Conductive copper busbar insulation rubber coating and preparation method thereof

By using high-strength and good-toughness insulating coating on conductive copper bars, the problem of low production efficiency of conductive copper bars is solved, efficient coating and voltage resistance are achieved, and it is suitable for high-voltage electrical applications.

CN117362997BActive Publication Date: 2024-10-29XIAMEN AIRUIKE ELECTRONICS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311442119.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-01
Publication Date
2024-10-29
Estimated Expiration
2043-11-01

AI Technical Summary

Technical Problem

The existing conductive copper bars have low production efficiency and require cutting, bending, casing and heating. The lengths and bending angles of the copper bars are different, which leads to high production equipment requirements and the inability to complete the processing by oneself. Moreover, the whole roll needs to be pulled after being sold. Straight and bent, resulting in higher strength, toughness and voltage resistance requirements for the insulation coating.

Method used

The preparation method of conductive copper bus insulation encapsulation is used, including nylon 12, modified thermoplastic elastomer, PCTG, compatibilizer and cross-linking agent. Through surface graft modification and dynamic vulcanization, high strength and good toughness insulation is obtained The encapsulation uses ultraviolet light source to cross-link to improve toughness, and through silicon carbide dispersion to improve high temperature resistance and antioxidant capacity, reducing the use of antioxidants.

Benefits of technology

The thermal shrinkage performance, volume resistivity and voltage resistance of the conductive copper bus insulation coating are improved, and it can shrink significantly when heated, ensuring coating integrity, improving production efficiency, reducing equipment requirements, and is suitable for high-voltage electrical application scenarios .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004526373770000051
    Figure BDA0004526373770000051
  • Figure BDA0004526373770000061
    Figure BDA0004526373770000061
  • Figure BDA0004526373770000071
    Figure BDA0004526373770000071
Patent Text Reader

Abstract

The present application belongs to the technical field of polymer material preparation, and the present application discloses a conductive copper busbar insulation coating and a preparation method. The conductive copper busbar insulation coating comprises the following components: nylon 12, modified thermoplastic elastomer, PCTG, compatibilizer, benzophenone and crosslinking agent; the modified thermoplastic elastomer comprises the following components: acrylate rubber, nylon 6, silica, silicon carbide particles, MPTMS, butyl acrylate, initiator and vulcanizer. The preparation method of the conductive copper busbar insulation coating comprises the following steps: (1) preparing the modified thermoplastic elastomer; (2) mixing, kneading, extruding and granulating the modified thermoplastic elastomer and other raw materials to obtain master batch particles; (3) extruding the master batch particles to obtain a sleeve and then irradiating and expanding it to obtain the conductive copper busbar insulation coating. The conductive copper busbar insulation coating prepared in the present application has high strength, good toughness, and strong high voltage resistance. It can reduce costs and improve efficiency in the production and use of conductive copper busbars.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer material preparation, and in particular to an insulating rubber coating for a conductive copper busbar and a preparation method thereof. Background Art

[0002] In the technical field of power distribution cabinets, a large number of conductive copper bars are often needed. When producing existing conductive copper bars, the copper bars are first cut to a specified length, and then the copper bars are straightened and bent according to actual needs. Then, a heat shrinkable insulating sleeve is put on the conductive copper bar, and finally the heat shrinkable insulating sleeve is heated. The heat shrinkable insulating sleeve will shrink and deform after being heated, so that the heat shrinkable insulating sleeve can be tightly put on the copper bar. The above technical scheme has defects when implemented: (1) The conductive copper bar needs to be cut, bent, sleeved, and heated first, and the overall production efficiency is low. In addition, because the length and bending angle of the conductive copper bar are various, the heating step has high requirements. The power distribution cabinet manufacturer is generally unable to purchase copper bars, cut, bend, sleeve, and heat them by themselves; (2) The sleeve step needs to be carried out one by one, which is inefficient and cannot be guaranteed, which also affects the production efficiency of the conductive copper bar. Therefore, the inventor added the step of rubber coating the conductive copper busbar into the production process of the conductive copper busbar, and directly prepared a whole roll of insulating rubber-coated mother copper busbar; after the production is completed, the whole roll of insulating rubber-coated mother copper busbar is sold, and after the downstream manufacturers purchase the whole roll of insulating rubber-coated mother copper busbar, they only need to unwind, cut, straighten, and bend it, which can save the steps of casing and heating shrinking tube, effectively improve production efficiency, and reduce production equipment requirements. However, in the implementation process, if the copper busbar is sold in a whole roll, it needs to be straightened and bent later, so the strength, toughness and voltage resistance requirements of the insulating rubber coating on the outside of the copper busbar are relatively high. Summary of the invention

