Resistance paste, heating element and aerosol generating device

By using a resistive slurry containing an organic carrier and metal powder in an aerosol generating device, with nickel-chromium alloy as the supporting skeleton, silver and nickel powder filling the gaps, and chromium powder improving the bonding strength, the problems of ceramic matrix cracking and resistance mismatch are solved, and low-temperature sintering and high-stability heating element are achieved.

CN117393202BActive Publication Date: 2026-11-17ALD GRP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210781757.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-04
Publication Date
2026-11-17
Estimated Expiration
2042-07-04

AI Technical Summary

Technical Problem

The porous ceramic thick-film heating element in existing aerosol generating devices is prone to cracking due to its high sintering temperature, and its resistance value does not meet the requirements, which affects the service life and cost of the heating element.

Method used

A resistance paste containing an organic carrier and dispersed metal and glass powders is used. A nickel-chromium alloy serves as the supporting framework, while silver and nickel powders fill the gaps. Chromium powder improves the bonding strength, lowers the sintering temperature, and meets the resistance value requirements.

Benefits of technology

The sintering temperature was lowered to prevent brittle fracture and cracking of the ceramic matrix, which improved the service life of the heating element and the stacking strength of the resistance paste, enhanced the stability and reliability of the heating element, and reduced the resistance value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117393202B_ABST
    Figure CN117393202B_ABST
Patent Text Reader

Abstract

This application relates to a resistance paste, a heating element, and an aerosol generating device. The resistance paste includes an organic carrier and metal powder and glass powder dispersed within the organic carrier. The metal powder includes silver powder, chromium powder, nickel powder, and a nickel-chromium alloy. The average particle size of the nickel-chromium alloy is larger than that of the silver, chromium, or nickel powder. The nickel-chromium alloy forms a supporting framework in the resistance paste, and the silver, chromium, and nickel powders fill the voids between the nickel-chromium alloy particles. The resistance paste, heating element, and aerosol generating device provided by this application can reduce the sintering temperature and damage to the porous ceramic matrix, prevent brittle fracture of the ceramic matrix, and improve the lifespan of the heating element.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of resistive paste technology, and more particularly to resistive paste, heating element and aerosol generating device. Background Technology

[0002] Existing porous ceramic thick-film heating elements in aerosol generating devices suffer from poor substrate structure, making it easy for metal powder to fall into the pits on the ceramic surface. To obtain a good heating circuit, the metal powder used is typically large in particle size, resulting in low sintering activity and high sintering temperatures, often exceeding 1000℃. Excessive sintering temperatures can degrade the mechanical properties of porous ceramics, causing cracking at the contact points between the ceramic substrate and the conductive film during operation. Furthermore, the high sintering temperature increases costs and wastes energy. While reducing the powder particle size improves sintering activity and lowers the sintering temperature, it results in a high resistance value, failing to meet performance requirements. Additionally, the high powder activity leads to severe powder shrinkage during sintering, resulting in insufficient heating circuit packing and numerous cracks in the heating element itself, causing large resistance variations or even burnout during operation.

[0003] Therefore, there is an urgent need for a resistance paste that can meet the resistance requirements of the heating element while reducing the sintering temperature and damage to the porous ceramic matrix, preventing brittle fracture and cracking of the ceramic matrix, and improving the lifespan of the heating element. Summary of the Invention

[0004] The present invention provides a resistive paste, a heating element, and an aerosol generating device, which can reduce the sintering temperature and reduce damage to the porous ceramic matrix, prevent the ceramic matrix from brittlely cracking, and improve the life of the heating element.

[0005] In a first aspect, this application provides a resistive paste, the resistive paste comprising an organic carrier and metal powder and glass powder dispersed within the organic carrier; wherein the metal powder comprises silver powder, chromium powder, nickel powder and nickel-chromium alloy, wherein the average particle size of the nickel-chromium alloy is larger than the average particle size of the silver powder, the chromium powder or the nickel powder, the nickel-chromium alloy forms a supporting skeleton in the resistive paste, and the silver powder, the chromium powder and the nickel powder fill the voids between the nickel-chromium alloy particles.

[0006] In conjunction with the first aspect, in one feasible implementation, the resistive paste satisfies at least one of the following characteristics:

[0007] (1) The metal powder also includes at least one of aluminum powder and iron powder;

[0008] (2) The nickel-chromium alloy includes at least one of NiCr20, NiCr70, NiCr50, and NiCrFe;

[0009] (3) The average particle size of the nickel-chromium alloy is 25 μm to 38 μm;

[0010] (4) The average particle size of the silver powder is 0.2 μm to 3 μm;

[0011] (5) The average particle size of the nickel powder is 1 μm to 5 μm;

[0012] (6) The average particle size of the chromium powder is 5 μm to 23 μm;

[0013] (7) The shape of the silver powder includes at least one of amorphous, spherical, near-spherical and flake-like.

[0014] In conjunction with the first aspect, in one feasible implementation, based on the mass of the resistive paste as 100%, the metal powder includes 4% to 10% silver powder, 2% to 6% chromium powder, 34% to 46% nickel-chromium alloy, and 20% to 30% nickel powder.

