A PMN-PT ferroelectric single crystal derived composite optical fiber, preparation and application
Through high-temperature glass fiber drawing technology, combined with silicate glass cladding and PMN-PT single crystal core, the problems of difficult preparation and short length of ferroelectric fibers in the existing technology are solved, and high-quality, long-size, and large-scale Ferroelectric fiber preparation has high light transmittance and low loss performance.
Patent Information
- Application Number
- CN202311401661.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-10-26
AI Technical Summary
It is difficult to prepare high-quality, long-size, large-volume ferroelectric fiber materials in the prior art, especially due to the difficulty of the process of laser heating base growth technology and the short fiber length.
Using glass fiber optic fiber wire drawing technology with improved reaction of core-cladding at high temperature, silicate glass is used as cladding material and PMN-PT single crystal is used as core material, and wire drawing is prepared by graphite furnace drawing tower to form PMN-PT Ferroelectric single crystal derived composite fiber.
Achieve high-quality, long-size, and large-batch ferroelectric fiber preparation. The fiber core has a continuous length of meter or above, with a light transmittance of up to 99%, and a loss of less than 1dB/cm. It is suitable for nonlinear optical and electro-optical modulators, etc. Device.
Smart Images

Figure CN117383818B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of novel functional optical fiber materials, and specifically relates to a PMN-PT ferroelectric single crystal derived composite optical fiber, and its preparation and application. Background Art
[0002] Electro-optic materials are a type of material whose refractive index can change under the action of an external electric field. They can be divided into linear electro-optic materials (Pockels electro-optic materials) and square electro-optic materials (Kerr electro-optic materials) according to their relationship with the modulated electric field. The electro-optic effect of electro-optic materials can be used to modulate light waves. The external electric field changes the refractive index of the material through the electro-optic effect, causing the main axis orientation and length of the refractive index ellipsoid to change, which corresponds to the change of the characteristic mode and characteristic value of the transmitted light beam, that is, the change of the polarization state and phase of the transmitted light beam, thereby producing a series of optical functional effects. Precise control of light propagation and intensity is crucial for many photonic devices such as lasers, optical amplifiers, and modulators, and is the core of a wide range of photonic applications.
[0003] Relaxor-lead titanate PMN-PT crystals with extremely high piezoelectricity are believed to have high electro-optical (EO) coefficients. However, due to light scattering and reflection of light by domain walls, the optical transparency of the crystals is severely reduced, limiting electro-optical applications. In recent years, PMN-PT single crystals have high transparency and excellent electro-optical modulation and nonlinear optical properties after AC polarization. In anti-reflection film coated crystals, a transmittance of 99.6% has been achieved, with an ultra-high EO coefficient of 900 pm / V, which is 30 times higher than the traditional lithium niobate (LN) crystals. PMN-PT transparent ferroelectric single crystals have included high-performance piezoelectric crystals in the ranks of optical devices, opening the door to the design of new acousto-optic-electric devices (Qiu C, Wang B, Zhang N, et al. Transparent ferroelectric crystals with ultrahigh piezoelectricity [J]. Nature, 2020, 577 (7790): 350-354).
[0004] So far, there has been no report on PMN-PT related crystals and glass composite optical fiber materials. In 2013, Wang et al. disclosed glass-clad LiNbO3 ferroelectric single crystal optical fiber (Wang JS, Tseng YH. ITO electrode-embedded double-cladding single-crystal LiNbO3 optical fiber [J]. Optics Letters, 2013, 38: 452-454). They used CO2 laser heating pedestal growth technology to prepare single crystal LiNbO3 optical fiber with quartz glass cladding, and the optical fiber transmission loss was as low as 1 dB / cm; however, the process of preparing ferroelectric single crystals by laser heating pedestal growth technology is extremely difficult, and the optical fiber length is relatively short, only at the centimeter level, making it difficult to achieve high-quality, long-size, and large-scale ferroelectric optical fiber preparation. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a PMN-PT ferroelectric single crystal derived composite optical fiber, preparation and application, which fully combines the functions of ferroelectric single crystals and the advantages of high light transmittance and easy drawing performance of glass cladding materials, and adopts glass optical fiber drawing technology improved by core-cladding reaction at high temperature to prepare ferroelectric composite optical fiber, so as to achieve high-quality, long-size, large-scale preparation of ferroelectric optical fibers.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A PMN-PT ferroelectric single crystal derived composite optical fiber, wherein the composite optical fiber cladding material is silicate glass and the core material is (1-x)Pb(Mg 1 / 3 Nb 2 / 3 )O3-xPbTiO3(PMN-PT, 0.2≤x≤0.4) compound crystals.