[0003] In order to solve at least one of the above technical problems, an insulating rubber coating for the outer covering of a copper busbar with high strength and good toughness is developed. The present application provides an insulating rubber coating for a conductive copper busbar and a preparation method thereof.

[0004] On the one hand, the present application provides a conductive copper busbar insulation coating, which includes the following components by weight: 100-150 parts of nylon 12, 80-110 parts of modified thermoplastic elastomer, 30-50 parts of PCTG, 10-20 parts of compatibilizer, 2-3 parts of benzophenone, and 2-4 parts of cross-linking agent; the raw materials of the modified thermoplastic elastomer include acrylic rubber, nylon 6, silica, silicon carbide, MPTMS, butyl acrylate, initiator and vulcanizer in a weight ratio of 70-100:40-53:10-13:4.5-6:0.2-0.5:0.3-0.5:0.8:1.

[0005] By adopting the above technical scheme, the modified thermoplastic elastomer is obtained by using MPTMS and butyl acrylate to carry out surface grafting modification on a mixture of silica and silicon carbide, and then blending the modified silica and silicon carbide mixture with acrylic rubber and nylon 6, and adopting a dynamic vulcanization method to obtain a modified thermoplastic elastomer; more than 90% of silica is natural crystalline silicon dioxide with a fineness of 8 to 20 μm, which not only plays a filling and increasing role like a general mineral filler, but also shows a unique reinforcing effect, and is a new type of functional mineral filler; dispersing silicon carbide particles into the thermoplastic elastomer, and then dispersing them into the insulating rubber coating of the conductive copper bus, can improve the overall strength, and can also improve its high temperature resistance and wear resistance. Silicon carbide dispersed on the surface of the insulating rubber coating can also improve the antioxidant capacity and extend its service life. The addition of silicon carbide can also reduce the use of antioxidants. Studies have shown that when the amount of antioxidant added is too much, the gel content of the finished product obtained after irradiation cross-linking will be significantly reduced, thereby affecting the toughness and strength of the finished product. The present invention adopts the method of surface grafting of inorganic particles to graft polybutyl acrylate molecular chains on the surface of silica, thereby improving the compatibility of silica, silicon carbide particles and nylon 6 / acrylate rubber type thermoplastic elastomer.

[0006] Furthermore, the conductive copper busbar insulation rubber coating comprises the following components in parts by weight: 120-150 parts of nylon 12, 80-95 parts of modified thermoplastic elastomer, 30-40 parts of PCTG, 10-20 parts of compatibilizer, 2-3 parts of benzophenone, and 2-4 parts of cross-linking agent; the raw materials of the modified thermoplastic elastomer include acrylic rubber, nylon 6, silica, silicon carbide, MPTMS, butyl acrylate, initiator and vulcanizer in a weight ratio of 70-90:40-45:10-13:4.5-6:0.2-0.5:0.3-0.5:0.8:1.

[0007] Optionally, the compatibilizer is one or more of ethylene-butyl acrylate-maleic anhydride copolymer, maleic anhydride grafted acrylonitrile-butadiene-styrene and styrene maleic anhydride copolymer.

[0008] Furthermore, the grafting rate of the compatibilizer is 1-1.6%.

