A denitration catalyst regeneration powder and its preparation method and application
By preparing a denitrification catalyst regeneration powder containing specific main active and secondary active components and contacting the spent denitrification catalyst in the flue, the problem of long regeneration treatment time of the spent denitrification catalyst is solved, and efficient denitrification activity recovery and economic benefits are achieved.
Patent Information
- Application Number
- CN202311222919.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-21
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-09-21
AI Technical Summary
The offline regeneration of spent denitrification catalysts in the existing technology takes a long time and cannot be matched with the short maintenance period of coal-fired power plants, resulting in the inability to effectively restore denitrification activity.
Provides a denitrification catalyst regeneration powder containing main active components (vanadium pentoxide, tungsten trioxide and molybdenum trioxide) and secondary active components (cerium oxide, etc.), which can be utilized by online contact with the spent denitrification catalyst in the flue. The compound components and carrier (such as titanium dioxide) are calcined and pulverized to form a regeneration powder that can effectively restore denitrification activity.
It significantly shortens the regeneration treatment cycle of spent denitration catalysts, improves the recovery rate of denitration activity, reduces production costs and energy consumption, and has huge economic and social benefits.
Smart Images

Figure BDA0004461263430000161
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material synthesis and preparation, and in particular to a denitration catalyst regeneration powder, a preparation method and application thereof. Background Art
[0002] Selective catalytic reduction (SCR) denitrification technology is an efficient, reliable and mature flue gas denitrification technology, which is widely used in coal-fired flue gas denitrification systems in my country. Denitrification catalyst is a key component of this technology. Since the implementation of denitrification of coal-fired flue gas in thermal power and non-power industries in my country, millions of tons of denitrification catalysts have been put into use. During the long-term operation, the denitrification catalyst gradually loses its denitrification activity due to the long-term erosion and accumulation of poisonous elements such as alkali metals, alkaline earth metals, heavy metals and arsenic in the flue gas, and becomes an inactivated waste denitrification catalyst.
[0003] At present, my country has listed deactivated waste denitrification catalysts as hazardous waste. In order to restore the denitrification activity of deactivated waste denitrification catalysts, they need to be regenerated offline by companies with professional regeneration technology qualifications. The offline regeneration process of waste denitrification catalysts includes: handling of five hazardous waste transfer forms, disassembly of waste denitrification catalysts from coal-fired power plants, transfer and transportation to regeneration plants, regeneration treatment, transportation to coal-fired power plants, and installation of regenerated denitrification catalysts. The offline regeneration process of waste denitrification catalysts is time-consuming and cannot be well matched with the shorter maintenance period of coal-fired power plants. Summary of the invention
[0004] The purpose of the present invention is to overcome the problem that the existing technology mainly adopts an offline method to regenerate the waste denitration catalyst, but the offline regeneration process is time-consuming and cannot be well matched with the short maintenance period of coal-fired power plants, and to provide a denitration catalyst regeneration powder and its preparation method and application. The regeneration powder provided by the present invention can be directly introduced into the flue to contact the waste denitration catalyst in the flue for online regeneration, which greatly shortens the regeneration process cycle of the waste denitration catalyst and can bring significant economic and social benefits.
[0005] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a denitrification catalyst regeneration powder, which contains a main active component, a secondary active component and a carrier; the main active component is selected from at least two of vanadium pentoxide, tungsten trioxide and molybdenum trioxide; the secondary active component is selected from at least two of cerium oxide, copper oxide, manganese oxide, iron oxide, antimony oxide, niobium oxide, cobalt oxide, nickel oxide, zinc oxide and tin oxide.
[0006] Preferably, based on the total weight of the denitration catalyst regeneration powder, the content of the main active component is 2-50% by weight, the content of the secondary active component is 1-20% by weight, and the content of the carrier is 30-97% by weight.
[0007] Preferably, the particle size of the denitration catalyst regeneration powder is 15-74 um.
[0008] Preferably, the carrier is selected from one or more of titanium dioxide, glass fiber, aluminum oxide, zirconium dioxide, silicon dioxide and calcium oxide.
[0009] A second aspect of the present invention provides a method for preparing a denitration catalyst regeneration powder, the method comprising the following steps:
[0010] (1) preparing a main active component precursor and a side active component precursor into a main active component solution and a side active component solution respectively;
[0011] (2) mixing the carrier, the surfactant and water to obtain a mixture;
[0012] (3) mixing the mixture obtained in step (2), the main active component solution, the secondary active component solution and the adhesive, forming, calcining and pulverizing;
[0013] Wherein, the main active component precursor is selected from at least two of ammonium metavanadate, ammonium metatungstate and ammonium heptamolybdate;
[0014] The secondary active component precursor is selected from at least two of cerium salts, copper salts, manganese salts, iron salts, antimony salts, niobium salts, cobalt salts, nickel salts, zinc salts and tin salts.
[0015] Preferably, the method for preparing the main active component solution in step (1) comprises: mixing the main active component precursor with an aqueous solution of a co-solvent.