[0008] A method for preparing a PMN-PT ferroelectric single crystal derived composite optical fiber comprises the following steps:
[0009] 1) Cleaning of glass tube: Use quartz or silicate glass tube with inner hole diameter of 1.5mm-3mm and wire drawing length greater than 5cm; Use dilute hydrochloric acid and anhydrous ethanol with volume concentration less than or equal to 5vol.% to clean the processed glass tube in an ultrasonic cleaning machine;
[0010] 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame and silicate thin rod to seal one end of the center hole of the glass tube, fill the PMN-PT crystal thin rod with a set ratio into the center hole of the glass tube, and then use hydrogen-oxygen flame and silicate thin rod to seal the other end of the center hole of the glass tube to form an optical fiber preform;
[0011] 3) Fiber drawing: The assembled optical fiber preform is placed in a graphite furnace drawing tower for drawing. The drawing process is protected by argon gas. The drawing temperature is 1500℃-2050℃. A continuous glass cladding / PMN-PT core composite optical fiber is obtained through the reaction melting of the core and cladding. The fiber diameter is adjusted by the parameters of the glass tube feeding speed and the fiber traction wheel speed.
[0012] The PMN-PT compound crystals in the optical fiber preform rod hole in step 3) have a melting point of 1300° C. to 1400° C. during high-temperature optical fiber reaction core drawing, and form the core of the ferroelectric microcrystalline glass optical fiber after melting reaction and cooling.
[0013] The invention discloses an application of a PMN-PT ferroelectric single crystal derived composite optical fiber, which is suitable for single-mode transmission of all-optical fiber waveguides in various devices such as nonlinear optics and electro-optic modulators; and can also be used for subsequent preparation of optical fiber devices.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] (1) The present invention combines the advantages of silicate glass and PMN-PT single crystal, and efficiently prepares high-quality composite optical fiber materials through hot wire drawing. The continuous length of the optical fiber core reaches more than meters and is easy to mass produce. The selection of materials can meet the preparation requirements of this composite optical fiber. The silicate glass used as the optical fiber cladding has a glass softening temperature of more than 1200°C. The PMN-PT single crystal used as the optical fiber core has a melting point of 1300°C to 1400°C. When the optical fiber is drawn at high temperature, the PMN-PT single crystal melts, and the core is derived into PMN-PT / SiO2 glass optical fiber after high-temperature drawing melting reaction and rapid cooling.
[0016] (2) The composite material ferroelectric optical fiber of the present invention, by means of rapid optical fiber drawing, obtains a standard optical fiber with a diameter of about 125 μm and a core diameter of the micron level; the cladding material is mainly silicate glass, and its transmittance from visible light to 2 μm band is as high as 99%, and the middle part of the core is a mixed phase of PMN-PT micro-nano coral-like microcrystals and more than 30 vol.% amorphous SiO2, and the microcrystals gradually react and diffuse into the cladding glass; and the glass optical fiber cladding can provide good flexibility and thermodynamic stability for the core PMN-PT microcrystals.
[0017] (3) The numerical aperture of the ferroelectric optical fiber of the present invention is about 0.3, and it has a low loss of less than 1 dB / cm in the spectral band of 1.0-1.5 μm. The nonlinearity can reach hundreds of times that of quartz optical fiber. It can be fused with standard quartz optical fiber and is suitable for single-mode transmission of all-fiber waveguides in various devices such as nonlinear optics and electro-optic modulators. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1The present invention is a flow chart of a method for preparing a PMN-PT ferroelectric single crystal derived composite optical fiber.
[0019] Figure 2 These are photos of the preform rod and the ferroelectric optical fiber of Example 1 of the present invention.
