A breathable electronic skin and its preparation method
By designing a breathable electronic skin with a porous electrolyte layer and SiO2 nanofiber electrodes, the problem of non-breathability in traditional electronic skin is solved, achieving good breathability, moisture permeability and passive cooling effect, and improving detection sensitivity and stability.
Patent Information
- Application Number
- CN202311315604.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-11
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-10-11
AI Technical Summary
Traditional polymer-based electronic skin is not breathable, leading to excessively high skin temperature, inflammation, and sweat buildup, which affects sensing performance and reliability.
A porous electrolyte layer and a nanofiber electrode containing SiO2 were used to prepare a breathable electronic skin by electrospinning. The microsphere structure of SiO2 was used to achieve passive cooling, and a hydrophobic layer was set on the electrode surface to improve breathability and detection sensitivity.
It achieves breathability and moisture permeability of electronic skin, reduces skin temperature, improves detection sensitivity and stability, prevents skin redness and swelling, and is suitable for long-term wear.
Smart Images

Figure CN117387803B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of flexible sensor technology, and in particular to a breathable electronic skin and its preparation method. Background Technology
[0002] The statements in this section are merely background information related to the present invention and do not necessarily constitute prior art.
[0003] Flexible sensors, as key sensing devices for environmental perception and information interaction, have attracted significant research attention due to their emerging potential applications in wearable medical monitoring, sports training, medical diagnosis and treatment, and human-computer interaction. Electronic skin, as a tactile sensor, is mostly fabricated on polymer substrates, such as polyethylene terephthalate (PET), polyimide (PI), polydimethylsiloxane (PDMS), and Ecoflex. However, traditional polymer substrates are solid and impermeable, hindering normal micro-mass exchange between the covered skin and the external environment. This causes skin temperature to exceed the comfortable range, leading to redness and inflammation after prolonged wear. Furthermore, accumulated sweat negatively impacts the physical formation, sensing performance, and reliability of the electronic skin. Summary of the Invention
[0004] To address the aforementioned problems, this invention proposes a breathable electronic skin and its preparation method. By employing a porous electrolyte layer, the breathability of the electronic skin is improved. Furthermore, by utilizing the microsphere structure of SiO2 in the upper and lower electrodes, the upper and lower electrodes possess excellent visible light reflection and high infrared emission capabilities, thereby achieving a passive cooling effect for the electronic skin.
[0005] To achieve the above objectives, the present invention adopts the following technical solution:
[0006] In the first aspect, a breathable electronic skin is proposed, comprising an upper electrode, a porous electrolyte layer, and a lower electrode; the porous electrolyte layer comprises a sponge and an ion gel, with the ion gel coating the sponge skeleton; both the upper and lower electrodes comprise nanofibers containing SiO2 and conductive materials, with the conductive materials covering the surface of the nanofibers; the porous electrolyte layer is located between the upper and lower electrodes, enabling charge transfer between the upper and lower electrodes.
[0007] Secondly, a method for preparing breathable electronic skin, as proposed in the first aspect, is presented, including:
[0008] A porous electrolyte layer was prepared by coating an ionogel onto a sponge skeleton.
[0009] Adding SiO2 to nanofibers yields nanofibers containing SiO2.
[0010] A conductive material is coated on the surface of nanofibers containing SiO2 to prepare an upper electrode and a lower electrode.
[0011] The upper and lower electrodes are respectively attached to the two sides of the porous electrolyte layer, enabling the porous electrolyte layer to carry out charge transfer between the upper and lower electrodes, thus preparing a breathable electronic skin.
[0012] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0013] 1. The porous electrolyte layer of the present invention uses a sponge as a base and coats an ion gel on the sponge skeleton, so that the electrolyte layer has a porous structure, thereby giving the electronic skin good breathability and increasing the detection sensitivity and detection range.
[0014] 2. This invention obtains nanofibers through electrospinning, giving the nanofibers a rich, uneven structure, thereby further improving the breathability and moisture permeability of electronic skin, as well as the detection sensitivity of electronic skin.