[0016] Preferably, the weight ratio of the main active component precursor to the auxiliary solvent aqueous solution is 0.1-5:1, more preferably 1-1.5:1; the concentration of the auxiliary solvent aqueous solution is 0.05-0.5 g / mL.
[0017] Preferably, the co-solvent is selected from one or more of oxalic acid, sulfuric acid and ethanolamine.
[0018] Preferably, the method for preparing the secondary active component solution in step (1) comprises: mixing the secondary active component precursor with water.
[0019] Preferably, the dosage ratio of the secondary active component precursor to water is 1 g: 4-10 mL.
[0020] Preferably, in step (2), the ratio of the carrier, surfactant and water is 10-1000 g: 1 g: 30-500 mL.
[0021] Preferably, the carrier is selected from one or more of titanium dioxide, glass fiber, aluminum oxide, zirconium dioxide, silicon dioxide and calcium oxide.
[0022] Preferably, the weight ratio of the main active component precursor, the secondary active component precursor, the carrier and the adhesive is 2-20:1-10:10-200:1.
[0023] Preferably, the surfactant is selected from one or more of palmitic acid, oleic acid, vaseline and paraffin.
[0024] Preferably, in step (2), the mixing conditions include: temperature of 70-90° C. and time of 30-100 min.
[0025] Preferably, in step (3), the mixing conditions include: temperature of 70-90° C. and time of 30-100 min.
[0026] Preferably, in step (3), the calcination conditions include: temperature of 300-550° C. and time of 4-8 h.
[0027] Preferably, in step (3), the adhesive is selected from one or more of cellulose ester, polyvinyl alcohol, epoxy resin and polyacrylate.
[0028] The third aspect of the present invention provides a denitration catalyst regeneration powder prepared by the method described above.
[0029] A fourth aspect of the present invention provides a method for regenerating a spent denitration catalyst, the method comprising: mixing a denitration catalyst regeneration powder with a gas, contacting the denitration catalyst with the spent denitration catalyst in a flue for regeneration; the denitration catalyst regeneration powder is the denitration catalyst regeneration powder described above.
[0030] Preferably, the regeneration conditions include: temperature of 20-380°C and time of 0.5-5h.
[0031] Preferably, the usage ratio of the denitration catalyst regeneration powder to the waste denitration catalyst is 0.005-0.1:1.
[0032] Through the above technical solution, the beneficial effects of the present invention are mainly:
[0033] (1) The denitration catalyst regeneration powder prepared by the present invention contains both a specific compounded main active component and a specific compounded secondary active component. The denitration catalyst regeneration powder having the specific properties can well restore the activity of the waste denitration catalyst in the process of regenerating the waste denitration catalyst in the flue. In a preferred case, the particle size of the prepared denitration catalyst regeneration powder is controlled within a specific range, which can further improve the online regeneration effect of the waste denitration catalyst.
[0034] (2) The present invention obtains a denitration catalyst regeneration powder by mixing a specific main active component solution and a specific secondary active component solution with a carrier, extruding and molding, calcining, and crushing. The prepared denitration catalyst regeneration powder flushes and rubs the surface of the waste denitration catalyst, and the higher concentration of main active component chemical bonds (AO, where A is the main active component element atom) such as vanadium, tungsten, and molybdenum on the surface of the regeneration powder are in friction contact with poisoning elements such as alkali metals, alkaline earth metals, heavy metals, and arsenic on the surface of the waste denitration catalyst to produce a chemical reaction similar to ion exchange, thereby breaking the original poisoning element valence bond (MOA, where M is the poisoning element atom) and forming a new poisoning element valence bond (AOM), thereby removing the poisoning element on the surface of the waste denitration catalyst.
[0035] (3) Under preferred conditions, the denitration catalyst regeneration powder is prepared by using the spent denitration catalyst regeneration titanium dioxide as a carrier, which can fully absorb the spent denitration catalyst regeneration titanium dioxide.
[0036] (4) The preparation method of the denitration catalyst regeneration powder described in the present invention has a simple process, low energy consumption, and low production cost. It can realize the online activity recovery of the denitration catalyst and greatly shorten the regeneration treatment cycle of the waste denitration catalyst. It can bring significant economic and social benefits and has great promotion and application value. DETAILED DESCRIPTION
[0037] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0038] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0039] A first aspect of the present invention provides a denitrification catalyst regeneration powder, which contains a main active component, a secondary active component and a carrier; the main active component is selected from at least two of vanadium pentoxide, tungsten trioxide and molybdenum trioxide; the secondary active component is selected from at least two of cerium oxide, copper oxide, manganese oxide, iron oxide, antimony oxide, niobium oxide, cobalt oxide, nickel oxide, zinc oxide and tin oxide.
[0040] In the present invention, the main active component and the secondary active component of specific ingredients are compounded and used to form a new composite component for fusion and sorting, which is beneficial for the main active component to be dispersed in the carrier more evenly and orderly. At the same time, the performance of the composite component in removing poisoning elements is richer and more comprehensive, thereby improving the online regeneration effect of the regeneration powder on the waste denitrification catalyst.