[0015] In conjunction with the first aspect, in one feasible implementation, the resistive paste satisfies at least one of the following characteristics:

[0016] (1) The glass powder is silicon borosilicate glass powder;

[0017] (2) The glass powder is silicon borosilicate glass powder, and the average particle size of the silicon borosilicate glass powder is 10μm to 20μm;

[0018] (3) The glass powder is a silicon borosilicate glass powder, and the melting point of the silicon borosilicate glass powder is 800℃~850℃;

[0019] (4) The mass ratio of the metal powder, the glass powder and the organic carrier is 100:(5-15):(10-30).

[0020] In conjunction with the first aspect, in one feasible embodiment, the organic carrier includes an organic solvent, an organic resin, and an organic additive, wherein the mass ratio of the organic solvent to the organic resin to the organic additive is 100:(15-25):(20-50).

[0021] In conjunction with the first aspect, in one feasible implementation, the resistive paste satisfies at least one of the following characteristics:

[0022] (1) The organic solvent includes at least one of ethylene glycol butyl ether, terpineol, diethylene glycol ethyl ether acetate, divalent ester, dodecyl alcohol ester, butyl formate, butyl carbitol and butyl carbitol acetate;

[0023] (2) The organic additives include thixotropic agents and dispersants;

[0024] (3) The organic additives include thixotropic agents and dispersants, wherein the thixotropic agents include at least one of organic bentonite, hydrogenated castor oil and polyamide wax;

[0025] (4) The organic additives include thixotropic agents and dispersants, wherein the dispersants include at least one of polyacrylamide, cellulose derivatives and acrylic acid;

[0026] (5) The organic resin includes at least one of acrylic resin and cellulose resin;

[0027] (6) The organic additive also includes a coupling agent, which includes at least one of silane coupling agents, bimetallic coupling agents and chromium complexes.

[0028] In a second aspect, embodiments of this application provide a heating element, the heating element comprising a porous ceramic substrate and a heating film layer formed on the porous ceramic substrate; the heating film layer is formed from the resistive paste as described in the first aspect.

[0029] In conjunction with the second aspect, in one feasible implementation, the heating element satisfies at least one of the following characteristics:

[0030] (1) The thickness of the heating film layer is 70μm to 100μm;

[0031] (2) The width of the heating film layer is 3.5μm to 4.5μm;

[0032] (3) The porous ceramic matrix is ​​a diatomite and montmorillonite mixed ceramic;

[0033] (4) The porosity of the porous ceramic matrix is ​​55% to 60%, and the oil conduction rate of the porous ceramic matrix is ​​1.3 μl / s to 2.5 μl / s.

[0034] Thirdly, embodiments of this application provide a method for preparing a heating element, the method comprising the following steps:

[0035] A resistive paste is printed on the surface of a porous ceramic substrate, dried, and then sintered at 850℃~950℃ for 20min~30min to obtain a heating element, wherein the resistive paste is as described in the first aspect.

[0036] Fourthly, embodiments of this application provide an aerosol generating device, including the heating element described in the third aspect.

[0037] Compared with the prior art, the technical solution provided in this application has at least the following beneficial effects:

[0038] The resistive slurry, heating element, and aerosol generating device provided in this application include a resistive slurry comprising an organic carrier and metal powder and glass powder dispersed within the organic carrier. The metal powder includes nickel powder, chromium powder, nickel-chromium alloy, and silver powder. While meeting the resistance requirements of the heating circuit, the large-particle-size nickel-chromium alloy acts as a spatial skeleton for the heating circuit, ensuring the slurry's packing strength and preventing excessive cracking of the heating element due to severe shrinkage and settling during high-temperature sintering. The silver, nickel, and chromium powders filling the gaps between the nickel-chromium alloy particles fill these gaps, increasing the solid content of the sintered heating circuit. Nickel powder enhances sintering activity and lowers the overall sintering temperature of the slurry. Chromium powder wets the porous ceramic substrate, improving bonding strength, and the nickel-chromium alloy formed by chromium and nickel powder improves the reliability of the heating element and the safety of the atomized smoke. Silver powder acts as an aid in sintering, lowering the sintering temperature and increasing the alloying effect, enhancing the stability and reliability of the heating element during operation. It also acts as a conductive agent, reducing the resistance value of the heating element.

[0039] Secondly, metal powder and glass powder are dispersed in an organic carrier. After the resistive slurry is coated onto a porous ceramic substrate, the porous ceramic substrate can absorb part of the slurry, preventing the slurry from flowing to both sides of the porous ceramic substrate, ensuring the stacking strength of the resistive slurry, and extending the service life of the sintered heating film layer, thereby ensuring the service life of the heating element. Attached Figure Description

[0040] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0041] Figure 1 This is a schematic flowchart of the method for preparing a heating element provided in the embodiments of this application. Detailed Implementation

[0042] To better understand the technical solution of the present invention, the embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0043] It should be understood that the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0044] The terminology used in the embodiments of this invention is for the purpose of describing particular embodiments only and is not intended to limit the invention. The singular forms “a,” “the,” and “the” as used in the embodiments of this invention and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise.

[0045] Furthermore, the features, operations, or characteristics described in the specification can be combined in any suitable manner to form various embodiments. At the same time, the steps or actions in the method description can be rearranged or adjusted in a manner obvious to those skilled in the art. Therefore, the various orders in the specification and drawings are only for the clear description of a particular embodiment and do not imply a necessary order, unless otherwise stated that a particular order must be followed.