[0009] Optionally, the glass transition temperature of the PCTG is between 120°C and 150°C.

[0010] In a second aspect, the present application provides a method for preparing the above-mentioned conductive copper busbar insulation coating, comprising the following steps:

[0011] S1, adding silica, silicon carbide, MPTMS, butyl acrylate and initiator to ethanol, carrying out polymerization reaction, filtering, taking filter residue, drying, grinding and sieving to obtain a modified mixture;

[0012] S2, adding acrylic rubber and nylon 6 into the mixing chamber of the rheometer to melt, adding the modified mixture prepared in step S1 and the vulcanizing agent after melting, vulcanizing, hot pressing and cold pressing on a flat vulcanizing press, cooling and standing, to obtain a modified thermoplastic elastomer;

[0013] S3, adding nylon 12, PCTG, compatibilizer, benzophenone, crosslinking agent and the modified thermoplastic elastomer prepared in step S2 into an internal mixer according to a proportion, mixing to obtain a mixture, kneading at a high speed, extruding and granulating to obtain masterbatch particles;

[0014] S4, extruding the masterbatch particles obtained in step S3 to obtain a sleeve, irradiating the sleeve with an ultraviolet light source, and controlling the irradiation dose to be 35-75 Mrad; expanding the irradiated sleeve by 2-3 times, cooling and shaping, and obtaining the conductive copper busbar insulation rubber coating.

[0015] By adopting the above technical scheme, nylon 12, as a long-chain nylon, has a relatively low amide group density, which is different from nylon 6 and nylon 66. Therefore, cross-linking modification thereof requires specific cross-linking agents, initiators and modification methods. In view of the relatively low amide group density of nylon 12, cross-linking modification is carried out by irradiation with ultraviolet light source, and the overall toughness of the material is improved by cross-linking modification after blending nylon 12 and thermoplastic elastomer. Benzophenone, the initiator of the cross-linking reaction in this application, is also a specific initiator for the cross-linking reaction of nylon 12. Only a suitable ultraviolet radiation dose can make the gel content of the obtained conductive copper busbar insulation coating within a suitable range. If the gel content is too low, it cannot be fully retracted into place; if the content is too high, it is easy to break when expanding.

[0016] Optionally, in step S2, the vulcanization time is controlled to be 6-8 minutes.

[0017] Optionally, in step S3, the temperature of the mixed material is controlled at 160-180° C. during high-speed kneading; and the temperature of the mixed material is controlled at 180-240° C. during granulation.

[0018] In summary, the present invention includes at least one of the following beneficial technical effects:

[0019] 1. The conductive copper busbar insulation coating obtained by the present application has good heat shrinkage performance. While ensuring a large lateral shrinkage rate, the longitudinal shrinkage rate can be well controlled. Therefore, when it is heated, the conductive copper busbar insulation coating can shrink greatly in the lateral direction and only cover the surface of the copper busbar. The longitudinal shrinkage range can closely follow the lateral shrinkage range to ensure the flatness of the surface after covering, while the longitudinal shrinkage range is not too large to cause the upper part of the copper busbar to not be covered in place, so that the copper busbar can be completely fitted.

[0020] 2. The conductive copper busbar insulation coating prepared in this application has high volume resistivity and strong voltage resistance, and can be used in high-voltage power application scenarios such as distribution boxes.

[0021] 3. The conductive copper busbar insulation coating obtained in this application has high tensile strength and elongation at break, good toughness, and can withstand subsequent straightening, bending and other steps after the copper busbar processing and coating are completed. DETAILED DESCRIPTION

[0022] The present application is further described in detail below with reference to the embodiments.

[0023] The present application designs a conductive copper busbar insulation rubber coating, which includes the following components by weight: 100-150 parts of nylon 12, 80-110 parts of modified thermoplastic elastomer, 30-50 parts of PCTG, 10-20 parts of compatibilizer, 2-3 parts of benzophenone and 2-4 parts of cross-linking agent; the raw materials of the modified thermoplastic elastomer include acrylic rubber, nylon 6, silica, silicon carbide, MPTMS, butyl acrylate, initiator and vulcanizer in a weight ratio of 70-100:40-53:10-13:4.5-6:0.2-0.5:0.3-0.5:0.8:1.

