A method for treating gaps between plastic and metal joints
By using low-modulus, high-elasticity adhesives, fiberglass mats, and epoxy resin leveling treatment, combined with a composite coating, the problems of cracking and appearance quality in vehicle gaps were solved, achieving a tight connection and aesthetically pleasing effect.
Patent Information
- Application Number
- CN202311200827.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-15
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-15
AI Technical Summary
Cracks of varying lengths often appear at the connection between the driver's cab cover and the car body of rail transit vehicles. Even after repair, the cracks may reappear, affecting the sealing performance and appearance quality.
The gaps are filled with a low-modulus, high-elasticity adhesive, and leveled with fiberglass mat and epoxy resin. A composite coating consisting of epoxy primer, unsaturated polyester putty, polyurethane intermediate coat, and polyurethane topcoat is used to ensure tight connections and good appearance.
It effectively avoids cracking of the adhesive joint caused by thermal stress, improves the surface smoothness and appearance quality of the joint, makes the connection smooth and beautiful, and prevents cracking from happening again.
Smart Images

Figure CN117402562B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of vehicle sealing and surface treatment technology, and specifically relates to a method for treating the gaps between plastic and metal joints. Background Technology
[0002] Cracks of varying lengths often appear at the connection between the driver's cab cover (e.g., fiberglass) and the car body (e.g., aluminum alloy) of rail transit vehicles. These cracks, even after repair, tend to reopen, indicating an inertial quality issue that significantly impacts the vehicle's sealing performance and appearance. During advanced vehicle maintenance, layer-by-layer grinding analysis of the cracked areas revealed cracks in both the surface coating and the sealant layer. The sealant layer exhibited failure modes including near-wall cohesive failure and adhesive failure. Currently, the industry urgently needs an effective method to address the cracking problem at the connection between the cover and the car body. Summary of the Invention
[0003] This invention aims to solve at least one of the technical problems existing in the prior art. To this end, this invention proposes a method for treating the gap between plastic and metal. The method of this invention can solve the problem of cracking at the joint between plastic and metal, and also solve the appearance quality problem at the joint. Applying the method of this invention to the gap at the connection between the driver's cab cover (e.g., fiberglass) and the vehicle body (e.g., aluminum alloy) can solve both the cracking and appearance quality problems.
[0004] The inventive concept of this invention is as follows: This invention fills the gap between plastic and metal by selecting a specific adhesive (i.e., sealant), and after curing, uses fiberglass mat and epoxy resin to level the joint around the perimeter, so that the plastic and metal are tightly connected, avoiding cracking at the joint again, and forming a complete whole between the plastic and metal.
[0005] This invention utilizes a low-modulus, high-elasticity adhesive to fill and seal the gaps between plastics (such as fiberglass for vehicle driver's cab covers) and metals (such as aluminum alloys), effectively preventing cracking of the adhesive joints due to thermal stress during vehicle operation. By adding fiberglass mat and epoxy resin to level the surface of the adhesive joint, the problem of surface unevenness caused by adhesive shrinkage and cracking of the epoxy resin coating is effectively solved. In other words, through the combined treatment of adhesive, fiberglass mat, and epoxy resin, the gaps between the plastic and metal are well filled and less prone to cracking.
[0006] Furthermore, after the aforementioned leveling treatment, a composite coating consisting of epoxy primer, unsaturated polyester putty, polyurethane intermediate coat, and polyurethane topcoat is applied to the surface of the formed fiberglass mat and epoxy resin plastic layer to further improve surface smoothness and appearance quality. This effectively solves the appearance quality problem at the connection between the plastic and the alloy, resulting in a smooth and aesthetically pleasing joint.
[0007] A first aspect of the present invention provides a method for treating the gap between plastic and metal.
[0008] Specifically, a method for treating the gap between plastic and metal includes the following steps:
[0009] (1) Cleaning treatment: Clean the plastic and metal areas to be joined, then grind the areas to be joined, and then clean them again;
[0010] (2) Adhesion accelerator treatment: Wipe the area to be joined with the adhesion accelerator and let it dry;
[0011] (3) Apply sealant: Apply sealant to the gaps in the joint area, smooth it out, and allow it to cure.
[0012] (4) Leveling treatment: Clean the area to be connected after step (3), apply epoxy resin to the surface of the area to be connected, then lay glass fiber mat with epoxy resin coating on the surface of the area to be connected, roll the glass fiber mat, and continue to lay glass fiber mat with epoxy resin coating. The upper glass fiber mat is at least 2 mm wider than the lower glass fiber mat, and then cure.