[0046] The serial numbers assigned to components in this document, such as "first" and "second," are used only to distinguish the described objects and have no sequential or technical meaning. Unless otherwise specified, the terms "connection" and "linkage" used in this application include both direct and indirect connections.

[0047] The term "aerosol generating device" as used in this article refers to a device that generates aerosols by heating the aerosol generating product to a temperature below its combustion temperature, thereby avoiding the generation of toxic and harmful substances due to the combustion of the aerosol generating product.

[0048] In a first aspect, this application provides a resistive paste, the resistive paste comprising an organic carrier and metal powder and glass powder dispersed within the organic carrier; the metal powder comprising silver powder, chromium powder, nickel powder and nickel-chromium alloy, wherein the average particle size of the nickel-chromium alloy is larger than the average particle size of the silver powder, the chromium powder or the nickel powder, the nickel-chromium alloy forms a supporting skeleton in the resistive paste, and the silver powder, the chromium powder and the nickel powder fill the voids between the nickel-chromium alloy particles.

[0049] In the above scheme, the resistive slurry includes an organic carrier and metal powder and glass powder dispersed within the organic carrier. The metal powder includes nickel powder, chromium powder, nickel-chromium alloy, and silver powder. While meeting the resistance requirements of the heating circuit, the large-particle-size nickel-chromium alloy acts as a spatial skeleton for the heating circuit, ensuring the slurry's packing strength and preventing excessive cracking of the heating element due to severe shrinkage and settling during high-temperature sintering. The silver, nickel, and chromium powders filling the gaps between the nickel-chromium alloy particles fill these gaps, increasing the solid content of the sintered heating circuit. Nickel powder enhances sintering activity and lowers the overall sintering temperature of the slurry. Chromium powder wets the porous ceramic substrate, improving bonding strength, and the nickel-chromium alloy formed by chromium and nickel powder improves the reliability of the heating element and the safety of atomized smoke. Silver powder acts as an aid in sintering, lowering the sintering temperature and increasing alloying effects, enhancing the stability and reliability of the heating element during operation. It also acts as a conductive agent, reducing the resistance of the heating element.

[0050] In some embodiments, based on the mass of the resistive paste as 100%, the metal powder includes 4%–10% silver powder, 2%–6% chromium powder, 34%–46% nickel-chromium alloy, and 20%–30% nickel powder by mass. Experiments have shown that the metal powder prepared according to this ratio, with silver, nickel, and chromium powders, can fully fill the gaps between nickel-chromium alloy particles, improving sintering activity, lowering the sintering temperature, and thus increasing the solid content of the sintered heating circuit, ensuring that the heating film layer meets the resistance value requirements.

[0051] The silver powder accounts for 4% to 10% of the mass of the resistive paste, specifically 4%, 5%, 7%, 9%, 10%, etc., and is not limited here. Too high a silver powder content will result in too low a resistance and the heating element will not heat up or work; too low a silver powder content will result in too high a resistance, leading to increased resistance and a shorter lifespan for the heating element due to dry and wet burning.

[0052] In some embodiments, the average particle size of the silver powder is 0.2 μm to 3 μm; specifically, it can be 0.2 μm, 0.35 μm, 0.5 μm, 0.8 μm, 1.0 μm, 1.2 μm, 1.3 μm, 1.5 μm, 1.8 μm, 2.0 μm, 2.4 μm, 2.8 μm, or 3.0 μm, etc., and is not limited here. Using silver powder with a smaller particle size allows it to act as an aid in sintering during the sintering process, lowering the sintering temperature while increasing the alloying effect, enhancing the stability and reliability of the heating element during atomization, and simultaneously acting as a conductive agent to reduce the resistance value of the heating element. Understandably, as the particle size of the silver powder decreases, the sintering temperature of the resistive slurry containing silver powder will decrease. However, if the particle size of the silver powder is too small, it is prone to agglomeration. By controlling the particle size of the silver powder, the sintering temperature of the resistive slurry can be ensured to be within a preset range, and the problem of uneven dispersion of silver powder in the resistive slurry can also be effectively avoided.

[0053] In some embodiments, the silver powder has at least one shape selected from amorphous, spherical, near-spherical, and flake-like. Preferably, the silver powder can be a mixture of amorphous silver powder and spherical or near-spherical silver powder. Using two different particle shapes of metal powder together ensures effective and dense packing of the metal powder in the formed heating film layer, improves sintering activity, ensures circuit conductivity, and reduces resistance.

[0054] In some embodiments, the nickel powder accounts for 20% to 30% of the resistive slurry by mass, specifically 20%, 22%, 24%, 25%, 27%, 28%, 30%, etc., and is not limited thereto. The nickel powder content affects the sintering activity of the resistive slurry. An appropriate mass percentage of nickel powder can improve sintering activity, reduce the overall sintering temperature of the slurry, and enable it to fully alloy with chromium powder, thereby improving the service life of the heating element.

[0055] In some embodiments, the average particle size of the nickel powder is 1 μm to 5 μm, specifically 1 μm, 1.2 μm, 1.5 μm, 1.7 μm, 2.1 μm, 2.8 μm, 3.2 μm, 3.5 μm, 4.0 μm, 4.5 μm, or 5 μm, etc., and is not limited thereto. By controlling the particle size of the nickel powder, smaller particles can improve the sintering activity of the resistance slurry and reduce the overall sintering temperature of the slurry.