[0020] Figure 3 (a) is the XRD spectrum of the PMN-PT ferroelectric single crystal derived composite optical fiber of Example 1 of the present invention, and (b) is the line scan of the composite fiber end face by electron probe spectrometer.
[0021] Figure 4 This is the refractive index distribution diagram of the cross section of the PMN-PT ferroelectric single crystal derived composite optical fiber in Example 1 of the present invention. DETAILED DESCRIPTION
[0022] In order to better understand the present invention, the contents of the present invention are further explained below in conjunction with examples, but the embodiments of the present invention are not limited thereto, and the process parameters not particularly described can be carried out with reference to conventional techniques.
[0023] Example 1, a PMN-PT ferroelectric single crystal derived composite optical fiber, the composite optical fiber cladding material is silicate glass, the core material is 0.72Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.28PbTiO3 compound crystal.
[0024] like Figure 1 As shown, a method for preparing a PMN-PT ferroelectric single crystal derived composite optical fiber comprises the following steps:
[0025] 1) Cleaning of glass tube: Use commercial pure quartz glass tube with a length of 150 mm, an outer diameter of 25 mm, a through hole diameter of 1.5 mm, and a drawing length of 5 cm; Use dilute hydrochloric acid (volume concentration 5 vol.%) and anhydrous ethanol to clean the glass tube in an ultrasonic cleaner (80 Hz, 100 W);
[0026] 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame with quartz thin rod to seal one end of the center hole of the glass tube, and fill the 0.72PMN-0.28PT single crystal thin rod into the center hole of the pure quartz glass tube. Figure 2 As shown in (a), a hydrogen-oxygen flame is used in conjunction with a quartz thin rod to seal the other end of the central hole of the pure quartz glass tube to form an optical fiber preform;
[0027] 3) Fiber drawing: The assembled fiber preform is placed in a graphite furnace drawing tower for drawing. During the drawing process, the graphite furnace drawing tower is protected by argon gas. The temperature in the graphite furnace drawing tower is raised to 2000℃ to draw the fiber. At this temperature, the glass of the fiber preform is in a viscous flow state, while the PMN-PT in the glass tube hole is in a molten state. After the optical fiber is hot-drawn, it cools and solidifies naturally to form a continuous glass cladding and PMN-PT core composite optical fiber. The actual optical fiber is shown in the figure. Figure 2 As shown in (b), the length is more than meters, and the flexibility can form a bending radius of centimeters; the XRD spectrum of ferroelectric fiber is as follows Figure 3 As shown in (a), the main body of the optical fiber is in a glassy state, with a small amount of PMN-PT crystals; the end face SEM spectrometer scan is as follows Figure 3 As shown in (b), it shows that after the PMN-PT crystal reacts with the cladding, the Pb, Mn, Nb, and Ti elements are mainly concentrated in the core and then diffuse and gradually enter the cladding.
[0028] The PMN-PT compound crystals in the optical fiber preform rod hole in step 3) have a melting point of 1350° C. during high-temperature optical fiber reaction core drawing, and form the core of the ferroelectric microcrystalline glass optical fiber after melting reaction and cooling.
[0029] Testing and application of a PMN-PT ferroelectric single crystal derived composite optical fiber: Using IFA100 optical fiber refractive index tester, the lateral interference method is used to test the optical fiber refractive index distribution, such as Figure 4 As shown, the refractive index of the quartz cladding in the 633nm band is 1.46, the refractive index at the center of the PMN-PT microcrystal core is the highest, which is 1.52, and the others are graded refractive indices; the fiber transmission loss is tested by the truncation method, and the loss at wavelengths of 1.0μm and 1.5μm is less than 1dB / cm, which is suitable for single-mode transmission of all-fiber waveguides in various devices such as nonlinear optics and electro-optic modulators.
[0030] Example 2, a PMN-PT ferroelectric single crystal derived composite optical fiber, the composite optical fiber cladding material is silicate glass, the core material is 0.8Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.2PbTiO3 compound crystal.