[0015] 3. The present invention adds SiO2 to nanofibers, so that the upper and lower electrodes can utilize the microsphere structure of SiO2, thereby having good visible light reflection and infrared emission capabilities, realizing the passive cooling effect of electronic skin, and further preventing the human skin temperature from rising.
[0016] Advantages of additional aspects of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0017] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments of this application and their descriptions are used to explain this application and do not constitute an undue limitation of this application.
[0018] Figure 1 The present invention discloses a schematic diagram of the structure of the electronic skin as an example.
[0019] Figure 2 The micro / nano structure and physical images of the electronic skin are disclosed as examples;
[0020] Figure 3 The following is a diagram showing the test results of the sensing performance of the electronic skin as an example.
[0021] Figure 4 The following diagram illustrates the test results of the hydrophobicity, breathability, and biocompatibility of the electronic skin as an example.
[0022] Figure 5 The passive cooling test and characterization results of the electronic skin are disclosed as an example.
[0023] The components are: 1. Upper electrode, 2. Porous electrolyte layer, 3. Lower electrode, and 4. Human skin. Detailed Implementation
[0024] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0025] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of this application. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.
[0026] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments according to this application. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.
[0027] Example 1
[0028] In this embodiment, a breathable electronic skin is disclosed, such as... Figure 1 As shown, it includes an upper electrode 1, a porous electrolyte layer 2, and a lower electrode 3; the porous electrolyte layer 2 includes a sponge and an ion gel, with the ion gel coating the sponge skeleton; both the upper electrode and the lower electrode include nanofibers containing SiO2 and conductive materials, with the conductive materials covering the surface of the nanofibers; the porous electrolyte layer 2 is located between the upper electrode 1 and the lower electrode 2, and is capable of charge transfer between the upper electrode 1 and the lower electrode 2.
[0029] In this embodiment, the upper electrode 1 is attached to the upper surface of the porous electrolyte layer 2, and the lower electrode 3 is attached to the lower surface of the porous electrolyte layer 2, thereby enabling charge transfer between the upper electrode 1 and the lower electrode 2 using the ion gel in the porous electrolyte layer 2.
[0030] The porous electrolyte layer 2 of this breathable electronic skin uses a sponge as a base and wraps the sponge skeleton with an ion gel, thereby enabling the porous electrolyte layer 2 to provide ions and utilize the porous structure of the sponge for breathability and heat dissipation.
[0031] The ion gel was prepared by 1-butyl-3-methylimidazolium tetrafluoroborate particle liquid ([BMIm][BF4]), polyvinylidene fluoride-hexafluoropropylene (P(VDF-HFP)) and N,N-dimethylformamide (DMF).
[0032] In this embodiment, a porous electrolyte layer is prepared by coating an ionogel onto a sponge skeleton. The process is as follows:
[0033] Preparation of ion gel solutions;
[0034] The sponge was immersed in an ion gel solution;
[0035] After soaking, the sponge is removed from the ionogel solution and dried to obtain a porous electrolyte layer.
[0036] In practice, [BMIm][BF4], P(VDF-HFP) and DMF are added to a beaker in a weight ratio of 1:1:10, 2:1:10 or 3:1:10. The beaker is then sealed with plastic wrap to prevent possible evaporation and exchange of substances with the outside environment, thus obtaining a mixed solution. The mixed solution is stirred in a 50°C water bath for 3 hours until the solution becomes transparent, indicating that the polymer particles are completely dissolved, thus obtaining an IL / P(VDF-HFP) ion gel solution.
[0037] The sponge was completely immersed in IL / P (VDF-HFP) ionogel solution, then removed and dried in an oven at 60°C for 40 min to obtain a porous electrolyte layer. The electron micrograph of this porous electrolyte layer is shown below. Figure 2 As shown in E.
[0038] Preferably, the sponge is made of PU sponge, and the electron micrograph of the PU sponge is shown in the figure below. Figure 2 As shown in D.