[0013] The sealant is a polyurethane sealant.
[0014] Preferably, the polyurethane sealant satisfies at least one of the following conditions:
[0015] (1) Tensile strength ≥ 7 MPa;
[0016] (2) Shear strength ≥ 4 MPa;
[0017] (3) Elongation at break ≥ 400%;
[0018] (4) Curing speed ≥ 3 mm / 24 h;
[0019] (5) Glass transition temperature ≤ 60℃;
[0020] (6) Uncut right-angle tear strength ≥15N / mm.
[0021] Preferably, in step (1), the plastic is a driver's cab cover; more preferably, the plastic is fiberglass.
[0022] Preferably, in step (1), the metal is the car body; more preferably, the metal is an aluminum alloy.
[0023] Preferably, in step (1), the surfaces of the plastic and metal to be joined are cleaned to remove grease and dust.
[0024] Preferably, the cleaning process is as follows: using a clean, lint-free wiping paper dipped in cleaning agent to wipe the surface of the plastic and metal areas to be connected, removing grease and dust.
[0025] Preferably, in step (1), the surface of the area to be joined is sanded with 80-150 grit sandpaper until the base material (plastic or metal) is exposed.
[0026] Preferably, in step (1), the specific process of further cleaning is as follows: use a clean, lint-free wiping paper dipped in cleaning agent to wipe the surface of the plastic and metal areas to be connected, and let it dry for more than 10 minutes. For example, let it dry for 11-100 minutes.
[0027] Preferably, in step (2), the adhesion promoter includes an activator and a primer, both of which are commercially available conventional products. For example, the adhesion promoter is Sika Aktivator activator and Sika206 G+P primer, wherein Sika Aktivator activator is a silane coupling agent and Sika206 G+P primer is an isocyanate homopolymer.
[0028] Preferably, in step (2), the drying time is 15 minutes or more, for example, 16-100 minutes.
[0029] Preferably, in step (2), the area to be joined is wiped with an adhesion promoter using a wiping paper or a sponge, and wiping back and forth is prohibited, i.e., wiping in one direction only.
[0030] Preferably, in step (2), the thinner the film layer formed by wiping with the adhesion promoter, the better, and it should fully cover the area to be joined without exposing the bottom.
[0031] Preferably, in step (3), a pneumatic or electric glue gun is used to apply sealant to the gap in the area to be connected. When applying the sealant, the nozzle should be inserted as deep as possible into the bottom of the gap. The sealant should be pressed and smoothed with a scraper to ensure that there are no voids in the seal.
[0032] Preferably, in step (3), for areas with poor appearance such as corners and interfaces, a sealant repair agent is used for fine repair to ensure that the sealant is flat and aesthetically pleasing.
[0033] Preferably, in step (3), the curing is performed at room temperature for 48 hours or more, for example, 50-100 hours.
[0034] Preferably, in step (3), when the gap depth exceeds 12mm, the sealant is applied in multiple applications, and before each application of the sealant, an adhesion promoter is applied as in step (2) (i.e., an adhesion promoter is applied to the surface of the sealant).
[0035] Preferably, in step (4), the specific cleaning process is as follows: use a clean, lint-free wiping paper dipped in cleaning agent to wipe the area to be connected until there is no grease or dust, use 80-150 grit sandpaper to sand the cleaned surface until the color of the substrate is exposed, use wiping paper dipped in cleaning agent to wipe the surface again, and let it dry for more than 10 minutes.
[0036] Preferably, in step (4), the curing is performed at room temperature for more than 24 hours, for example, 15-35 hours.
[0037] Preferably, in step (4), the bottom layer bubbles are removed by rolling.
[0038] Preferably, in step (4), the number of layers of glass fiber mat laid is at least 3, for example 3-10 layers.
[0039] Preferably, after step (4), the process further includes step (5) epoxy primer spraying treatment, step (6) scraping elastic polyester putty, step (7) spraying polyurethane intermediate coat, and step (8) spraying polyurethane color paint.
[0040] Preferably, the specific process of step (5) epoxy primer spraying is as follows: use 80-150 grit sandpaper to sand the surface of the glass fiber mat, and at the same time use a dust cloth to clean and remove dust, mix the epoxy primer, and at the same time use a wet-on-wet spraying process to spray 2-5 coats of epoxy primer on the surface of the glass fiber mat. Each coat needs to be surface dry for about 30-40 minutes. After the overall spraying is completed, it is cured at room temperature for more than 16 hours.