[0056] In some embodiments, the nickel-chromium alloy accounts for 34% to 46% of the mass of the resistance slurry, specifically 34%, 36%, 38%, 40%, 42%, 44%, 46%, etc., and is not limited thereto. The nickel-chromium alloy content affects the sintering activity of the resistance slurry. An appropriate mass percentage of nickel-chromium alloy can ensure the packing strength of the resistance slurry, prevent excessive cracking of the heating element due to severe shrinkage and settling during high-temperature sintering, and avoid the slurry penetrating too deeply into the ceramic during sintering, leading to carbon buildup, core clogging, or even burn-out.

[0057] In some embodiments, the nickel-chromium alloy includes at least one of NiCr20, NiCr70, NiCr50, and NiCrFe.

[0058] In some embodiments, the average particle size of the nickel-chromium alloy is 25μm to 38μm, specifically 25μm, 28μm, 30μm, 35μm, or 38μm, etc., and is not limited thereto. By controlling the particle size of the nickel-chromium alloy, the larger particles of nickel-chromium alloy can serve as the spatial framework of the heating film layer, preventing excessive cracking of the heating element due to severe shrinkage of the resistive paste during high-temperature sintering.

[0059] In some embodiments, the chromium powder accounts for 2% to 6% of the mass of the resistor paste, specifically 2%, 3%, 4%, 5%, 6%, etc., and is not limited here.

[0060] The average particle size of the chromium powder is 5μm to 23μm, specifically 5μm, 5.5μm, 7.5μm, 10μm, 12μm, 13μm, 15μm, 18μm, 20μm, 21μm, or 23μm, etc., and is not limited here. The chromium powder has a slightly larger particle size than the nickel powder, which is beneficial for the formation of a nickel-chromium alloy with larger particle size during the sintering process. This alloy can serve as the spatial framework of the heating film layer, preventing excessive cracking of the heating element due to severe shrinkage of the resistance paste during high-temperature sintering. By controlling the particle size of the chromium powder, it is beneficial to control the particle size of the formed nickel-chromium alloy.

[0061] In some embodiments, the metal powder further includes at least one of aluminum powder and iron powder.

[0062] In some embodiments, the glass powder is a silicon borosilicate glass powder.

[0063] In some embodiments, the average particle size of the silicon borosilicate glass powder is 10μm to 20μm; specifically, it can be 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm or 20μm, etc., and is not limited here.

[0064] It should be noted that in this specification, the average particle size is D50, where "D50" represents the 50% particle size on a volume basis in the cumulative particle size distribution. Specifically, it refers to the particle size that accounts for 50% of the cumulative amount on a volume basis in the cumulative particle size curve of the particle size distribution measured using a laser diffraction / scattering particle size distribution measuring device.

[0065] In some embodiments, the melting point of the borosilicate glass powder is 800℃~850℃, specifically 800℃, 810℃, 820℃, 830℃ or 850℃, etc., which are not limited here.

[0066] In some embodiments, the mass ratio of the metal powder, the glass powder, and the organic carrier is 100:(5-15):(10-30), specifically 100:5:10, 100:5:15, 100:5:20, 100:5:25, 100:5:30, 100:10:10, 100:10:20, 100:10:30, 100:15:10, 100:15:20, 100:15:30, etc., and is not limited here.

[0067] In some embodiments, the organic carrier includes an organic solvent, an organic resin, and an organic additive, wherein the mass ratio of organic solvent:organic resin:organic additive is 100:(15-25):(20-50). Specifically, it can be 100:15:20, 100:15:30, 100:15:40, 100:15:50, 100:20:20, 100:20:30, 100:20:40, 100:20:50, 100:25:20, 100:25:30, 100:25:40, 10:25:50, etc., and is not limited thereto.

[0068] In some embodiments, the organic solvent includes at least one selected from ethylene glycol butyl ether, terpineol, diethylene glycol ethyl ether acetate, divalent ester (abbreviated as DBE), dodecyl alcohol ester, butyl formate, butyl carbitol, and butyl carbitol acetate.

[0069] In some embodiments, the organic additive includes a thixotropic agent and a dispersant. In other embodiments, the organic additive may also include a coupling agent, specifically at least one selected from silane coupling agents, bimetallic coupling agents, and chromium complexes.

[0070] In some embodiments, the thixotropic agent comprises at least one selected from organobentonite, hydrogenated castor oil, and polyamide wax. The dispersant comprises at least one selected from polyacrylamide, cellulose derivatives, and acrylic acid.

[0071] In some embodiments, the organic resin includes at least one of acrylic resins and cellulose resins. Specifically, the acrylic resin may be at least one of methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-hydroxyethyl methacrylate, methyl acrylate, ethyl acrylate, butyl acrylate, 2-hydroxyethyl acrylate, etc. The cellulose resin may be at least one of methylcellulose, ethylcellulose, carboxymethylcellulose, hydroxyethylcellulose, benzylcellulose, propylcellulose, nitrocellulose, etc. Preferably, the acrylic resin is methyl acrylate, and the cellulose resin is ethylcellulose.