[0041] In a preferred embodiment, the main active component is a combination of vanadium pentoxide, tungsten trioxide and molybdenum trioxide. In the present invention, the main active component is a combination of vanadium pentoxide, tungsten trioxide and molybdenum trioxide, which can significantly improve the removal rate of alkali metals, alkaline earth metals, heavy metals and arsenic, and significantly improve the denitration activity of the regenerated denitration catalyst.
[0042] In the present invention, the content of the main active component and the content of the secondary active component have a great influence on the online regeneration effect of the waste denitration catalyst. In some preferred embodiments, based on the total weight of the denitration catalyst regeneration powder, the content of the main active component is 2-50% by weight, the content of the secondary active component is 1-20% by weight, and the content of the carrier is 30-97% by weight.
[0043] In the present invention, in order to effectively remove poisoning elements such as alkali metals, alkaline earth metals, heavy metals and arsenic on the surface of the waste denitration catalyst, the particle size of the denitration catalyst regeneration powder can be controlled within a specific range. In a preferred embodiment, the particle size of the denitration catalyst regeneration powder is 15-74 μm.
[0044] In the present invention, the carrier may be a conventional choice in the art. Specifically, the carrier may be selected from one or more of titanium dioxide, glass fiber, aluminum oxide, zirconium dioxide, silicon dioxide and calcium oxide.
[0045] The titanium dioxide may be titanium dioxide regenerated from waste denitration catalyst and / or conventional titanium dioxide. In order to realize waste utilization and dispose of titanium dioxide regenerated from waste denitration catalyst, the titanium dioxide is preferably titanium dioxide regenerated from waste denitration catalyst.
[0046] A second aspect of the present invention provides a method for preparing a denitration catalyst regeneration powder, the method comprising the following steps:
[0047] (1) preparing a main active component precursor and a side active component precursor into a main active component solution and a side active component solution respectively;
[0048] (2) mixing the carrier, the surfactant and water to obtain a mixture;
[0049] (3) The mixture obtained in step (2), the main active component solution, the secondary active component solution and the adhesive are mixed, molded, calcined and crushed.
[0050] Among them, the main active component precursor is selected from at least two of ammonium metavanadate, ammonium metatungstate and ammonium heptamolybdate; the secondary active component precursor is selected from at least two of cerium salts, copper salts, manganese salts, iron salts, antimony salts, niobium salts, cobalt salts, nickel salts, zinc salts and tin salts.
[0051] In the present invention, in order to further improve the online regeneration effect of the prepared regeneration powder on the spent denitration catalyst, in a preferred case, the main active component precursor is a combination of ammonium metavanadate, ammonium metatungstate and ammonium heptamolybdate.
[0052] In the method described in the present invention, the main active component solution, the secondary active component solution and the carrier are mixed, extruded, calcined and crushed to obtain the denitration catalyst regeneration powder, wherein the main active component solution and the secondary active component solution are obtained by compounding the main active component precursor and the secondary active component precursor. The main active component solution and the secondary active component solution are used together, which is beneficial to uniformly disperse the main active component in the carrier. The denitration catalyst regeneration powder obtained by this method can effectively restore the activity of the waste denitration catalyst.
[0053] In the method of the present invention, the method for preparing the main active component solution can be a conventional choice in the art. Specifically, the method for preparing the main active component solution in step (1) comprises: mixing the main active component precursor with a co-solvent aqueous solution, wherein the co-solvent aqueous solution helps to promote the dissolution of the main active component precursor.
[0054] In a preferred embodiment, the co-solvent is selected from one or more of oxalic acid, sulfuric acid and ethanolamine.
[0055] In a preferred embodiment, the weight ratio of the main active component precursor to the co-solvent aqueous solution is 0.1-5:1, and the concentration of the co-solvent aqueous solution is 0.05-0.5 g / mL. In a more preferred embodiment, the weight ratio of the main active component precursor to the co-solvent aqueous solution is 1-1.5:1, for example, 1:1, 1.19:1 or 1.37:1.
[0056] In a preferred embodiment, the mixing of the main active component precursor and the auxiliary solvent aqueous solution can be carried out under heating and stirring conditions. Specifically, the mixing conditions include: a temperature of 20-96° C. and a time of 30-100 min.
[0057] In the method of the present invention, the method for preparing the secondary active component solution can be a conventional choice in the art. Specifically, the method for preparing the secondary active component solution in step (1) comprises: mixing the secondary active component precursor with water.
[0058] In a preferred embodiment, the dosage ratio of the secondary active component precursor to water is 1 g:4-10 mL, for example, 1 g:1 mL, 1 g:5 mL, 1 g:8.3 mL or 1 g:10 mL.
[0059] In the method described in the present invention, in a preferred embodiment, in step (2), the usage ratio of the carrier, surfactant and water is 10-1000g:1g:30-500mL, for example, 10g:1g:30mL, 11.3g:1g:33.3mL, 34.5g:1g:30mL, 970g:1g:500mL, 1000g:1g:500mL.