[0039] In this embodiment, SiO2 is added to nanofibers to obtain SiO2-containing nanofibers. A conductive material is then coated onto the surface of the SiO2-containing nanofibers to prepare the upper and lower electrodes. The SiO2-containing nanofibers are fabricated using an electrospinning process.
[0040] Preferably, the nanofibers containing SiO2 are made of TPU nanofibers, and silica (SiO2) is embedded in the TPU nanofibers. The process for preparing the nanofibers containing SiO2 is as follows:
[0041] Preparation of TPU solution;
[0042] A TPU / SiO2 solution was prepared by adding SiO2 to the TPU solution.
[0043] Electrospinning of TPU / SiO2 solution yielded nanofibers containing SiO2.
[0044] In practice, TPU (thermoplastic polyurethane elastomer rubber) particles are added to a mixed organic solution of THF (tetrahydrofuran) and DMF in a weight ratio of 1:1. The mixed solution is then stirred at 70°C for 2 hours until all TPU particles are dissolved, thus preparing a TPU solution with a TPU concentration of 17 wt.%.
[0045] SiO2 microspheres were added to a TPU solution and stirred for 20 minutes using an emulsifying shear mixer to prepare a TPU / SiO2 solution with a SiO2 concentration of 1.0 wt%.
[0046] The prepared TPU / SiO2 solution was added to a plastic syringe equipped with a metal needle, and then a high voltage of 20 kV was applied at the syringe needle tip at a rate of 0.1 ml / min. -1 Electrospinning was performed at a constant flow rate for 1 hour. All electrospun TPU / SiO2 nanofibers were carefully collected on an aluminum foil-covered collector placed 20 cm from the syringe nozzle. The collection was then peeled off to form TPU / SiO2 nanofibers, which are nanofibers containing SiO2. An electron micrograph of the nanofibers is shown below. Figure 2 As shown in Figure A, the EDS elemental distribution diagram of this nanofiber is as follows: Figure 2 As shown in C.
[0047] In this embodiment, after preparing nanofibers containing SiO2, the nanofibers containing SiO2 are cleaned to obtain cleaned nanofibers; a conductive material is sprayed onto the surface of the cleaned nanofibers to obtain an upper electrode or a lower electrode.
[0048] Specifically, SiO2-containing nanofibers were placed in a plasma cleaner and subjected to oxygen cleaning at a vacuum degree of 100 Pa for 1 minute under a plasma cleaner power of 30W, obtaining cleaned nanofibers; then, 5 mg·ml... -1 A conductive material solution is sprayed onto the cleaned nanofiber surface for 1 minute to form the upper or lower electrode. SEM images and EDS elemental distribution maps of the upper and lower electrodes are shown below. Figure 2 As shown in B.
[0049] Preferably, the conductive material is MXene conductive material.
[0050] In this embodiment, nanofibers containing SiO2 are obtained through electrospinning, so that both the upper and lower electrodes have an uneven nanofiber structure, thereby improving the breathability and moisture permeability of the electronic skin and enhancing its sensitivity.
[0051] Furthermore, both the upper and lower electrodes contain SiO2, which utilizes the microsphere structure of SiO2 to provide excellent light reflection capabilities, thereby enabling the electronic skin to have a good passive cooling effect and thus delay the rise in skin temperature.
[0052] In addition, to protect the upper and lower electrodes, this embodiment also provides hydrophobic layers on the surfaces of the upper and lower electrodes respectively.
[0053] In this embodiment, when preparing electronic skin, a hydrophobic layer is first set on the surface of the upper electrode and the surface of the lower electrode respectively; then the upper electrode with the hydrophobic layer is attached to the upper surface of the porous electrolyte layer, and the lower electrode with the hydrophobic layer is attached to the lower surface of the porous electrolyte layer to prepare a breathable electronic skin.
[0054] The process of preparing hydrophobic layers on the surfaces of the upper and lower electrodes is as follows:
[0055] Preparation of stearic acid solution;
[0056] A stearic acid solution is sprayed onto the surfaces of the upper and lower electrodes and dried to create hydrophobic layers on the surfaces of the upper and lower electrodes, respectively.