[0041] Preferably, the specific process of step (6) of applying elastic polyester putty is as follows: use a soft scraper to apply elastic polyester putty to the epoxy primer surface. Usually, it is necessary to apply 2 or 4 coats. Between each two coats, a crisscrossing scraping method should be used. The thickness of each coat should not exceed 1 mm, and the total thickness should not exceed 3 mm until the surface smoothness meets the requirements. Each coat should be cured at room temperature for more than 3 hours.
[0042] Preferably, the specific process of spraying polyurethane intermediate paint in step (7) is as follows: after spraying polyurethane intermediate paint, it needs to be cured at room temperature for more than 16 hours. At the same time, check the surface flatness of the area to be connected. If there are still depressions, use elastic polyester putty to fill them. After drying and sanding, spray white polyurethane topcoat. Find defects under high-gloss conditions. If there are defects, use elastic polyester putty to smooth them again.
[0043] Preferably, the specific process of spraying polyurethane paint in step (8) is as follows: according to the art requirements, spray the polyurethane topcoat with the corresponding color number onto the surface of the sprayed polyurethane intermediate paint.
[0044] A second aspect of the present invention provides an application of a method for treating gaps between plastic and metal joints.
[0045] The above-mentioned method for treating the gap between plastic and metal is applied to the gap between the fixed cover of the driver's cab and the vehicle body.
[0046] Preferably, the vehicle is a rail transit vehicle.
[0047] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0048] (1) The present invention fills the gap between plastic and metal by selecting a specific adhesive (i.e. sealant). After curing, glass fiber mat and epoxy resin are used to level the joint around the perimeter, so that the plastic and metal are tightly connected, avoiding cracking at the joint and forming a complete whole.
[0049] (2) This invention utilizes a low-modulus, high-elasticity adhesive to fill and seal the gaps between plastics (e.g., the driver's cab cover of a vehicle, often made of fiberglass) and metals (e.g., aluminum alloy), effectively preventing cracking of the adhesive joints due to thermal stress during vehicle operation. By adding fiberglass mat and epoxy resin to level the surface of the adhesive joints, the problems of surface unevenness caused by adhesive shrinkage and cracking of the epoxy resin coating are effectively solved. In other words, through the combined treatment of adhesive, fiberglass mat, and epoxy resin, the gaps between the plastic and metal are well filled and less prone to cracking.
[0050] (3) After the above leveling treatment, a composite coating of epoxy primer + unsaturated polyester putty + polyurethane intermediate coat + polyurethane topcoat is applied to the surface of the formed glass fiber felt and epoxy resin plastic layer to further improve the surface smoothness and appearance quality. This effectively solves the appearance quality problem at the connection between plastic and alloy, resulting in a smooth and aesthetically pleasing connection. Attached Figure Description
[0051] Figure 1 This is a diagram showing a gap at the connection between the driver's cab cover and the car body in Example 1.
[0052] Figure 2 This is the state of the connection between the driver's cab fixing cover and the car body after step (4) of Example 1;
[0053] Figure 3 This is the state of the connection between the driver's cab fixing cover and the car body after step (6) of Example 1;
[0054] Figure 4 This is the state of the connection between the driver's cab fixing cover and the car body after step (12) of Example 1;
[0055] Figure 5 The image shows the condition of the EMU driver's cab fixing cover and the car body after two years of outdoor all-weather aging, following the treatment method in Example 1. Detailed Implementation
[0056] To enable those skilled in the art to more clearly understand the technical solutions described in this invention, the following embodiments are provided for illustration. It should be noted that the following embodiments do not constitute a limitation on the scope of protection claimed by this invention.
[0057] Unless otherwise specified, the raw materials, reagents or devices used in the following examples are available from conventional commercial sources or can be obtained by existing known methods.
[0058] Example 1
[0059] Taking the gap at the connection between the driver's cab fixed cover (made of fiberglass) and the car body (made of aluminum alloy) of a high-speed train as an example (e.g.) Figure 1 As shown, the method of the present invention is used to seal, bond and surface treat the material.