[0031] like Figure 1 As shown, a method for preparing a PMN-PT ferroelectric single crystal derived composite optical fiber comprises the following steps:
[0032] 1) Cleaning of glass tube: Use commercial pure quartz glass tube with a length of 150 mm, an outer diameter of 30 mm, a through hole diameter of 3 mm, and a drawing length of 5 cm; Use dilute hydrochloric acid (volume concentration 5 vol.%) and anhydrous ethanol to clean the glass tube in an ultrasonic cleaner (80 Hz, 100 W);
[0033] 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame and quartz thin rod to seal one end of the center hole of the glass tube, fill the 0.8PMN-0.2PT single crystal thin rod into the center hole of the quartz glass tube, and then use hydrogen-oxygen flame and quartz thin rod to seal the other end of the center hole of the quartz glass tube to form an optical fiber preform;
[0034] 3) Fiber drawing: The assembled optical fiber preform is placed in a graphite furnace drawing tower for drawing. During the drawing process, argon gas is passed through the graphite furnace drawing tower for protection, and the temperature in the graphite furnace drawing tower is raised to 2050°C to draw the fiber. At this temperature, the glass of the optical fiber preform is in a viscous flow state, while the PMN-PT in the glass tube hole is in a molten state. After hot drawing, the optical fiber is naturally cooled and solidified to form a continuous glass cladding and PMN-PT core composite optical fiber.
[0035] The PMN-PT compound crystals in the optical fiber preform rod hole in step 3) have a melting point of 1400° C. during high-temperature optical fiber reaction core drawing, and form the core of the ferroelectric microcrystalline glass optical fiber after melting reaction and cooling.
[0036] The test performance of a PMN-PT ferroelectric single crystal derived composite optical fiber in this embodiment is similar to that in embodiment 1.
[0037] Example 3, a PMN-PT ferroelectric single crystal derived composite optical fiber, the composite optical fiber cladding material is silicate glass, the core material is 0.6Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.4PbTiO3 compound crystal.
[0038] like Figure 1 As shown, a method for preparing a PMN-PT ferroelectric single crystal derived composite optical fiber comprises the following steps:
[0039] 1) Cleaning of glass tube: Use commercial pure quartz glass tube with a length of 150 mm, an outer diameter of 30 mm, a through hole diameter of 2 mm, and a drawing length of 5 cm; Use dilute hydrochloric acid (volume concentration 5 vol.%) and anhydrous ethanol to clean the pure quartz glass tube in an ultrasonic cleaning machine (80 Hz, 100 W);
[0040] 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame and quartz thin rod to seal one end of the center hole of pure quartz glass tube, fill 0.8PMN-0.2PT single crystal thin rod into the center hole of pure quartz glass tube, and then use hydrogen-oxygen flame and quartz thin rod to seal the other end of the center hole of pure quartz glass tube to form optical fiber preform;
[0041] 3) Fiber drawing: The assembled optical fiber preform is placed in a graphite furnace drawing tower for drawing. During the drawing process, argon gas is passed through the graphite furnace drawing tower for protection, and the temperature in the graphite furnace drawing tower is raised to 1500°C to draw the fiber. At this temperature, the glass of the optical fiber preform is in a viscous flow state, while the PMN-PT in the glass tube hole is in a molten state. After hot drawing, the optical fiber is naturally cooled and solidified to form a continuous glass cladding and PMN-PT core composite optical fiber.
[0042] The PMN-PT compound crystals in the optical fiber preform rod hole in step 3) have a melting point of 1300° C. during high-temperature optical fiber reaction core drawing, and form the core of the ferroelectric microcrystalline glass optical fiber after melting reaction and cooling.
[0043] The test performance of a PMN-PT ferroelectric single crystal derived composite optical fiber in this embodiment is similar to that in embodiment 1.
Claims
1. A PMN-PT ferroelectric single crystal derived composite optical fiber, characterized by: The composite optical fiber cladding material is silicate glass, and the core material is (1-x)Pb(Mg 1 / 3 Nb 2 / 3 )PMN-PT compound crystal of O3-xPbTiO3, 0.2≤x≤0.
4.