[0057] In practice, 0.2 g of stearic acid is added to 50 mL of hot water under magnetic stirring at 1000 rpm, and then stirred at 70 °C for 1 hour to obtain a stearic acid solution.
[0058] The prepared stearic acid emulsion was uniformly sprayed onto the surface of the upper electrode for 10 seconds and the surface of the lower electrode for 10 seconds. Then, the sprayed upper and lower electrodes were placed in an oven at 70°C and dried for 20 minutes, thereby setting hydrophobic layers on the surfaces of the upper and lower electrodes respectively, making the upper and lower electrodes change from hydrophilic to hydrophobic.
[0059] In this embodiment, the upper and lower electrodes are attached to both sides of the porous electrolyte layer using an adhesive method. Specifically:
[0060] A small amount of viscous IG solution was uniformly applied to the upper and lower surfaces of the porous electrolyte layer as an adhesive. Then, the upper electrode was attached to the upper surface of the porous electrolyte layer and the lower electrode was attached to the lower surface of the porous electrolyte layer. The mixture was dried in an oven at 50°C for 20 minutes to obtain a breathable electronic skin with thermal management function.
[0061] The expected EDS elemental distribution map corresponding to the cross-sectional electron microscope image of the breathable electronic skin disclosed in this embodiment is as follows: Figure 2 As shown in F.
[0062] This embodiment discloses a breathable electronic skin that can be pressed, bent, and twisted without compromising its structure and performance, and also possesses ultra-lightweight properties, such as... Figure 2 As shown in G.
[0063] This embodiment discloses a breathable electronic skin that can be attached to human skin 6 to monitor human health.
[0064] When the electronic skin disclosed in this embodiment is attached to human skin for 6 hours, if the pressure between the human skin and the electronic skin changes, the upper electrode, the porous electrolyte layer and the lower electrode will deform, causing the contact area between the upper electrode, the lower electrode and the porous electrolyte layer to change, thereby changing the capacitance value of the electronic skin. Therefore, by measuring the capacitance value of the electronic skin, the pressure between the electronic skin and the human skin can be obtained, and the health status of the human body can be judged based on the pressure.
[0065] The sensor performance of a breathable electronic skin disclosed in this embodiment was tested, and the sensitivity curve of the electronic skin was obtained as follows: Figure 3 As shown in Figure A, the corresponding time curve of the electronic skin is as follows: Figure 3 As shown in Figure B, the stepped test curve of the electronic skin is as follows: Figure 3 As shown in Figure C, the stability test results of the electronic skin are as follows: Figure 3 As shown in D.
[0066] The sensitivity curve shows that the sensitivity of this electronic skin in the first stage is 11.20 kPa. -1 The sensitivity of the second stage is 105.77 kPa. -1 The response time curves show that the response time is 30ms under 1kPa pressure and 40ms under pressure release. The stepped test curves show that the capacitance of the electronic skin increases proportionally with the applied pressure. Stability tests show that after 15,000 cycles of pressure at 1kPa, the capacitance response curve of the electronic skin did not show significant performance degradation, demonstrating the stability and reliability of the electronic skin disclosed in this embodiment.
[0067] The electronic skin disclosed in this embodiment was subjected to hydrophobicity, breathability, and biocompatibility tests. The hydrophobicity test results, breathability test results, and biocompatibility test results are as follows: Figure 4 As shown in A, B, and C.
[0068] The hydrophobicity test results show that the contact angle between artificial sweat, water, and the electronic skin is greater than 135°, proving the hydrophobic properties of the electronic skin. The breathability test results show that the sensor's breathability rate is 48.5 mm / s, which is better than nylon, PDMS film, and medical tape. The biocompatibility test results show that the electronic skin will not cause redness or swelling after prolonged wear, ensuring comfort during long-term wear.
[0069] Passive cooling tests were conducted on the electronic skin disclosed in this embodiment to obtain passive cooling test results and characterization. Figure 5 Figure A shows the solar reflectance and thermal emissivity of TPU nanofibers and TPU nanofibers with added SiO2. It can be seen that adding SiO2 to TPU nanofibers significantly improves the reflectance and emissivity of the electronic skin, effectively increasing its outdoor radiative cooling capacity.