[0072] When the organic resin binder is a cellulose-based resin, diethylene glycol monobutyl ether, terpineol, diethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, and propylene glycol diacetate are preferred organic solvents. When the organic resin binder is an acrylic-based resin, diethylene glycol monobutyl ether, methyl ethyl ketone, terpineol, diethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, and propylene glycol diacetate are preferred solvents. These solvents can be used alone or in combination.

[0073] Secondly, this application provides a heating element, the heating element comprising a porous ceramic substrate and a heating film layer formed on the porous ceramic substrate; the heating film layer is formed from the above-mentioned resistive paste.

[0074] In some embodiments, the porous ceramic matrix is ​​made of a diatomaceous earth and montmorillonite mixed ceramic.

[0075] In some embodiments, the porosity of the porous ceramic matrix is ​​55%-60%. Specifically, the porosity can be 55%, 56%, 57%, 58%, 59%, or 60%, etc., and is not limited thereto. Controlling the porosity of the porous ceramic matrix can improve its stability in use.

[0076] In some embodiments, the oil conduction rate of the porous ceramic substrate is 1.3 μl / s to 2.5 μl / s, specifically 1.3 μl / s, 1.4 μl / s, 1.5 μl / s, 1.6 μl / s, 1.7 μl / s, 1.8 μl / s, 1.9 μl / s, 2.0 μl / s, 2.3 μl / s, 2.5 μl / s, etc., and is not limited thereto. Controlling the oil conduction rate of the porous ceramic substrate can facilitate the formation of a heating film layer of uniform thickness on the surface of the resistive slurry.

[0077] In some embodiments, the width of the heating film layer is 3.5μm to 4.5μm, specifically it can be 3.5μm, 3.6μm, 3.7μm, 3.8μm, 3.9μm, 4.0μm, 4.2μm, 4.4μm or 4.5μm, etc., and is not limited here.

[0078] The thickness of the heating film layer is 70μm to 100μm; specifically, it can be 70μm, 72μm, 75μm, 78μm, 80μm, 82μm, 85μm, 88μm, 89μm, 90μm, 95μm or 100μm, etc., and is not limited here.

[0079] Thirdly, embodiments of this application also provide a method for preparing a heating element, such as... Figure 1 As shown, the method includes the following steps:

[0080] S10, a resistive paste is printed on the surface of a porous ceramic substrate, dried, and then sintered at 850℃~950℃ for 20min~30min to obtain a heating element. The resistive paste is the resistive paste described in the first aspect.

[0081] In the above scheme, due to the relatively low sintering temperature, the strength of the porous ceramic matrix is ​​not affected after the second sintering following the printing of the resistance paste, which can effectively prevent the ceramic from brittlely cracking. The resistance paste can still meet the resistance value required for the operation of the heating element at a low sintering temperature, which can improve the service life of the heating element. In terms of performance, it can meet the assembly and use requirements of the aerosol generating device.

[0082] Specifically, prior to step S10, the method further includes:

[0083] S01, the mixture including organic carrier, metal powder and glass powder is dispersed to obtain resistor slurry.

[0084] The performance parameters of the organic carrier, metal powder and glass powder are detailed in the first part and will not be repeated here.

[0085] In some embodiments, the dispersion treatment includes at least one of mechanical stirring, magnetic stirring, or ultrasonic stirring. Specifically, the dispersion treatment is mechanical stirring, with a stirring speed of 500 r / min to 1000 r / min, and the stirring temperature can be controlled between 20°C and 30°C, for example, 20°C, 25°C, 30°C, etc., which are not limited here, as long as the various components in the resistive slurry are evenly dispersed.

[0086] Prior to S01, the method further includes:

[0087] Formulate an organic carrier comprising organic solvents, organic resins, and organic additives.

[0088] During the preparation of the organic carrier, the mass ratio of organic solvent: organic resin: organic additive is controlled to be 100:(15-25):(20-50), specifically 100:15:20, 100:15:30, 100:15:40, 100:15:50, 100:20:20, 100:20:30, 100:20:40, 100:20:50, 100:25:20, 100:25:30, 100:25:40, 10:25:50, etc., which are not limited here.

[0089] During the preparation process, the uniformity of the organic carrier can be improved by stirring. The conditions for preparing the organic carrier include: heating temperature of 80℃~110℃, time of 2h~3h, and stirring speed of 500r / min~1000r / min; understandably, it is sufficient to ensure that the organic carrier is fully dispersed.

[0090] In actual preparation, the organic solvent and organic resin can be mixed first under heating, and then organic additives (thixotropic agents and dispersants) can be added. This staged mixing helps improve the uniformity of the liquid organic carrier.

[0091] S10 involves printing a resistive paste onto the surface of a porous ceramic substrate, drying it, and then sintering it at 850℃~950℃ for 20min~30min to obtain a heating element.

[0092] In some embodiments, the drying temperature is 150℃~200℃, and the drying time is 10min~15min. Specifically, the drying temperature can be 150℃, 160℃, 170℃, 180℃, 185℃, 190℃ or 200℃, etc., and the drying time can be 10min, 11min, 12min, 13min, 14min or 15min, etc.

[0093] In specific embodiments, the drying method includes forced-air drying, steam drying, oven drying, etc. Specifically, a porous ceramic substrate printed with resistive paste can be placed on a quartz boat or graphite boat and then placed in a forced-air drying oven for drying.

