invention, the average molecular weight and molecular weight distribution of the polymer were determined by size exclusion chromatography according to GB / T 36214.5-2018, and the absolute determination was performed using a light scattering method. The results of the examples are shown in Table 1, and the results of the comparative examples are shown in Table 2.

[0123] Table 1 Reaction temperature, product molecular weight and total conversion rate data table of the examples

[0124]

[0125] As shown in Table 1, the compound of ferric chloride hexahydrate and anhydrous ferric chloride as initiator can form a high reaction activity after low-temperature aging and complexation. It is also applicable in non-polar solvents, which can reduce or even eliminate the need for chlorinated solvents, avoiding serious environmental damage due to its toxicity, volatility, and strong corrosiveness. At the same time, there is no need to add additional auxiliary catalysts, and the preparation of medium molecular weight polyisobutylene with high conversion rate can be achieved with a very small amount, and the conversion rate can reach more than 85% even at -30℃. With the third component, the molecular weight distribution of the product is less than 1.5.

[0126] Table 2 Reaction temperature, product molecular weight and total conversion rate data table of comparative examples

[0127]

[0128] As shown in Table 1 and Table 2, by comparing Comparative Example 1 and Example 1, it can be seen that the effect of the third component is significant. A highly active initiation system can achieve fast initiation and fast growth, but a too fast reaction speed will lead to a large heat release per unit time, and chain transfer is prone to occur and terminate, resulting in low conversion rate and wide molecular weight distribution. Therefore, by adding food-grade N-ethylmenthanamide as the third component, the active center is stabilized and chain transfer is inhibited, which can greatly improve the conversion rate while achieving the preparation of a narrow molecular weight distribution product.

[0129] As shown in Table 1 and Table 2, by comparing Comparative Example 2 with Example 1, it can be seen that the reaction activity of the composite of the present invention is much greater than that of titanium tetrachloride, but at the same addition amount, titanium tetrachloride cannot successfully initiate polymerization in a non-polar solvent, and the monomer conversion rate is only 15%.

[0130] As shown in Table 1 and Table 2, by comparing Comparative Example 3 with Example 1, it can be seen that when the amount of titanium tetrachloride used is 15 times that of the main initiator, the conversion rate can reach 50%, and the reaction can be initiated in a non-polar solvent. However, this also leads to a sharp increase in metal residues, which cannot be effectively removed by a simple purification process.

[0131] The embodiments of the present invention are intended to protect a food-grade medium molecular weight polyisobutylene and its preparation and application, and have the following effects:

[0132] 1. The food-grade medium molecular weight polyisobutylene prepared by the present invention has a narrow molecular weight distribution, which can well prevent deformation, make fragment processing relatively easy, and thus improve the taste of food.

[0133] 2. Since ferric chloride has high Lewis acidity, the food-grade medium molecular weight polyisobutylene prepared by the present invention can achieve high reactivity with a small addition amount, and there is no need to prepare the polymer at an extremely low temperature.

[0134] 3. In the food-grade medium molecular weight polyisobutylene prepared by the present invention, the residual metal ion content measured in the unpurified polymer is only 10% of the residual amount of other catalysts.

[0135] 4. In the post-treatment process of the polymer, the present invention can quickly remove the residual metal ions in the polymer simply by using the dissolution-alcohol washing method, and the metal ion removal rate can reach 100% after three washings.

[0136] 5. The food-grade medium molecular weight polyisobutylene prepared by the present invention can be widely used in the fields of chewing gum base, food adhesives, food packaging, food-grade hot melt adhesives and medical plasters.

[0137] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

Claims

1. A method for preparing food-grade medium molecular weight polyisobutylene, characterized in that: include: Configure the initiator system; A third component is added to the initiator system to initiate monomer polymerization to prepare food-grade medium molecular weight polyisobutylene; The initiator system includes ferric chloride hexahydrate and anhydrous ferric chloride, and also includes a solvent; The third component includes at least one of a ketone compound, an ether compound and an amide compound; The monomer is selected from isobutylene compounds; The temperature range of the monomer polymerization reaction is -30°C to -80°C; The chemical formula of the polyisobutylene is -[CH2-C(CH3)2] n -, where n is in the range of 180 <n<1800; The polyisobutylene contains Mn, and the content of Mn ranges from 10000 to 100000 g / mol; The molecular weight distribution of the polyisobutylene is between 1.0 and 1.5; The ketone compound is benzophenone; The ether compound is p-tert-butylphenyl ethyl ether; The amide compound adopts food grade N-ethylmenthane amide; In the initiator system, the molar ratio of the ferric chloride hexahydrate to the anhydrous ferric chloride is 1:(5-29).

2. The method for preparing food-grade medium molecular weight polyisobutylene according to claim 1, characterized in that: The ferric chloride hexahydrate in the initiator system is ferric chloride saturated with crystal water, which is prepared by precipitation of ferric chloride from an aqueous solution, and has a chemical formula of FeCl3·6H2O; The anhydrous ferric chloride in the initiator system is an ionic crystal, which is obtained by heating ferric chloride hexahydrate and removing the water in the ferric chloride saturated with water of crystallization, and has a chemical formula of FeCl3.

3. The method for preparing food-grade medium molecular weight polyisobutylene according to claim 1, characterized in that: After the initiator system is prepared, the initiator system is aged at low temperature to activate the initiator system; The temperature range of low temperature aging of the initiator system is -30°C to -80°C; The low-temperature aging time of the initiator system ranges from 2 minutes to 20 minutes.

4. The method for preparing food-grade medium molecular weight polyisobutylene according to claim 1, characterized in that: The molar ratio of the ferric chloride hexahydrate to the third component is 1:(0.1-10).

5. The method for preparing food-grade medium molecular weight polyisobutylene according to claim 1, characterized in that: The solvent is a polar solvent and / or a non-polar solvent.

6. The method for preparing food-grade medium molecular weight polyisobutylene according to claim 5, characterized in that: The polar solvent is a chlorinated alkane compound; The non-polar solvent is at least one of a hexane compound, a methylcyclohexane compound and a cyclohexane compound; The volume ratio of the polar solvent to the non-polar solvent is (0-5):(5-10).

Citation Information

Patent Citations

  • Method for preparing medium molecular weight polyisobutene by use of Fe / Ti composite catalyst

    CN110183560A

  • Inductive system for activated cation

    CN1201800A

  • Production of isobutene-based polymer

    JP1996053514A

  • Method for producing isobutylene polymer

    JP2009126889A