[0070] Figure 5 Figure B shows the cooling performance results of various materials tested continuously for 6 hours. It can be seen that the nanofibers obtained after adding SiO2 to TPU nanofibers have the lowest temperature, proving that nanofibers containing SiO2 have the best cooling effect.
[0071] Figure 5 In Figure C, cotton cloth, TPU nanofibers, and nanofibers containing SiO2 were applied to the arm, and the skin was exposed to sunlight for 10 minutes. The skin covered by the nanofibers containing SiO2 had the lowest temperature, indicating its cooling effect.
[0072] This embodiment also tested the sensitivity and strain range of electronic skin made of ion gel solutions of different concentrations (different ion liquid contents), and the test results are shown in Table 1.
[0073] Table 1
[0074] Ionic liquid content (wt%) <![CDATA[Sensitivity S1 (kPa -1 )]]> Pressure range (kPa) <![CDATA[Sensitivity S2(kPa -1 )]]> Pressure range (kPa) 10 4.11 0-20 17.76 40-74 20 7.62 0-26 71.54 46-74 30 11.2 0-26 105.77 48-74
[0075] This indicates that the electronic skin disclosed in this embodiment has good sensitivity and a large pressure measurement range.
[0076] Therefore, this embodiment discloses a breathable electronic skin that is breathable, sweat-proof, and has passive radiative cooling and health monitoring functions. In hot environments, it can effectively reduce body temperature, monitor physiological signals, and determine the body's health status based on the characteristics of these signals. Its porous electrolyte layer uses a sponge as a base, with an ionogel coated on the sponge skeleton, giving the electrolyte layer a porous structure. This results in excellent breathability and increases the sensitivity and range of detection. Nanofibers are obtained through electrospinning, giving them a rich, uneven structure, further improving the breathability and moisture permeability of the electronic skin, as well as its detection sensitivity.
[0077] In this embodiment, SiO2 is added to the nanofibers, so that the upper and lower electrodes can utilize the microsphere structure of SiO2, thereby possessing good visible light reflection capability and high infrared emission capability, achieving the passive cooling effect of electronic skin, and further preventing the human skin temperature from rising.
[0078] Example 2
[0079] In this embodiment, a method for preparing a breathable electronic skin as disclosed in Example 1 is disclosed, comprising:
[0080] A porous electrolyte layer was prepared by coating an ionogel onto the framework of a sponge.
[0081] Adding SiO2 to nanofibers yields nanofibers containing SiO2.
[0082] A conductive material is coated on the surface of nanofibers containing SiO2 to prepare an upper electrode and a lower electrode.
[0083] The upper and lower electrodes are respectively attached to the two sides of the porous electrolyte layer, enabling the porous electrolyte layer to carry out charge transfer between the upper and lower electrodes, thus preparing a breathable electronic skin.
[0084] Furthermore, the process for preparing the porous electrolyte layer is as follows:
[0085] Preparation of ion gel solutions;
[0086] The sponge was immersed in an ion gel solution;
[0087] After soaking, the sponge is removed from the ionogel solution and dried to obtain a porous electrolyte layer.
[0088] Furthermore, the process for preparing nanofibers containing SiO2 is as follows:
[0089] Preparation of TPU solution;
[0090] A TPU / SiO2 solution was prepared by adding SiO2 to the TPU solution.
[0091] Electrospinning of TPU / SiO2 solution yielded nanofibers containing SiO2.
[0092] Furthermore, the nanofibers containing SiO2 are cleaned to obtain cleaned nanofibers.
[0093] Conductive material is sprayed onto the cleaned nanofiber surface to obtain an upper electrode or a lower electrode.
[0094] Furthermore, the upper electrode is attached to the upper surface of the porous electrolyte layer, and the lower electrode is attached to the lower surface of the porous electrolyte layer.