[0094] In some embodiments, the sintering temperature is 850℃~950℃, and the sintering time is 20min~30min. Specifically, the sintering temperature can be 850℃, 860℃, 870℃, 880℃, 895℃, 900℃, 920℃, 930℃, or 950℃, etc., and the sintering time can be 20min, 22min, 24min, 25min, 28min, or 30min, etc.

[0095] Understandably, by using the resistance paste provided in the first aspect, the sintering temperature can be reduced during sintering, thus avoiding damage to or blockage of the porous structure of the porous ceramic matrix, preventing excessive cracking of the heating element due to severe shrinkage during high-temperature sintering, and reducing the resistance value of the heating element.

[0096] In some embodiments, the sintered heating element is cooled, and the cooling can be furnace cooling, natural cooling or rapid cooling, which is not limited here.

[0097] In the above-mentioned solution, the heating element provided in this application has a high bonding strength and low resistivity between the heating film layer formed by the resistive paste and the porous ceramic matrix, which can improve the structural stability of the heating element, reduce the contact resistance between the power supply and the heating element, and reduce energy consumption.

[0098] This application also provides an aerosol generating device, including the heating element described above.

[0099] The embodiments of the present invention will be further described below with reference to several examples. However, the embodiments of the present invention are not limited to the specific embodiments described below. Appropriate modifications can be made within the scope of the original claims.

[0100] Example 1

[0101] The method for preparing the heating element in this embodiment:

[0102] (1) Preparation of resistance paste

[0103] Two parts of organic resin (a mixture of ethyl cellulose and acrylic resin) and 9.1 parts of organic solvent (a mixture of butyl carbitol, dicarboxylic acid ester, and butyl acetate) were mixed and mechanically stirred at a speed of 500 r / min and a heating temperature of 80℃ for 5 h to obtain an organic carrier precursor. Then, 3.6 parts of a mixture of (hydrogenated castor oil) thixotropic agent, (acrylic acid) dispersant, and (silane coupling agent) coupling agent were added, and the mixture was mechanically stirred again to obtain the organic carrier.

[0104] (2) Metal powder, silicon borosilicate glass powder and organic carrier in a mass ratio of 77.3:8:14.7 are mixed evenly and then ground and dispersed evenly in a three-roll mill to obtain a resistive slurry; wherein the metal powder includes 38.6 parts of NiCr20 alloy powder (D50=25μm), 5.8 parts of Cr powder (D50=10μm), 4 parts of amorphous Ag powder (D50=0.5μm) and 28.9 parts of Ni powder (D50=1μm);

[0105] (3) Print the resistive paste onto the porous ceramic substrate, dry it at 100°C for 30 min, and then sinter it at 900°C for 30 min to obtain the heating element; wherein the thickness of the heating film layer prepared by printing is 80 μm and the width is 4 μm.

[0106] Example 2

[0107] The heating element in this embodiment has a resistive paste that is basically the same as that in Example 1, except that 38.6 parts of NiCr20 alloy powder (D50 = 38 μm), 3.8 parts of Cr powder (D50 = 10 μm), 6 parts of amorphous silver powder (D50 = 0.2 μm) and 28.9 parts of Ni powder (D50 = 2 μm) are added to every 100 parts of resistive paste.

[0108] Example 3

[0109] The heating element in this embodiment has a resistive paste that is basically the same as that in Example 1, except that 38.6 parts of NiCr20 alloy powder (D50 = 25 μm), 3.8 parts of Cr powder (D50 = 20 μm), 8 parts of amorphous silver powder (D50 = 0.5 μm) and 26.9 parts of Ni powder (D50 = 5 μm) are added to every 100 parts of resistive paste.

[0110] Example 4

[0111] The heating element in this embodiment has a resistive paste that is basically the same as that in Example 1, except that 38.6 parts of NiCr20 alloy powder (D50 = 30 μm), 3.8 parts of Cr powder (D50 = 15 μm), 6 parts of amorphous silver powder (D50 = 3 μm) and 28.9 parts of Ni powder (D50 = 3 μm) are added to every 100 parts of resistive paste.

[0112] Example 5:

[0113] The heating element in this embodiment has a resistive paste that is basically the same as that in Example 1, except that 38.6 parts of NiCr20 alloy powder (D50 = 25 μm), 3.8 parts of Cr powder (D50 = 10 μm), 6 parts of amorphous silver powder (D50 = 3 μm) and 28.9 parts of Ni powder (D50 = 2 μm) are added to every 100 parts of resistive paste.

[0114] Example 6:

[0115] The heating element in this embodiment has a resistive paste that is basically the same as that in Example 1, except that 38.6 parts of NiCr20 alloy powder (D50 = 28 μm), 3.8 parts of Cr powder (D50 = 10 μm), 6 parts of silver powder with a spherical or near-spherical morphology (D50 = 3 μm) and 28.9 parts of Ni powder (D50 = 2 μm) are added to every 100 parts of resistive paste.

[0116] Example 7:

[0117] The heating element in this embodiment has a resistive paste that is basically the same as that in Example 1, except that 38.6 parts of NiCr20 alloy powder (D50 = 25 μm), 3.8 parts of Cr powder (D50 = 10 μm), 6 parts of silver powder with a flake-like morphology (D50 = 2 μm) and 28.9 parts of Ni powder (D50 = 2 μm) are added to every 100 parts of resistive paste.