[0060] A method for treating gaps between plastic and metal joints includes the following steps:
[0061] (1) Before operation, confirm the ambient temperature and humidity. The temperature should be 15℃-35℃ and the relative humidity should be 50%-75%. Apply protective tape around the gap between the driver's cab cover and the vehicle body. The tape should be applied starting 3mm from the outside of the gap to ensure that the sealing surface meets the requirements for subsequent adhesive application.
[0062] (2) Wipe the surface of the fixing cover and the area to be connected on the vehicle body with clean, lint-free wiping paper dipped in anhydrous alcohol until there is no grease or dust. Use a pneumatic grinder with 80-grit sandpaper to grind the surface of the area to be connected until the original color of the fiberglass and aluminum alloy is exposed (Note: Grinding of deeper areas in the gaps should be completed before the fixing cover is installed). Wipe the surface of the fixing cover and the area to be connected on the vehicle body with wiping paper dipped in anhydrous alcohol again and let it dry for 15 minutes.
[0063] (3) Use a nano sponge to apply Sika Aktivator activator to the area to be connected and let it dry for 20 minutes. Use a nano sponge to apply Sika206 G+P primer to the surface of the area to be connected and brush a thin film layer onto it. Let it dry for 20 minutes. The thinner the film layer, the better. It should fully cover the area to be connected without exposing the base layer. Do not brush back and forth.
[0064] (4) Use a pneumatic glue gun to apply Sika265 single-component moisture-curing polyurethane sealant to the gap between the fixed cover and the vehicle body. When applying the sealant, the nozzle of the pneumatic glue gun should be inserted as deep as possible into the bottom of the gap to ensure that the sealant overflows from the bottom outwards. After application, use a scraper to press and smooth the sealant to ensure that there are no voids. After the sealant is applied, it needs to be cured at room temperature for 50 hours.
[0065] (5) After the sealant has cured, remove the protective tape and wipe the vehicle body, mounting cover and sealant surface with clean, lint-free wiping paper dipped in anhydrous alcohol until there is no grease and dust. Use a pneumatic grinder with 80-grit sandpaper to grind the cleaned surface until the color of the mounting cover (fiberglass) and vehicle body (aluminum alloy) is exposed. Wipe the surface again with wiping paper dipped in anhydrous alcohol and let it dry for 15 minutes.
[0066] (6) Cut glass fiber mats with widths of 80mm, 100mm, and 120mm and lengths of 5890mm for later use. Mix epoxy resin with a weight ratio of 3:1 between the main agent (the main agent is a mixture of epoxy resin (50%) and modified toughening resin (40%), the main agent product model is MegaGlue4006 / B20) and the curing agent (the curing agent is modified amine, the product model is MegaGlue HD4006 / B20) and let it stand for about 30 minutes to activate. Use a roller to apply epoxy resin evenly to the car body, the fixed cover, and the surface that needs to be leveled with sealant. In the same way, apply epoxy resin evenly to the surface of the 80mm wide glass fiber mat and lay the glass fiber mat on the surface that needs to be leveled with sealant. After completion, use a roller to apply epoxy resin to the surface of the laid glass fiber mat to ensure that the epoxy resin completely wets the glass fiber mat layer. At the same time, remove the bottom air bubbles by rolling.
[0067] (7) After the 80mm wide glass fiber mat (first layer) is laid and bonded, the 100mm wide glass fiber mat (second layer) and the 120mm wide glass fiber mat (third layer) are laid and bonded in the same way, and cured at room temperature for 30 hours.
[0068] (8) After the glass fiber mat layer has cured, use 80-grit sandpaper to sand the surface of the glass fiber mat layer and clean the dust with a tack cloth. Mix the epoxy primer with the main agent (the main agent is mainly epoxy resin, and the main agent product model is THD06WEP-200) and the curing agent (the curing agent is mainly polyamide emulsion, and the curing agent product model is WEP-200-G) in a weight ratio of 5:1. Use a high-pressure airless spray gun and a wet-on-wet spraying process to spray two coats of epoxy primer onto the surface of the glass fiber mat layer. Each coat needs to be surface dry for about 30 minutes. After the overall spraying is completed, cure at room temperature for 20 hours. The average dry film thickness is controlled at about 60μm.