[0060] In the present invention, the carrier can be a conventional choice in the art, specifically, the carrier can be selected from one or more of titanium dioxide, glass fiber, aluminum oxide, zirconium dioxide, silicon dioxide and calcium oxide. Preferably, the diameter of the glass fiber is 5-20 um.
[0061] The titanium dioxide may be titanium dioxide regenerated from waste denitration catalyst and / or conventional titanium dioxide. In order to realize waste utilization and dispose of titanium dioxide regenerated from waste denitration catalyst, the titanium dioxide is preferably titanium dioxide regenerated from waste denitration catalyst.
[0062] In a specific embodiment, when the carrier is selected from one substance, step (2) comprises: mixing the carrier, a surfactant and water to obtain a mixture; when the carrier is selected from two different substances, in order to ensure uniform dispersion of the carrier, the two different carriers are added in steps, and step (2) comprises: mixing the first carrier, a surfactant and water, and then adding the second carrier to mix to obtain a mixture.
[0063] In the present invention, the mixing process in step (2) can be carried out in a kneader; the process of mixing the mixture obtained in step (2), the main active component solution, the secondary active component solution and the adhesive in step (3) can also be carried out in a kneader.
[0064] In a preferred embodiment, in step (2), the mixing conditions include: temperature of 70-90° C. and time of 30-100 min.
[0065] In a preferred embodiment, in step (3), the mixing conditions include: temperature of 70-90° C. and time of 30-100 min.
[0066] In a preferred embodiment, the weight ratio of the main active component precursor, the secondary active component precursor, the carrier and the adhesive is 2-20:1-10:10-200:1, for example, 2:1:10:1, 2.68:2:194:1, 14.88:3:34.5:1, 19.8:5.3:11.3:1, 8.53:3:34.5:1 or 20:10:200:1.
[0067] In the present invention, the surfactant can be a conventional choice of those skilled in the art. In a preferred embodiment, the surfactant is selected from one or more of palmitic acid, oleic acid, vaseline and paraffin.
[0068] In the present invention, the adhesive can be a conventional choice of those skilled in the art. In a preferred embodiment, the adhesive is selected from one or more of cellulose ester, polyvinyl alcohol, epoxy resin and polyacrylate.
[0069] In a preferred embodiment, the calcination conditions in step (3) include: a temperature of 300-550°C, for example, 300°C, 350°C, 400°C, 425°C, 450°C, 500°C or 550°C; and a time of 4-8h, for example, 4h, 5h, 6h, 6.5h, 7h, 7.5h or 8h.
[0070] The third aspect of the present invention provides a denitration catalyst regeneration powder prepared by the method described above.
[0071] In a preferred embodiment, the denitration catalyst regeneration powder contains a main active component, a secondary active component and a carrier; the main active component is selected from at least two of vanadium pentoxide, tungsten trioxide and molybdenum trioxide; the secondary active component is selected from at least two of oxides, copper oxides, manganese oxides, iron oxides, antimony oxides, niobium oxides, cobalt oxides, nickel oxides, zinc oxides and tin oxides. The denitration catalyst regeneration powder can effectively restore the activity of the spent denitration catalyst.
[0072] A fourth aspect of the present invention provides a method for regenerating a spent denitration catalyst, the method comprising: mixing a denitration catalyst regeneration powder with a gas, contacting the denitration catalyst with the spent denitration catalyst in a flue for regeneration; the denitration catalyst regeneration powder is the denitration catalyst regeneration powder described above.
[0073] In a preferred embodiment, the gas is flue gas or compressed air.
[0074] In the regeneration method described in the present invention, when the denitration system is in operation, the prepared denitration catalyst regeneration powder is mixed with the flue gas in the flue, flushes and rubs the surface of the waste denitration catalyst in the flue, and forms metal bonds with the alkali metals, alkaline earth metals, heavy metals, arsenic and other poisoning elements on the surface of the waste denitration catalyst, thereby removing the poisoning elements on the surface of the waste denitration catalyst, and then restoring the denitration activity of the waste denitration catalyst; when the denitration system is shut down, compressed air can be used to mix with the denitration catalyst regeneration powder, and then flush the surface of the waste denitration catalyst, remove the alkali metals, alkaline earth metals, heavy metals, arsenic and other poisoning elements on the surface of the waste denitration catalyst, and restore the denitration activity of the waste denitration catalyst.
[0075] In a specific embodiment, the regeneration conditions include: temperature is room temperature (about 20°C)-flue gas temperature (about 380°C), and time is 0.5-5h.
[0076] In a preferred embodiment, the weight ratio of the denitration catalyst regeneration powder to the spent denitration catalyst is 0.001-0.05:1.
[0077] The present invention will be described in detail below by way of examples. Unless otherwise specified, all methods are conventional in the art. The experimental materials used in the following examples, unless otherwise specified, can be purchased from reagent suppliers.