[0118] Example 8:

[0119] The heating element in this embodiment has a resistive paste that is basically the same as that in Example 1, except that 43 parts of NiCr20 alloy powder (D50 = 25 μm), 2 parts of Cr powder (D50 = 20 μm), 8 parts of amorphous silver powder (D50 = 0.5 μm) and 24.3 parts of Ni powder (D50 = 2 μm) are added to every 100 parts of resistive paste.

[0120] Example 9:

[0121] The heating element in this embodiment has a resistive paste that is basically the same as that in Example 1, except that: 38.6 parts of NiCr20 alloy powder (D50 = 25 μm), 3.8 parts of Cr powder (D50 = 10 μm), 3 parts of amorphous silver powder (D50 = 2 μm), 3 parts of spherical silver powder (D50 = 2 μm) and 28.9 parts of Ni powder (D50 = 2 μm) are added to every 100 parts of resistive paste.

[0122] Example 10:

[0123] The heating element in this embodiment has a resistive paste that is basically the same as that in Example 1, except that 38.6 parts of NiCrFe alloy powder (D50 = 28 μm), 3.8 parts of Cr powder (D50 = 15 μm), 10 parts of amorphous silver powder (D50 = 3 μm) and 24.9 parts of Ni powder (D50 = 2 μm) are added to every 100 parts of resistive paste.

[0124] Example 11:

[0125] The heating element in this embodiment has a resistive paste that is basically the same as that in Example 1, except that: 28.6 parts of NiCr20 alloy powder (D50 = 30 μm), 15 parts of NiCrFe alloy powder (D50 = 20 μm), 2 parts of Cr powder (D50 = 10 μm), 7 parts of amorphous silver powder (D50 = 3 μm) and 24.7 parts of Ni powder (D50 = 2 μm) are added to every 100 parts of resistive paste.

[0126] Example 12:

[0127] The heating element in this embodiment has a resistive paste that is basically the same as that in Example 1, except that: 28.6 parts of NiCr20 alloy powder (D50 = 25 μm), 15 parts of NiCrFe alloy powder (D50 = 25 μm), 3.8 parts of Cr powder (D50 = 10 μm), 7 parts of amorphous silver powder (D50 = 3 μm) and 22.9 parts of Ni powder (D50 = 2 μm) are added to every 100 parts of resistive paste.

[0128] Comparative Example 1:

[0129] The heating element in this embodiment uses a resistive paste that is basically the same as that in Example 4, except that:

[0130] For every 100 parts of resistor paste, add 38.6 parts of NiCr20 alloy powder (D50 = 10 μm), 3.8 parts of Cr powder (D50 = 10 μm), 8 parts of amorphous silver powder (D50 = 5 μm) and 26.9 parts of Ni powder (D50 = 5 μm).

[0131] The sintering temperature is 900℃ and the sintering time is 20min-30min.

[0132] Comparative Example 2:

[0133] The heating element in this embodiment uses a resistive paste that is basically the same as that in Example 4, except that:

[0134] For every 100 parts of resistance paste, add 50 parts of NiCrFe alloy powder (D50 = 20 μm), 3.8 parts of Cr powder (D50 = 10 μm), and 23.5 parts of Ni powder (D50 = 2 μm).

[0135] The sintering temperature is 900℃ and the sintering time is 20min-30min.

[0136] Comparative Example 3:

[0137] The heating element in this embodiment uses a resistive paste that is basically the same as that in Example 4, except that:

[0138] For every 100 parts of resistance paste, add 30 parts of NiCrFe alloy powder (D50 = 20 μm), 5.8 parts of Cr powder (D50 = 10 μm), 15 parts of silver powder (D50 = 3 μm) and 26.5 parts of Ni powder (D50 = 2 μm).

[0139] The sintering temperature is 900℃ and the sintering time is 20min-30min.

[0140] Performance testing:

[0141] The surface of the sintered heating element was observed, and the resistance of the heating element was tested. The test data are shown in Table 1 below.

[0142] Table 1

[0143]

[0144]

[0145] As shown in the table above, in the 12 embodiments, the resistance change rate after 500 suction cycles is less than 3%, and the initial resistance values ​​in all embodiments are less than 1.2Ω, which is also less than the initial resistance values ​​in the comparative examples. This is because silver powder can act as a sintering aid during the sintering process, reducing the sintering temperature and increasing the alloying effect. It can also act as a conductive agent, reducing the resistance of the heating element. Furthermore, after sintering, no brittle fracture or cracking occurred on the surface of the heating element in the above embodiments. This demonstrates that the prepared resistance slurry can reduce the sintering temperature and avoid damaging or blocking the porous structure of the porous ceramic matrix. This prevents excessive cracking of the heating element due to severe shrinkage during high-temperature sintering, without affecting the strength of the porous ceramic itself.

[0146] In the resistance paste of Comparative Example 1, the particle size of the nickel-chromium alloy is similar to that of the chromium powder, nickel powder, and silver powder. This makes it difficult for the silver powder, chromium powder, and nickel powder to fill the gaps between the nickel-chromium alloy particles. During the coating process, the resistance paste flows to both sides of the porous ceramic substrate, making it difficult to ensure the stacking strength of the resistance paste. During the high-temperature sintering process, the resistance paste shrinks and sinks severely, causing cracks to appear on the surface of the heating element.