[0069] (9) Use sandpaper to lightly sand the epoxy primer surface and clean it with a dust cloth. Mix the elastic polyester putty (manufacturer Sifang Weikai, model UP100) at a weight ratio of 100:2.5. Level the areas with larger depressions in advance. After curing for 3 hours, use a soft scraper to apply the elastic polyester putty to the surface. Apply the elastic polyester putty horizontally along the outside of the fixed cover for the first time. Apply the putty vertically along the perimeter of the fixed cover for the second time. For the third and fourth times, the consistency of the elastic polyester putty needs to be slightly reduced (add 2% of thinner in 3 stages. The main component of the thinner is styrene, which improves the fluidity of the putty until the putty can fully fill the pores and small pits on the surface). Apply the putty to the surface using horizontal and vertical scraping methods respectively. The thickness of each scraping should not exceed 1mm, and the total thickness should be 3mm until the surface flatness meets the requirements. Cure each layer at room temperature for 4 hours to form a putty layer.
[0070] (10) Use 80-grit, 120-grit, and 180-grit sandpaper to sand the putty layer step by step and clean it with a dust cloth. Mix polyurethane intermediate paint (polyurethane intermediate paint includes main agent and curing agent, the main agent is mainly acrylic resin emulsion, model TBZ04 WIPU-100, and the curing agent is mainly 1,6-hexamethylene diisocyanate homopolymer, model WIPU-100-G) with an air spray gun and a wet-on-wet spraying process to spray two coats of polyurethane intermediate paint on the surface of the putty layer. Each coat needs to be surface dry for about 30 minutes. After the overall spraying is completed, cure at room temperature for 18 hours. The average dry film thickness is controlled at about 50 μm to form a polyurethane intermediate coating.
[0071] (11) Visually inspect the surface of the polyurethane intermediate coating under light intensity of not less than 400 Lx to check for any obvious uneven areas. If any are found, sand them and then fill them with putty. After that, sand the polyurethane intermediate coating with 240 grit sandpaper and clean it with a dust cloth. Mix the white polyurethane topcoat (which includes the main agent and the curing agent, the main agent being an acrylic copolymer, model TBS04B WPU-400. The curing agent is mainly composed of 1,6-hexamethylene diisocyanate homopolymer, model WPU-400-G) with an air spray gun and a wet-on-wet spraying process. Apply two coats of white polyurethane topcoat to the surface of the polyurethane intermediate coating. Each coat should be surface dry for about 30 minutes. After the overall spraying is completed, allow it to level for 2 hours, dry it at 60°C for 3 hours, and then air dry it at room temperature for 9 hours. The average dry film thickness should be controlled at about 30 μm.
[0072] (12) Visually inspect the surface of the white polyurethane topcoat layer again under light intensity of not less than 400 Lx to check for pits or other defects. If any are found, treat them by sanding and then patching with putty. After completion, sand the polyurethane topcoat layer with 320 grit sandpaper and clean it with a dust cloth. Mix the white polyurethane topcoat according to a weight ratio of 4:1. Use an air spray gun and a wet-on-wet spraying process to spray the white polyurethane topcoat in two coats. Each coat should be surface dry for about 30 minutes. After the topcoat is surface dry for 1 hour, spray the polyurethane clear varnish. The polyurethane clear varnish should be mixed with a main agent to curing agent weight ratio of 3:1 (the main agent is acrylic copolymer, manufactured by Sifang Weikai; the main components of the curing agent are 1,6-hexamethylene diisocyanate homopolymer (80%) and propylene glycol diacetate (20%), manufactured by Sifang Weikai). After the overall spraying is completed, level it for 2 hours, dry it at 60℃ for 2.5 hours, and then air dry it at room temperature for 18 hours. The average dry film thickness should be controlled at about 50 μm.
[0073] Figure 2 This is the state of the connection between the driver's cab fixing cover and the car body after step (4) of Example 1; Figure 3 This is the state of the connection between the driver's cab fixing cover and the car body after step (6) of Example 1; Figure 4 The image shows the state of the connection between the fixed cover of the driver's cab and the car body after step (12) of Example 1; it can be seen that there are no cracks at the connection between the fixed cover of the driver's cab and the car body. Figure 5 This is the state of the EMU driver's cab mounting cover and car body after two years of outdoor all-weather aging, treated using the method in Example 1. Even after two years of all-weather aging, no cracks have appeared.
[0074] Comparative Example 1
[0075] Compared with Example 1, the sealant used in Comparative Example 1 was Nogawa Chemical 309 sealant, and the rest of the process was the same as in Example 1.