2. The method for preparing a PMN-PT ferroelectric single crystal derived composite optical fiber according to claim 1, characterized in that: The following steps are involved: 1) Glass tube cleaning: Use quartz or silicate glass tubes with an inner pore diameter of 1.5 mm to 3 mm, and a drawable length greater than 5 cm. Clean the processed glass tubes in an ultrasonic cleaner using dilute hydrochloric acid and anhydrous ethanol with a volume concentration of 5 vol.% or less. 2) Assembly of the optical fiber preform: Use an oxyhydrogen flame with a silicate rod to seal one end of the central hole of the glass tube. Fill the central hole of the glass tube with a PMN-PT crystal rod of a predetermined ratio. Then, use an oxyhydrogen flame with a silicate rod to seal the other end of the central hole of the glass tube to form the optical fiber preform. 3) Fiber drawing: The assembled optical fiber preform is placed in a graphite furnace drawing tower for drawing. The drawing process is protected by argon gas and the drawing temperature is 1500℃-2050℃. A continuous glass cladding / PMN-PT core composite optical fiber is obtained through the reaction melting of the core and cladding. The fiber diameter is adjusted by the parameters of the glass tube feeding speed and the fiber pulling wheel speed.
3. The preparation method according to claim 2, characterized in that The PMN-PT compound crystals in the optical fiber preform rod hole in step 3) have a melting point of 1300° C. to 1400° C. during high-temperature optical fiber reaction core drawing, and form the core of the ferroelectric microcrystalline glass optical fiber after melting reaction and cooling.
4. A PMN-PT ferroelectric single crystal derived composite optical fiber, characterized by: The composite optical fiber cladding material is silicate glass, and the core material is 0.72Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.28PbTiO3 compound crystal.
5. The PMN-PT ferroelectric single crystal derived composite optical fiber according to claim 4, characterized in that: The IFA100 fiber refractive index tester and the lateral interferometry method were used to test the refractive index distribution of the optical fiber. The refractive index of the quartz cladding in the 633nm band is 1.46, the refractive index of the center of the PMN-PT microcrystal core is the highest, 1.52, and the others are graded refractive indices. The fiber transmission loss was tested using the truncation method. The loss at wavelengths of 1.0μm and 1.5μm was less than 1 dB / cm, which is suitable for single-mode transmission of all-fiber waveguides in various devices such as nonlinear optics and electro-optic modulators.
6. The method for preparing a PMN-PT ferroelectric single crystal derived composite optical fiber according to claim 4, characterized in that: The following steps are involved: 1) Glass tube cleaning: Use commercial pure quartz glass tubes with a length of 150 mm, an outer diameter of 25 mm, a through-hole diameter of 1.5 mm, and a drawable length of 5 cm. Clean the glass tubes in an ultrasonic cleaner at 80 Hz and 100 W using 5 vol.% dilute hydrochloric acid and anhydrous ethanol. 2) Assembly of the optical fiber preform: Use an oxyhydrogen flame with a quartz rod to seal one end of the center hole of the glass tube, fill the center hole of the pure quartz glass tube with a 0.72PMN-0.28PT single crystal rod, and then use an oxyhydrogen flame with a quartz rod to seal the other end of the center hole of the pure quartz glass tube to form the optical fiber preform; 3) Fiber Drawing: The assembled optical fiber preform is placed in a graphite furnace drawing tower for drawing. During the drawing process, argon gas is passed through the graphite furnace drawing tower for protection. The temperature in the graphite furnace drawing tower is raised to 2000℃ to draw the fiber. At this temperature, the glass of the optical fiber preform is in a viscous flow state, while the PMN-PT in the glass tube hole is in a molten state. After hot drawing, the optical fiber is naturally cooled and solidified to form a continuous glass cladding and PMN-PT fiber core composite optical fiber with a length of more than meters and a flexible bending radius of centimeters.
7. The preparation method according to claim 6, characterized in that The PMN-PT compound crystals in the optical fiber preform rod hole in step 3) have a melting point of 1350° C. during high-temperature optical fiber reaction core drawing, and form the core of the ferroelectric microcrystalline glass optical fiber after melting reaction and cooling.
8. Use of a PMN-PT ferroelectric single crystal derived composite optical fiber according to claim 1, 4 or 5, characterized in that: It is suitable for single-mode transmission of all-fiber waveguides in various devices of nonlinear optics and electro-optic modulators; it can also be used for subsequent preparation of optical fiber devices.