[0147] The resistive slurry of Comparative Example 2 did not contain silver powder. The same sintering temperature resulted in higher resistance and poorer taste. The resistance change rate was higher during the same power suction test. Some samples of Comparative Example 2 even experienced burn-out.

[0148] The mass ratio of metal powder in the resistivity slurry of Comparative Example 3 was out of range, and the same sintering curve resulted in the heating element having an excessively low initial resistance and failing to function.

[0149] According to the test data of Examples 1 to 12, the use of resistance paste can effectively reduce the sintering temperature, so that the strength of the porous ceramic matrix is ​​not affected after sintering after printing the resistance paste, and the ceramic can be effectively prevented from brittlely cracking. The resistance paste can still meet the resistance value of the heating element at a lower sintering temperature, reduce the initial resistance of the heating element, and improve the service life of the heating element.

[0150] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A resistive paste, characterized in that, The resistive paste comprises an organic carrier and metal powder and glass powder dispersed within the organic carrier; the metal powder comprises silver powder, chromium powder, nickel powder, and nickel-chromium alloy, wherein the average particle size of the nickel-chromium alloy is larger than the average particle size of the silver powder, the chromium powder, or the nickel powder, the average particle size of the chromium powder is larger than the average particle size of the nickel powder, the average particle size of the chromium powder is 10μm~23μm, the average particle size of the silver powder is 0.2μm~3μm, the average particle size of the nickel-chromium alloy is 25μm~38μm, and the average particle size of the nickel powder is 1μm~5μm; Based on the mass of the resistive paste as 100%, the metal powder includes 4%~10% silver powder, 2%~6% chromium powder, 34%~46% nickel-chromium alloy and 20%~30% nickel powder. The nickel-chromium alloy forms a supporting skeleton in the resistive slurry, and the silver powder, chromium powder, and nickel powder fill the gaps between the nickel-chromium alloy particles.

2. The resistive paste according to claim 1, characterized in that, The resistive paste satisfies at least one of the following characteristics: (1) The metal powder also includes at least one of aluminum powder and iron powder; (2) The nickel-chromium alloy includes at least one of NiCr20, NiCr70, NiCr50, and NiCrFe; (3) The shape of the silver powder includes at least one of amorphous, spherical, quasi-spherical and flake-like.

3. The resistive paste according to claim 1, characterized in that, The resistive paste satisfies at least one of the following characteristics: (1) The glass powder is a silicon borosilicate glass powder; (2) The glass powder is a silicon borosilicate glass powder, and the average particle size of the silicon borosilicate glass powder is 10μm~20μm; (3) The glass powder is a silicon borosilicate glass powder, and the melting point of the silicon borosilicate glass powder is 800℃~850℃; (4) The mass ratio of the metal powder, the glass powder and the organic carrier is 100:(5-15):(10-30).

4. The resistive paste according to claim 1, characterized in that, The organic carrier includes an organic solvent, an organic resin, and an organic additive, wherein the mass ratio of the organic solvent to the organic resin to the organic additive is 100:(15-25):(20-50).

5. The resistive paste according to claim 4, characterized in that, The resistive paste satisfies at least one of the following characteristics: (1) The organic solvent includes at least one of ethylene glycol butyl ether, terpineol, diethylene glycol ethyl ether acetate, divalent ester, dodecyl alcohol ester, butyl formate, butyl carbitol and butyl carbitol acetate; (2) The organic additives include thixotropic agents and dispersants; (3) The organic additives include thixotropic agents and dispersants, wherein the thixotropic agents include at least one of organic bentonite, hydrogenated castor oil and polyamide wax; (4) The organic additives include thixotropic agents and dispersants, wherein the dispersant includes at least one of polyacrylamide, cellulose derivatives and acrylic acid; (5) The organic resin includes at least one of acrylic resin and cellulose resin; (6) The organic additive also includes a coupling agent, which includes at least one of silane coupling agents, bimetallic coupling agents and chromium complexes.

6. A heating element, characterized in that, The heating element comprises a porous ceramic substrate and a heating film layer formed on the porous ceramic substrate; the heating film layer is formed from the resistive paste as described in any one of claims 1 to 5.

7. The heating element according to claim 6, characterized in that, The heating element satisfies at least one of the following characteristics: (1) The thickness of the heating film layer is 70μm~100μm; (2) The width of the heating film layer is 3.5μm~4.5μm; (3) The porous ceramic matrix is ​​a diatomite and montmorillonite mixed ceramic; (4) The porosity of the porous ceramic matrix is ​​55%~60%, and the oil conduction rate of the porous ceramic matrix is ​​1.3μl / s~2.5μl / s.

8. A method for preparing a heating element, characterized in that, The method includes the following steps: A resistive paste is printed on the surface of a porous ceramic substrate, dried, and then sintered at 850℃~950℃ for 20min~30min to obtain a heating element, wherein the resistive paste is the resistive paste as described in any one of claims 1 to 5.

9. An aerosol generating device, characterized in that, Includes the heating element as described in claim 6.

Citation Information

Patent Citations

  • Electric heating resistance paste as well as preparation method and application thereof

    CN112670009A

  • Metal slurry, heating circuit, atomizing core, preparation method of atomizing core, and electronic cigarette