[0024] Furthermore, the conductive copper busbar insulation rubber coating comprises the following components in parts by weight: 120-150 parts of nylon 12, 80-95 parts of modified thermoplastic elastomer, 30-40 parts of PCTG, 10-20 parts of compatibilizer, 2-3 parts of benzophenone, and 2-4 parts of cross-linking agent; the raw materials of the modified thermoplastic elastomer include acrylic rubber, nylon 6, silica, silicon carbide, MPTMS, butyl acrylate, initiator and vulcanizer in a weight ratio of 70-90:40-45:10-13:4.5-6:0.2-0.5:0.3-0.5:0.8:1.

[0025] The conductive copper busbar insulation rubber coating of the present application is prepared by the following method, including the following steps:

[0026] S1, adding silica, silicon carbide, MPTMS, butyl acrylate and initiator to ethanol, carrying out polymerization reaction, filtering, taking filter residue, drying, grinding and sieving to obtain a modified mixture;

[0027] S2, adding acrylic rubber and nylon 6 into the mixing chamber of the rheometer to melt, adding the modified mixture prepared in step S1 and the vulcanizing agent after melting, vulcanizing, hot pressing and cold pressing on a flat vulcanizing press, cooling and standing, to obtain a modified thermoplastic elastomer;

[0028] S3, adding nylon 12, PCTG, compatibilizer, benzophenone, crosslinking agent and the modified thermoplastic elastomer prepared in step S2 into an internal mixer according to a proportion, mixing to obtain a mixture, kneading at a high speed, extruding and granulating to obtain masterbatch particles;

[0029] S4, extruding the masterbatch particles obtained in step S3 to obtain a sleeve, irradiating the sleeve with an ultraviolet light source, and controlling the irradiation dose to be 35-75 Mrad; expanding the irradiated sleeve by 2-3 times, cooling and shaping, and obtaining the conductive copper busbar insulation rubber coating.

[0030] The main technical problem solved by this application is that the conductive copper busbar needs to be cut, bent, sleeved, and heated first, and the overall production efficiency is low. In addition, because the length and bending angles required for the conductive copper busbar vary, the heating step requires high requirements, and the distribution cabinet manufacturers are generally unable to purchase the copper busbar, cut, bend, sleeve, and heat it by themselves; if the copper busbar is sold in rolls, it needs to be straightened and bent later, so the strength, toughness, and voltage resistance requirements of the insulating rubber coating on the outside of the copper busbar are relatively high. The raw materials for the insulating rubber coating of the conductive copper busbar in this application include nylon 12, modified thermoplastic elastomer, PCTG, compatibilizer, benzophenone, and cross-linking agent. The conductive copper busbar insulation rubber coating prepared by the present application has good heat shrinkage performance, and can well control the longitudinal shrinkage rate while ensuring a large lateral shrinkage rate, so that when it is heated, the conductive copper busbar insulation rubber coating can shrink greatly in the lateral direction and only cover the surface of the copper busbar, and the longitudinal shrinkage range can closely follow the lateral shrinkage range to ensure the flatness of the surface after covering, while at the same time, the longitudinal shrinkage range is not too large to cause the upper part of the copper busbar to not be covered in place, so that the copper busbar can be completely fitted. The conductive copper busbar insulation rubber coating prepared by the present application has high volume resistivity and strong voltage resistance, and can be used in high-voltage power application scenarios such as distribution boxes. The conductive copper busbar insulation rubber coating prepared by the present application has high tensile strength and elongation at break, good toughness, and can withstand subsequent straightening, bending and other steps after the copper busbar processing and covering is completed.