[0076] Comparative Example 2
[0077] Compared to Example 1, Comparative Example 2 did not use the fiberglass mat from Example 1, but the rest of the process was the same as in Example 1. As a result, after treatment by the method in Comparative Example 1, a crack with a length of 50 mm appeared at the connection between the vehicle body and the driver's cab cover.
[0078] Product effectiveness test
[0079] The driver's cab mounting cover and vehicle body, after being treated by the methods of Example 1 and Comparative Examples 1-2, were tested under all-weather aging and normal online operation conditions. The results are shown in Table 1.
[0080] Table 1
[0081]
[0082] As can be seen from Table 1, the driver's cab fixing cover treated by the method of Embodiment 1 of the present invention is firmly connected to the vehicle body and is not prone to cracking, while the driver's cab fixing cover treated by the methods of Comparative Examples 1-2 is not firmly connected to the vehicle body and is prone to cracking. Therefore, it is evident that the driver's cab fixing cover treated by the method of the present invention is firmly connected to the vehicle body and is not prone to cracking.
Claims
1. A method of treating a plastic-to-metal joint gap, characterized in that, Includes the following steps: (1) Cleaning treatment: Clean the plastic and metal areas to be joined, then grind the areas to be joined, and then clean them again; (2) Adhesion accelerator treatment: Wipe the area to be joined with the adhesion accelerator and let it dry; (3) Apply sealant: Apply sealant to the gaps in the joint area, smooth it out, and allow it to cure; (4) Leveling treatment: Clean the area to be connected after step (3), apply epoxy resin to the surface of the area to be connected, then lay glass fiber mat with epoxy resin coating on the surface of the area to be connected, roll the glass fiber mat, and continue to lay glass fiber mat with epoxy resin coating. The upper glass fiber mat is at least 2 mm wider than the lower glass fiber mat, and then cure. The sealant is a polyurethane sealant; In step (1), the plastic is fiberglass; the metal is aluminum alloy; After step (4), the process includes step (5) epoxy primer spraying, step (6) applying elastic polyester putty, step (7) spraying polyurethane intermediate coat, and step (8) spraying polyurethane color paint.
2. The method of claim 1, wherein, In step (1), the plastic is the driver's cab cover; the metal is the vehicle body.
3. The method of claim 1, wherein, In step (3), when the gap depth exceeds 12 mm, the sealant is applied in multiple applications. Before each application of the sealant, the adhesion promoter is applied as in step (2).
4. The method according to claim 1, characterized in that, In step (4), the number of layers of fiberglass mat laid is at least 3.
5. The method according to claim 1, characterized in that, The specific process of step (5) epoxy primer spraying is as follows: use 80-150 grit sandpaper to sand the surface of the glass fiber mat, and at the same time use a dust cloth to clean and remove dust. Mix the epoxy primer, and at the same time use a wet-on-wet spraying process to spray 2-5 coats of epoxy primer on the surface of the glass fiber mat. Each coat needs to be surface dry for 30-40 minutes. After the overall spraying is completed, it should be cured at room temperature for more than 16 hours. The specific process of applying elastic polyester putty in step (6) is as follows: Use a soft scraper to apply elastic polyester putty to the epoxy primer surface. Two or four coats are required. Between each two coats, a crisscrossing scraping method should be used. The thickness of each coat should not exceed 1 mm, and the total thickness should not exceed 3 mm until the surface smoothness meets the requirements. Each coat should be cured at room temperature for more than 3 hours.
6. The method according to claim 1, characterized in that, The specific process of spraying polyurethane intermediate paint in step (7) is as follows: after spraying polyurethane intermediate paint, it needs to be cured at room temperature for more than 16 hours. At the same time, check the surface flatness of the area to be connected. If there are still depressions, use elastic polyester putty to fill them. After drying and sanding, spray white polyurethane topcoat. Find defects under high-gloss conditions. If there are defects, use elastic polyester putty to smooth them again.
7. The method according to claim 1, characterized in that, The specific process of step (8) spraying polyurethane paint is as follows: according to the art requirements, spray the polyurethane topcoat with the corresponding color number onto the surface of the sprayed polyurethane intermediate paint.
8. The application of the method for treating the joint gap between plastic and metal according to any one of claims 1-7 in treating the joint gap between the driver's cab cover and the vehicle body.
Citation Information
Patent Citations
Surface treatment method for enhancing adhesive property of epoxy resin adhesive-bonded joint
CN112574677A
Sealing structure of pressure-maintaining glass fiber reinforced plastic product and processing method
CN116476279A