[0078] Example 1
[0079] (1) Preparation of the main active component solution: 1.27 g of ammonium metavanadate, 1.07 g of ammonium metatungstate and 0.98 g of oxalic acid aqueous solution were mixed and stirred at room temperature (20° C.) for 30 min to dissolve; the concentration of the oxalic acid aqueous solution was 0.05 g / mL;
[0080] Preparation of the secondary active component solution: 0.25 g of cerium nitrate, 0.25 g of copper sulfate, 0.25 g of manganese sulfate and 0.25 g of ferrous acetate were mixed and dissolved in 10 mL of deionized water;
[0081] (2) 87 g of spent denitration catalyst regenerated titanium dioxide, 0.1 g of palmitic acid and 50 mL of deionized water were placed in a kneader and stirred at a constant temperature of 70° C. for 30 min, and then 10 g of glass fiber (5-20 um) was added and stirred for another 30 min to obtain a mixture;
[0082] (3) The mixture obtained in step (2), the main active component solution and the secondary active component solution prepared in step (1) and 0.5 g of cellulose ester are placed in a kneader and stirred at a constant temperature of 70° C. for 30 min to obtain a granular product, which is then extruded into strips on an extruder, followed by calcination at 300° C. for 4 h, and the calcined product is crushed to 74 μm to obtain a denitration catalyst regeneration powder.
[0083] Example 2
[0084] (1) Preparation of the main active component solution: 6.35 g of ammonium metavanadate, 10.7 g of ammonium metatungstate, 12.7 g of ammonium heptamolybdate, 25 g of oxalic acid aqueous solution and 5 g of sulfuric acid aqueous solution were mixed and dissolved at 50° C. for 50 min; the concentrations of the oxalic acid aqueous solution and the sulfuric acid aqueous solution were both 0.3 g / mL;
[0085] Preparation of the secondary active component solution: 1 g of cerium nitrate, 1 g of copper sulfate, 1 g of manganese sulfate, 1 g of ferrous acetate, 1 g of antimony nitrate and 1 g of niobium oxalate were mixed and dissolved in 50 mL of deionized water;
[0086] (2) 63 g of spent denitration catalyst regenerated titanium dioxide, 2 g of palmitic acid and 60 mL of deionized water were placed in a kneader and stirred at a constant temperature of 80° C. for 50 min, and then 6 g of glass fiber (5-20 μm) was added and stirred for 50 min to obtain a mixture;
[0087] (3) The mixture obtained in step (2), the main active component solution and the secondary active component solution prepared in step (1) and 2 g of cellulose ester are placed in a kneader and stirred at a constant temperature of 80° C. for 50 min to obtain a granular product, which is then extruded into strips on an extruder, and then calcined at 450° C. for 6 h. The calcined product is crushed to 25 μm to obtain a denitration catalyst regeneration powder.
[0088] Example 3
[0089] (1) Preparation of the main active component solution: 12.7 g of ammonium metavanadate, 21.4 g of ammonium metatungstate, 25.4 g of ammonium heptamolybdate and 50 g of an aqueous solution of ethanolamine were mixed and dissolved at 96° C. with stirring for 80 min; the concentration of the aqueous solution of ethanolamine was 0.5 g / mL;
[0090] Preparation of the secondary active component solution: 2 g of cerium nitrate, 2 g of copper sulfate, 2 g of manganese sulfate, 2 g of ferrous acetate, 2 g of antimony nitrate, 2 g of niobium oxalate, 2 g of cobalt sulfate and 2 g of nickel nitrate were mixed and dissolved in 80 mL of deionized water;
[0091] (2) 30 g of spent denitration catalyst regenerated titanium dioxide, 3 g of palmitic acid and 100 mL of deionized water were placed in a kneader and stirred at a constant temperature of 90° C. for 60 min, and then 4 g of glass fiber (5-20 um) was added and stirred for 80 min to obtain a mixture;
[0092] (3) The mixture obtained in step (2), the main active component solution and the secondary active component solution prepared in step (1) and 3 g of cellulose ester are placed in a kneader and stirred at a constant temperature of 90° C. for 80 min to obtain a granular product, which is then extruded into strips on an extruder, followed by calcination at 550° C. for 8 h, and the calcined product is crushed to 15 μm to obtain a denitration catalyst regeneration powder.