[0031] The sources of the raw materials and equipment used in the examples of this application are as follows:

[0032] Acrylic rubber, Jinjinle Chemical Co., Ltd.;

[0033] Nylon 6 and Nylon 12, Sigma-Aldrich (Shanghai) Trading Co., Ltd.;

[0034] Silica, Guangdong Wengjiang Chemical Reagent Co., Ltd.;

[0035] Silicon carbide particles, Shanghai Baishun Biotechnology Co., Ltd.;

[0036] MPTMS (methacryloxypropyltrimethoxysilane), Jiangsu Chenguang Coupling Agent Co., Ltd.;

[0037] Butyl acrylate, Sigma-Aldrich (Shanghai) Trading Co., Ltd.;

[0038] Benzoyl peroxide, Fuchen (Tianjin) Chemical Reagent Co., Ltd.;

[0039] N,N-Dicinnamyl-1,6-hexanediamine, Zhengzhou Aikemu Chemical Co., Ltd.;

[0040] Polypropylene grafted with maleic anhydride, Dongguan Bailing New Materials Co., Ltd.;

[0041] PCTG (polyethylene terephthalate-1,4-cyclohexanedimethanol), Suzhou Qihuida Engineering Plastics Co., Ltd.;

[0042] Benzophenone, Lianyungang Haiheng Biochemical Technology Co., Ltd.;

[0043] EBS (ethylene bisstearamide), Sigma-Aldrich (Shanghai) Trading Co., Ltd.;

[0044] Color powder, Dongguan Taifeng Pigment Co., Ltd.;

[0045] Ethylene-butyl acrylate-maleic anhydride copolymer, CAS No.: 64652-60-4;

[0046] CJF-200 ultraviolet irradiation device, Dymax Company, USA.

[0047] Preparation Example 1-6

[0048] Preparation Examples 1-6 are modified thermoplastic elastomers prepared with different raw material ratios. The specific raw material ratios are shown in Table 1.

[0049] Table 1

[0050]

[0051] The raw materials of Preparation Example 1-6 also include an initiator, a vulcanizing agent and a compatibilizer, wherein the initiator used in Preparation Example 1-6 is 0.8 kg of benzoyl peroxide, the vulcanizing agent used in Preparation Example 1-6 is 1 kg of N,N-secinnamyl-1,6-hexanediamine, and the compatibilizer used in Preparation Example 1-6 is 5 kg of polypropylene grafted maleic anhydride.

[0052] The preparation process of Preparation Example 1-6 is:

[0053] S1. Add silica, silicon carbide, MPTMS, butyl acrylate and benzoyl peroxide to 50 kg of 95 wt% ethanol, polymerize at 70-80° C. for 2 h, and then polymerize under ethanol reflux for another 12 h; after the reaction is completed, filter, take the filter residue, dry it for 6 h, grind it, and pass it through a 100 mesh sieve to obtain a mixture of modified silica and modified silicon carbide, referred to as modified mixture;

[0054] S2, drying nylon 6 at 100°C for 5h, then adding nylon 6 and acrylic rubber into the mixing chamber of the rheometer to fully melt, adding the modified mixture, compatibilizer and vulcanizing agent for vulcanization, the vulcanization time is 6-8min. After the vulcanization is completed, the obtained product is hot pressed at 180°C for 5min, cold pressed for 5min, and left to stand for 24h to obtain the modified thermoplastic elastomer.

[0055] Preparation Comparative Example 1

[0056] Preparation Example 1 is based on Preparation Example 2, except that the amount of silica used in Preparation Example 1 is changed to 16 kg.

[0057] Examples 1-10

[0058] Examples 1-10 are conductive copper busbar insulation rubber coatings made with different raw material ratios. The specific raw material ratios are shown in Table 2.

[0059] Table 2

[0060]

[0061]

[0062] The raw materials of Examples 1-10 also include an antioxidant, EBS and toner, wherein the antioxidant is a mixture of 1 kg of 2,8-di-tert-butyl-4-methylphenol and 0.5 kg of triphenyl phosphite; the amount of EBS is 1.5 kg, and the amount of toner is 1.6 kg.