[0095] Furthermore, hydrophobic layers are respectively provided on the surface of the upper electrode and the surface of the lower electrode;
[0096] An upper electrode with a hydrophobic layer is attached to the upper surface of a porous electrolyte layer, and a lower electrode with a hydrophobic layer is attached to the lower surface of the porous electrolyte layer to prepare a breathable electronic skin.
[0097] Further, a stearic acid solution is prepared;
[0098] A stearic acid solution is sprayed onto the surfaces of the upper and lower electrodes and dried to create hydrophobic layers on the surfaces of the upper and lower electrodes, respectively.
[0099] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A breathable electronic skin, characterized in that, It includes an upper electrode, a porous electrolyte layer, and a lower electrode; the porous electrolyte layer includes a sponge and an ion gel, with the ion gel coating the sponge skeleton; both the upper and lower electrodes include nanofibers containing SiO2 and conductive materials, with the conductive materials covering the surface of the nanofibers; the porous electrolyte layer is located between the upper and lower electrodes and is capable of charge transfer between the upper and lower electrodes. Hydrophobic layers are respectively provided on the surface of the upper electrode and the surface of the lower electrode; The ion gel was prepared by using 1-butyl-3-methylimidazolium tetrafluoroborate particles liquid, polyvinylidene fluoride-hexafluoropropylene and N,N-dimethylformamide; The nanofibers containing SiO2 are made by embedding SiO2 into TPU nanofibers. SiO2 is added to TPU solution to prepare TPU / SiO2 solution; the concentration of SiO2 in TPU / SiO2 solution is 1.0 wt%.
2. The breathable electronic skin as described in claim 1, characterized in that, The sponge is made of PU sponge; the conductive material is MXene conductive material; and the nanofibers containing SiO2 are made by electrospinning.
3. The method for preparing a breathable electronic skin as described in any one of claims 1-2, characterized in that, include: A porous electrolyte layer was prepared by coating an ionogel onto the framework of a sponge. Adding SiO2 to nanofibers yields nanofibers containing SiO2. A conductive material is coated on the surface of nanofibers containing SiO2 to prepare an upper electrode and a lower electrode. The upper and lower electrodes are respectively attached to the two sides of the porous electrolyte layer, enabling the porous electrolyte layer to carry out charge transfer between the upper and lower electrodes, thus preparing a breathable electronic skin.
4. The method for preparing a breathable electronic skin as described in claim 3, characterized in that, The process for preparing a porous electrolyte layer is as follows: Preparation of ion gel solutions; The sponge was immersed in an ion gel solution; After soaking, the sponge is removed from the ionogel solution and dried to obtain a porous electrolyte layer.
5. The method for preparing a breathable electronic skin as described in claim 3, characterized in that, The process for preparing nanofibers containing SiO2 is as follows: Preparation of TPU solution; A TPU / SiO2 solution was prepared by adding SiO2 to the TPU solution. Electrospinning of TPU / SiO2 solution yielded nanofibers containing SiO2.
6. The method for preparing a breathable electronic skin as described in claim 3, characterized in that, The nanofibers containing SiO2 were cleaned to obtain cleaned nanofibers. Conductive material is sprayed onto the cleaned nanofiber surface to obtain an upper electrode or a lower electrode.
7. The method for preparing a breathable electronic skin as described in claim 3, characterized in that, The upper electrode is attached to the upper surface of the porous electrolyte layer, and the lower electrode is attached to the lower surface of the porous electrolyte layer.
8. The method for preparing a breathable electronic skin as described in claim 7, characterized in that, Hydrophobic layers are respectively provided on the surface of the upper electrode and the surface of the lower electrode; An upper electrode with a hydrophobic layer is attached to the upper surface of a porous electrolyte layer, and a lower electrode with a hydrophobic layer is attached to the lower surface of the porous electrolyte layer to prepare a breathable electronic skin.
Citation Information
Patent Citations
Radiation refrigeration fiber membrane and preparation method and application thereof
CN110042564A
Flexible sensor, preparation method and application thereof, and wearable device
CN113280954A
Microstructured tactile sensor based on pseudocapacitance principle and preparation method thereof