[0093] Example 4
[0094] The method of Example 1 is followed, except that only one carrier is selected, namely, titanium dioxide regenerated from the spent denitration catalyst. The specific method is as follows:
[0095] (1) Preparation of the main active component solution: 1.27 g of ammonium metavanadate, 1.07 g of ammonium metatungstate and 0.98 g of oxalic acid aqueous solution were mixed and stirred at room temperature (20° C.) for 30 min to dissolve; the concentration of the oxalic acid aqueous solution was 0.05 g / mL;
[0096] Preparation of the secondary active component solution: 0.25 g of cerium nitrate, 0.25 g of copper sulfate, 0.25 g of manganese sulfate and 0.25 g of ferrous acetate were mixed and dissolved in 10 mL of deionized water;
[0097] (2) 97 g of spent denitration catalyst regenerated titanium dioxide, 0.1 g of palmitic acid and 50 mL of deionized water were placed in a kneader and stirred at a constant temperature of 70° C. for 30 min to obtain a mixture;
[0098] (3) The mixture obtained in step (2), the main active component solution and the secondary active component solution prepared in step (1) and 0.5 g of cellulose ester are placed in a kneader and stirred at a constant temperature of 70° C. for 30 min to obtain a granular product, which is then extruded into strips on an extruder, followed by calcination at 300° C. for 4 h, and the calcined product is crushed to 74 μm to obtain a denitration catalyst regeneration powder.
[0099] Example 5
[0100] The method of Example 1 is used for implementation, except that only one carrier is selected, namely glass fiber. The specific method is as follows:
[0101] (1) Preparation of the main active component solution: 1.27 g of ammonium metavanadate, 1.07 g of ammonium metatungstate and 0.98 g of oxalic acid aqueous solution were mixed and stirred at room temperature (20° C.) for 30 min to dissolve; the concentration of the oxalic acid aqueous solution was 0.05 g / mL;
[0102] Preparation of the secondary active component solution: 0.25 g of cerium nitrate, 0.25 g of copper sulfate, 0.25 g of manganese sulfate and 0.25 g of ferrous acetate were mixed and dissolved in 10 mL of deionized water;
[0103] (2) placing 97 g of glass fiber (5-20 μm), 0.1 g of palmitic acid and 50 mL of deionized water in a kneader and stirring at a constant temperature of 70° C. for 30 min to obtain a mixture;
[0104] (3) The mixture obtained in step (2), the main active component solution and the secondary active component solution prepared in step (1) and 0.5 g of cellulose ester are placed in a kneader and stirred at a constant temperature of 70° C. for 30 min to obtain a granular product, which is then extruded into strips on an extruder, followed by calcination at 300° C. for 4 h, and the combustion product is crushed to 74 μm to obtain a denitration catalyst regeneration powder.
[0105] Example 6
[0106] The method of Example 2 is used for implementation, except that in the preparation process of the main active component solution, the main active component precursors only use ammonium metavanadate and ammonium metatungstate. The specific method is as follows:
[0107] (1) Preparation of the main active component solution: 6.35 g of ammonium metavanadate, 10.7 g of ammonium metatungstate, 25 g of oxalic acid aqueous solution and 5 g of sulfuric acid aqueous solution were mixed and dissolved at 50° C. with stirring for 50 min; the concentration of the oxalic acid aqueous solution was 0.3 g / mL, and the concentration of the sulfuric acid aqueous solution was 0.3 g / mL;
[0108] Preparation of the secondary active component solution: 1 g of cerium nitrate, 1 g of copper sulfate, 1 g of manganese sulfate, 1 g of ferrous acetate, 1 g of antimony nitrate and 1 g of niobium oxalate were mixed and dissolved in 50 mL of deionized water;
[0109] (2) 63 g of spent denitration catalyst regenerated titanium dioxide, 2 g of palmitic acid and 60 mL of deionized water were placed in a kneader and stirred at a constant temperature of 80° C. for 50 min, and then 6 g of glass fiber (5-20 μm) was added and stirred for 50 min to obtain a mixture;
[0110] (3) The mixture obtained in step (2), the main active component solution and the secondary active component solution prepared in step (1) and 2 g of cellulose ester are placed in a kneader and stirred at a constant temperature of 80° C. for 50 min to obtain a granular product, which is then extruded into strips on an extruder, and then calcined at 450° C. for 6 h. The calcined product is crushed to 25 μm to obtain a denitration catalyst regeneration powder.
[0111] Comparative Example 1
[0112] The method of Example 1 is used for implementation, except that there is only one main active component precursor for preparing the main active component solution, namely ammonium metavanadate. The specific method is as follows:
[0113] (1) Preparation of the main active component solution: 1.27 g of ammonium metavanadate and 0.98 g of oxalic acid aqueous solution were mixed and stirred at room temperature (20° C.) for 30 min to dissolve; the concentration of the oxalic acid aqueous solution was 0.05 g / mL;
[0114] Preparation of the secondary active component solution: 0.25 g of cerium nitrate, 0.25 g of copper sulfate, 0.25 g of manganese sulfate and 0.25 g of ferrous acetate were mixed and dissolved in 10 mL of deionized water;
[0115] (2) 87 g of spent denitration catalyst regenerated titanium dioxide, 0.1 g of palmitic acid and 50 mL of deionized water were placed in a kneader and stirred at a constant temperature of 70° C. for 30 min, and then 10 g of glass fiber (5-20 um) was added and stirred for another 30 min to obtain a mixture;
[0116] (3) The mixture obtained in step (2), the main active component solution and the secondary active component solution prepared in step (1) and 0.5 g of cellulose ester are placed in a kneader and stirred at a constant temperature of 70° C. for 30 min to obtain a granular product, which is then extruded into strips on an extruder, followed by calcination at 300° C. for 4 h, and the combustion product is crushed to 74 μm to obtain a denitration catalyst regeneration powder.