[0063] The modified thermoplastic elastomers used in Examples 1-10 are all the conductive copper busbar insulation rubber coatings prepared in Preparation Example 1.

[0064] The compatibilizer used in Example 1-10 is ethylene-butyl acrylate-maleic anhydride copolymer, wherein the grafting rate of the ethylene-butyl acrylate-maleic anhydride copolymer is 1%.

[0065] The crosslinking agent used in Examples 1-10 was pentaerythritol tetraacrylate.

[0066] The antioxidant used in Examples 1-10 is a mixture of 2,8-di-tert-butyl-4-methylphenol and triphenyl phosphite in a weight ratio of 1:1.

[0067] The glass transition temperature of PCTG used in Examples 1-10 is 125°C.

[0068] The preparation process of Examples 1-10 is:

[0069] (1) First, nylon 12 is dried at 100°C for 6 hours. Then, nylon 12, modified thermoplastic elastomer, PCTG, compatibilizer, benzophenone, crosslinking agent, antioxidant, EBS, and color powder are added to an internal mixer according to a proportion and mixed. The mixing temperature is set to 180°C and the mixing time is 20 minutes to obtain a mixture. Then, the temperature of the mixture is controlled at 160°C, high-speed kneading is performed for 15 minutes, and the mixture is extruded at 180°C through a twin-screw extruder, and then granulated to obtain masterbatch particles.

[0070] (2) The masterbatch particles are extruded through a single screw extruder to obtain a sleeve; then, the sleeve is irradiated with an ultraviolet light source. The ultraviolet equipment is composed of a Dymax 38560 bulb with a power of 400W, a wavelength range of 290-395nm, and a distance from the sample to the light source of 15cm. The irradiation is performed by rotating while irradiating. The irradiation dose is controlled at 50Mrad and the irradiation time is controlled at 10min. The irradiated sleeve is expanded by an expansion device at 120°C to expand by 2 times, and then cooled and shaped to obtain a conductive copper busbar insulation rubber coating.

[0071] Examples 11-15

[0072] Examples 11-15 are conductive copper busbar insulation rubber coatings made using different modified thermoplastic elastomers. Examples 11-15 are based on Example 1, with the difference that the modified thermoplastic elastomers used in Examples 11-15 correspond to the modified thermoplastic elastomers prepared in Preparation Examples 2-6, respectively.

[0073] The corresponding relationship between the modified thermoplastic elastomers in Examples 11-15 and the preparation examples is shown in Table 3.

[0074] Table 3

[0075]

[0076]

[0077] Example 16

[0078] Example 16 is based on Example 1, with the difference that the compatibilizer in Example 16 is a mixture of 10 kg of maleic anhydride grafted acrylonitrile-butadiene-styrene and 10 kg of styrene maleic anhydride copolymer.

[0079] Embodiment 17

[0080] Example 17 is based on Example 1, except that the glass transition temperature of PCTG in Example 17 is 110°C.

[0081] Embodiment 18

[0082] Example 18 is based on Example 1, with the difference that the grafting rate of the compatibilizer ethylene-butyl acrylate-maleic anhydride copolymer in Example 18 is 0.8%.

[0083] Examples 19-22

[0084] Example 19 is based on Example 1, with the difference that: in Example 19, the temperature of the mixture is controlled at 150°C during high-speed kneading in step S3.

[0085] Example 20 is based on Example 1, with the difference that: in Example 20, the temperature of the mixture is controlled at 140°C during high-speed kneading in step S3.

[0086] Example 21 is based on Example 1, with the difference that: in step S3 of Example 21, the temperature of the mixed material is controlled at 170°C when the screw extruder is used for granulation.

[0087] Example 22 is based on Example 1, with the difference being that in step S3 of Example 22, the temperature of the mixed material is controlled at 160°C when the screw extruder is used for granulation.

[0088] Comparative Examples 1-4

[0089] Comparative Example 1 is based on Example 1, except that the amount of nylon 12 used in Comparative Example 1 is changed to 180 kg.

[0090] Comparative Example 2 is based on Example 1, except that the modified thermoplastic elastomer in Comparative Example 2 adopts the modified thermoplastic elastomer prepared in Comparative Example 1.

[0091] Comparative Example 3 is based on Example 1, except that PCTG is not added in Comparative Example 3.

[0092] Comparative Example 4 is based on Example 1, except that in step S4 of Comparative Example 4, the irradiation dose of the ultraviolet light source is 80 Mrad.

[0093] Performance Testing

[0094] The performance of the conductive copper busbar insulation rubber coating obtained in Examples 1-20 and Comparative Examples 1-4 was tested, and the test items were as follows: 1. The tensile strength (MPa) of the conductive copper busbar insulation rubber coating was measured according to the reference standard ASTM-D882;

[0095] 2. Determine the elongation at break of the insulation coating of the conductive copper busbar according to the ASTM-D882 standard (%);

[0096] 3. Determine the voltage resistance of the insulation rubber coating of the conductive copper busbar according to the standard GB / T7113.2 to see whether it can pass the test;

[0097] 4. Determine the volume resistivity (Ω.cm) of the insulation coating of the conductive copper busbar according to standard GB / T7113.2;

[0098] 5. Determine the transverse shrinkage of the insulation rubber of the conductive copper busbar according to standard Q / SCT004-2015, and test the transverse shrinkage in a water bath at 98±2℃ for 30s;

[0099] 6. Determine the longitudinal shrinkage of the insulation coating of the conductive copper busbar according to standard Q / SCT004-2015, and test the longitudinal shrinkage in a water bath at 98±2℃ for 30s.

[0100] The test results are shown in the following table. Table 4 is the test results of tensile strength, elongation at break and withstand voltage of Examples 1-10 and Comparative Examples 1-4; Table 5 is the test results of tensile strength, elongation at break and withstand voltage of Examples 11-22; Table 6 is the test results of transverse shrinkage, longitudinal shrinkage and volume resistivity of Examples 1-10 and Comparative Examples 1-4; Table 7 is the test results of transverse shrinkage, longitudinal shrinkage and volume resistivity of Examples 11-22.

[0101] Table 4

[0102]

[0103] Table 5

[0104]

[0105]

[0106] Table 6

[0107]

[0108]

[0109] Table 7

[0110]

[0111] Through the analysis of the data in Table 3, the elongation at break of Examples 1-10 is significantly stronger than that of Comparative Examples 1-4, that is, the toughness of the conductive copper busbar insulation rubber coating obtained in Examples 1-10 is significantly stronger; it can be concluded that the amount of silica added to the modified thermoplastic elastomer, the vulcanization time of the modified thermoplastic elastomer, the ratio of nylon 12 and the modified thermoplastic elastomer, the ratio of nylon 12 and PCTG, and the irradiation dose will have a significant effect on the toughness of the conductive copper busbar insulation rubber coating obtained. Through the analysis of the data in Table 4, it can be obtained that the temperature during high-speed kneading and the extrusion temperature have a significant effect on the toughness and tensile strength of the conductive copper busbar insulation rubber coating obtained. Through the analysis of the data in Table 5, the lateral shrinkage rate of Examples 1-10 is significantly higher than that of the comparative example. It can be concluded that the heat shrinkage performance of the conductive copper busbar insulation coating obtained in Examples 1-10 is also significantly stronger than that of the comparative example, and can meet the production needs of the conductive copper busbar; in Example 17, the glass transition temperature of the added PCTG is relatively low, the strength of the conductive copper busbar insulation coating obtained will be reduced, and its elongation at break will increase, the heat shrinkage performance is relatively strong, the lateral and longitudinal shrinkage rates will be relatively large, and the overall toughness will be reduced; in Example 18, when the grafting rate of the compatibilizer is relatively low, the strength of the conductive copper busbar insulation coating obtained will be reduced, and its elongation at break will increase, the heat shrinkage performance is relatively strong, the lateral and longitudinal shrinkage rates will be relatively large, and the overall toughness will be reduced.