[0117] Comparative Example 2
[0118] The method of Example 1 is followed, except that there is only one precursor of the secondary active component for preparing the secondary active component solution. The specific method is as follows:
[0119] (1) Preparation of the main active component solution: 1.27 g of ammonium metavanadate, 1.07 g of ammonium metatungstate and 0.98 g of oxalic acid aqueous solution were mixed and stirred at room temperature (20° C.) for 30 min to dissolve; the concentration of the oxalic acid aqueous solution was 0.05 g / mL;
[0120] Preparation of the secondary active component solution: Dissolve 0.25 g of cerium nitrate in 10 mL of deionized water;
[0121] (2) 87 g of spent denitration catalyst regenerated titanium dioxide, 0.1 g of palmitic acid and 50 mL of deionized water were placed in a kneader and stirred at a constant temperature of 70° C. for 30 min, and then 10 g of glass fiber (5-20 um) was added and stirred for another 30 min to obtain a mixture;
[0122] (3) The mixture obtained in step (2), the main active component solution and the secondary active component solution prepared in step (1) and 0.5 g of cellulose ester are placed in a kneader and stirred at a constant temperature of 70° C. for 30 min to obtain a granular product, which is then extruded into strips on an extruder, followed by calcination at 300° C. for 4 h, and the combustion product is crushed to 74 μm to obtain a denitration catalyst regeneration powder.
[0123] Comparative Example 3
[0124] The method of Example 1 is used for implementation, except that only one kind of main active component precursor and one kind of secondary active component precursor are used for preparing the main active component solution and the secondary active component solution. The specific method is as follows:
[0125] (1) Preparation of the main active component solution: 1.27 g of ammonium metavanadate and 0.98 g of oxalic acid aqueous solution were mixed and stirred at room temperature (20° C.) for 30 min to dissolve; the concentration of the oxalic acid aqueous solution was 0.05 g / mL;
[0126] Preparation of the secondary active component solution: Dissolve 0.25 g of cerium nitrate in 10 mL of deionized water;
[0127] (2) 87 g of spent denitration catalyst regenerated titanium dioxide, 0.1 g of palmitic acid and 50 mL of deionized water were placed in a kneader and stirred at a constant temperature of 70° C. for 30 min, and then 10 g of glass fiber (5-20 um) was added and stirred for another 30 min to obtain a mixture;
[0128] (3) The mixture obtained in step (2), the main active component solution and the secondary active component solution prepared in step (1) and 0.5 g of cellulose ester are placed in a kneader and stirred at a constant temperature of 70° C. for 30 min to obtain a granular product, which is then extruded into strips on an extruder, followed by calcination at 300° C. for 4 h, and the combustion product is crushed to 74 μm to obtain a denitration catalyst regeneration powder.
[0129] Comparative Example 4
[0130] The method of Example 2 is followed, except that in step (1), ammonium metavanadate is replaced by aluminum sulfate. The specific method is as follows:
[0131] (1) Preparation of the main active component solution: 6.35 g of aluminum sulfate, 10.7 g of ammonium metatungstate, 12.7 g of ammonium heptamolybdate, 25 g of oxalic acid aqueous solution and 5 g of sulfuric acid aqueous solution were mixed and dissolved at 50° C. for 50 min; the concentrations of the oxalic acid aqueous solution and the sulfuric acid aqueous solution were both 0.3 g / mL;
[0132] Preparation of the secondary active component solution: 1 g of cerium nitrate, 1 g of copper sulfate, 1 g of manganese sulfate, 1 g of ferrous acetate, 1 g of antimony nitrate and 1 g of niobium oxalate were mixed and dissolved in 50 mL of deionized water;
[0133] (2) 63 g of spent denitration catalyst regenerated titanium dioxide, 2 g of palmitic acid and 60 mL of deionized water were placed in a kneader and stirred at a constant temperature of 80° C. for 50 min, and then 6 g of glass fiber (5-20 μm) was added and stirred for 50 min to obtain a mixture;
[0134] (3) The mixture obtained in step (2), the main active component solution and the secondary active component solution prepared in step (1) and 2 g of cellulose ester are placed in a kneader and stirred at a constant temperature of 80° C. for 50 min to obtain a granular product, which is then extruded into strips on an extruder, and then calcined at 450° C. for 6 h. The calcined product is crushed to 25 μm to obtain a denitration catalyst regeneration powder.
[0135] Test Example 1
[0136] 10g of the denitration catalyst regeneration powder obtained in Examples 1-6 and Comparative Examples 1-4 was mixed with compressed air, and then the surface of 100g of the used denitration catalyst was flushed, and the cycle was repeated 10 times at a temperature of 20°C for 0.5h. The removal of poisoning elements such as alkali metals, alkaline earth metals, heavy metals, arsenic, etc. on the surface of the waste denitration catalyst was determined, and the denitration activity K value of the waste denitration catalyst before and after treatment was determined.