[0112] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A conductive copper busbar insulation rubber coating, It is characterized in that By weight, it includes the following components: Nylon 12 100-150 parts, Modified thermoplastic elastomer 80-110 parts, PCTG 30-50 parts, Compatibilizer 10-20 parts, 2-3 parts of benzophenone, 2-4 parts of cross-linking agent; The raw materials of the modified thermoplastic elastomer include acrylic rubber, nylon 6, silica, silicon carbide, MPTMS, butyl acrylate, initiator and vulcanizer in a weight ratio of 70-100:40-53:10-13:4.5-6:0.2-0.5:0.3-0.5:0.8:1; The method for preparing the conductive copper bus insulation rubber coating comprises the following steps: S1, adding silica, silicon carbide, MPTMS, butyl acrylate and initiator to ethanol, carrying out polymerization reaction, filtering, taking filter residue, drying, grinding and sieving to obtain a modified mixture; S2, adding acrylic rubber and nylon 6 into the mixing chamber of the rheometer to melt, adding the modified mixture prepared in step S1 and the vulcanizing agent after melting, vulcanizing, hot pressing and cold pressing on a flat vulcanizing press, cooling and standing, to obtain a modified thermoplastic elastomer; S3, adding nylon 12, PCTG, compatibilizer, benzophenone, crosslinking agent and the modified thermoplastic elastomer prepared in step S2 into an internal mixer according to a proportion, mixing to obtain a mixture, kneading at a high speed, extruding and granulating to obtain masterbatch particles; S4, extruding the masterbatch particles obtained in step S3 to obtain a sleeve, irradiating the sleeve with an ultraviolet light source, and controlling the irradiation dose to be 35-75 Mrad; expanding the irradiated sleeve by 2-3 times, cooling and shaping, and obtaining the conductive copper busbar insulation rubber coating.

2. The conductive copper busbar insulation rubber coating according to claim 1, It is characterized in that By weight, it includes the following components: Nylon 12 120-150 parts, Modified thermoplastic elastomer 80-95 parts, PCTG 30-40 parts, Compatibilizer 10-20 parts, 2-3 parts of benzophenone, 2-4 parts of cross-linking agent.

3. The conductive copper busbar insulation rubber coating according to claim 1, It is characterized in that The raw materials of the modified thermoplastic elastomer include acrylic rubber, nylon 6, silica, silicon carbide, MPTMS, butyl acrylate, initiator and vulcanizer in a weight ratio of 70-90:40-45:10-13:4.5-6:0.2-0.5:0.3-0.5:0.8:

1.

4. The conductive copper busbar insulation rubber coating according to claim 1, It is characterized in that The compatibilizer is one or more of ethylene-butyl acrylate-maleic anhydride copolymer, maleic anhydride grafted acrylonitrile-butadiene-styrene and styrene-maleic anhydride copolymer.

5. The conductive copper busbar insulation rubber coating according to claim 4, It is characterized in that The grafting rate of the compatibilizer is 1-1.6%.

6. The conductive copper busbar insulation rubber coating according to claim 1, It is characterized in that The glass transition temperature of the PCTG is between 120°C and 150°C.

7. The conductive copper busbar insulation rubber coating according to claim 1, It is characterized in that In step S2, the vulcanization time is controlled to be 6-8 minutes.

8. The conductive copper busbar insulation rubber coating according to claim 1, It is characterized in that In the step S3, the temperature of the mixed material is controlled at 160-180° C. during high-speed kneading; and the temperature of the mixed material is controlled at 180-240° C. during granulation.

Citation Information

Patent Citations

  • Joint filling sealing material, preparation method and application thereof

    CN111961426A

  • Crosslinked nylon medical equipment, preparation method thereof, nylon composition and application