[0137] Table 1
[0138]
[0139] It can be seen from the results in Table 1 that, compared with the comparative example, the denitration catalyst regeneration powder prepared by the method of the present invention has a higher removal rate of poisoning elements, and can effectively remove poisoning elements such as alkali metals, alkaline earth metals, heavy metals, arsenic, etc. on the surface of the waste denitration catalyst; and can well restore the activity of the waste denitration catalyst.
[0140] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for regenerating a spent denitration catalyst, It is characterized in that The method comprises: mixing denitration catalyst regeneration powder with gas, and contacting the denitration catalyst in the flue to regenerate the denitration catalyst; The denitration catalyst regeneration powder contains a main active component, a secondary active component and a carrier; The main active component is selected from a combination of at least one of tungsten trioxide and molybdenum trioxide and vanadium pentoxide; The secondary active components are selected from at least two of cerium oxide, copper oxide, manganese oxide, iron oxide, antimony oxide, niobium oxide, cobalt oxide, nickel oxide, zinc oxide and tin oxide; Based on the total weight of the denitration catalyst regeneration powder, the content of the main active component is 2-50% by weight, the content of the secondary active component is 1-20% by weight, and the content of the carrier is 30-97% by weight.
2. The method according to claim 1, It is characterized in that The particle size of the denitration catalyst regeneration powder is 15-74 um.
3. The method according to claim 2, It is characterized in that The carrier is selected from one or more of titanium dioxide, glass fiber, aluminum oxide, zirconium dioxide, silicon dioxide and calcium oxide.
4. The method according to claim 1, It is characterized in that The preparation method of the denitration catalyst regeneration powder comprises the following steps: (1) preparing a main active component precursor and a side active component precursor into a main active component solution and a side active component solution respectively; (2) mixing the carrier, the surfactant and water to obtain a mixture; (3) mixing the mixture obtained in step (2), the main active component solution, the secondary active component solution and the adhesive, forming, calcining and crushing; Wherein, the main active component precursor is selected from a combination of at least one of ammonium metatungstate and ammonium heptamolybdate and ammonium metavanadate; The secondary active component precursor is selected from at least two of cerium salts, copper salts, manganese salts, iron salts, antimony salts, niobium salts, cobalt salts, nickel salts, zinc salts and tin salts.
5. The method according to claim 4, It is characterized in that The method for preparing the main active component solution in step (1) comprises: mixing the main active component precursor with an aqueous solution of a co-solvent.
6. The method according to claim 5, It is characterized in that The weight ratio of the main active component precursor to the auxiliary solvent aqueous solution is 0.1-5:1; the concentration of the auxiliary solvent aqueous solution is 0.05-0.5 g / mL.
7. The method according to claim 6, It is characterized in that The weight ratio of the main active component precursor to the auxiliary solvent aqueous solution is 1-1.5:
1.
8. The method according to claim 5 or 6, It is characterized in that The co-solvent is selected from one or more of oxalic acid, sulfuric acid and ethanolamine.
9. The method according to claim 4, It is characterized in that The method for preparing the secondary active component solution in step (1) comprises: mixing the secondary active component precursor with water.
10. The method according to claim 9, It is characterized in that The dosage ratio of the secondary active component precursor to water is 1g:4-10mL.
11. The method according to claim 4, It is characterized in that In step (2), the usage ratio of the carrier, surfactant and water is 10-1000 g: 1 g: 30-500 mL.
12. The method according to claim 4 or 5, It is characterized in that The carrier is selected from one or more of titanium dioxide, glass fiber, aluminum oxide, zirconium dioxide, silicon dioxide and calcium oxide.
13. The method according to claim 4, It is characterized in that The weight ratio of the main active component precursor, the secondary active component precursor, the carrier and the adhesive is 2-20:1-10:10-200:
1.
14. The method according to claim 4 or 5, It is characterized in that The surfactant is selected from one or more of palmitic acid, oleic acid, vaseline and paraffin.
15. The method according to claim 4, It is characterized in that In step (2), the mixing conditions include: temperature of 70-90°C and time of 30-100 min.
16. The method according to claim 4, It is characterized in that In step (3), the mixing conditions include: temperature of 70-90°C and time of 30-100 min.
17. The method according to claim 4, It is characterized in that In step (3), the calcination conditions include: temperature of 300-550°C and time of 4-8h.
18. The method according to claim 4, It is characterized in that In step (3), the adhesive is selected from one or more of cellulose ester, polyvinyl alcohol, epoxy resin and polyacrylate.
19. The method according to claim 1, It is characterized in that The regeneration conditions include: temperature of 20-380° C. and time of 0.5-5 h.
20. The method according to claim 1, It is characterized in that The weight ratio of the denitration catalyst regeneration powder to the waste denitration catalyst is 0.005-0.1:1.