Optical thin film materials, optical thin film preparation methods, and display panels
By introducing aromatic rings and sulfur atoms into optical thin film materials, the toxicity and scattering problems caused by halogen atoms and nanoparticles are solved, resulting in high refractive index and stable optical thin films suitable for display panels.
Patent Information
- Application Number
- CN202310546143.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-05-15
AI Technical Summary
In the prior art, the use of halogen atoms is restricted due to their toxicity and the corrosive gases produced during combustion, while nanoparticles have poor dispersion and stability in optical devices, leading to a decline in optical performance.
Compounds containing aromatic rings and/or sulfur atoms are used as optical thin film materials. The refractive index of the polymer is increased through cross-linking polymerization, avoiding the use of halogen atoms and nanoparticles, thus forming a high-refractive-index optical thin film.
High refractive index optical thin films were achieved, avoiding the generation of toxic gases and the scattering of nanoparticles, and improving the mechanical properties and stability of optical thin films.
Smart Images

Figure CN117447652B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of display technology, and in particular to an optical thin film material, a method for preparing the optical thin film, and a display panel. Background Technology
[0002] Currently, high-refractive-index polymer materials are often used in sensors, displays, and other devices to improve optical sensing and display effects.
[0003] In related technologies, halogen atoms or nanoparticles can be used to improve the refractive index of materials. However, the use of halogen atoms is restricted due to their toxicity and the corrosive gases produced during combustion. Nanoparticles and polymers have poor dispersibility and stability, and when applied to optical devices, nanoparticles are prone to scattering, which in turn affects the optical performance of the devices. Summary of the Invention
[0004] This invention provides an optical thin film material, a method for preparing an optical thin film, and a display panel, which can improve the refractive index of the optical thin film.
[0005] This invention provides an optical thin film material, the optical thin film material comprising at least one compound represented by the following general formula;
[0006]
[0007] One of R1 and R2 includes an aromatic ring and / or a sulfur atom, and the other includes at least one of an acryloyloxy group, an aromatic ring, and a sulfur atom.
[0008] In one embodiment of the present invention, both R1 and R2 comprise an acryloxy group.
[0009] In one embodiment of the present invention, the optical thin film material includes at least one of a first compound, a second compound, and a third compound;
[0010] The structural formula of the first compound is shown below:
[0011]
[0012] The structural formula of the second compound is shown below:
[0013]
[0014] The structural formula of the third compound is shown below:
[0015]
[0016] In one embodiment of the present invention, the optical thin film material comprises 50 to 100 parts by mass of the first compound, 0 to 50 parts by mass of the second compound, and 0 to 50 parts by mass of the third compound.
[0017] In one embodiment of the present invention, the optical thin film material further includes an active diluent and a photoinitiator, wherein the active diluent includes an active diluent containing a monofunctional group or an active diluent containing a difunctional group, and the photoinitiator includes a type I photoinitiator and / or a type II photoinitiator.
[0018] In one embodiment of the present invention, the optical thin film material comprises 10 to 30 parts by weight of the active diluent and 1 to 10 parts by weight of the photoinitiator.
[0019] According to the above-mentioned objectives of the present invention, embodiments of the present invention also provide a method for preparing an optical thin film, which includes the following steps:
[0020] An optical thin film material is provided, the optical thin film material comprising at least one compound represented by the following general formula; Wherein, one of R1 and R2 includes an aromatic ring and / or a sulfur atom, and the other includes at least one of an acryloyloxy group, an aromatic ring, and a sulfur atom;
[0021] The optical thin film is prepared using the aforementioned optical thin film material.
[0022] In one embodiment of the present invention, the step of providing the optical thin film material further includes:
[0023] The optical thin film material also includes an active diluent and a photoinitiator;
[0024] The optical thin film materials are mixed to form a mixture;
[0025] The mixture is used for coating to obtain an intermediate film;
[0026] The intermediate film is cured to obtain the optical film.
[0027] In one embodiment of the present invention, the refractive index of the optical thin film is greater than or equal to 1.5 and less than or equal to 1.8.
[0028] In accordance with the above-mentioned objectives of the present invention, embodiments of the present invention also provide a display panel, the display panel comprising an optical thin film, the optical thin film being prepared using the optical thin film preparation method.
[0029] The beneficial effects of the present invention are as follows: By forming aromatic rings and / or sulfur atoms in the optical thin film material, the present invention can effectively improve the refractive index of the polymer. Therefore, the optical thin film material provided in the embodiments of the present invention can form an optical thin film with a high refractive index. Moreover, the optical thin film material does not contain halogen atoms or added metal oxide nanoparticles, thus avoiding the phenomenon of being restricted in use due to toxicity and corrosive gases generated during combustion, and eliminating the adverse effects of nanoparticles on light scattering. Attached Figure Description
[0030] The technical solution and other beneficial effects of the present invention will become apparent from the following detailed description of specific embodiments of the invention, in conjunction with the accompanying drawings.
[0031] Figure 1 A flowchart illustrating the method for preparing an optical thin film according to an embodiment of the present invention;
[0032] Figure 2 This is a schematic diagram of a display panel provided in an embodiment of the present invention. Detailed Implementation
[0033] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0034] The following disclosure provides many different embodiments or examples for implementing various structures of the invention. To simplify the disclosure, specific examples of components and arrangements are described below. These are merely examples and are not intended to limit the invention. Furthermore, reference numerals and / or letters may be repeated in different examples; such repetition is for simplification and clarity and does not in itself indicate a relationship between the various embodiments and / or arrangements discussed. In addition, examples of various specific processes and materials are provided in this invention, but those skilled in the art will recognize the application of other processes and / or the use of other materials.
[0035] This invention provides an optical thin film material comprising at least one compound represented by the following general formula;
[0036]
[0037] One of R1 and R2 includes an aromatic ring and / or a sulfur atom, and the other includes at least one of an acryloyloxy group, an aromatic ring, and a sulfur atom.
[0038] In practical applications, embodiments of the present invention form aromatic rings and / or sulfur atoms in the optical thin film material. Both aromatic rings and sulfur atoms can effectively increase the refractive index of the polymer. Therefore, the optical thin film material provided by the embodiments of the present invention can form an optical thin film with a high refractive index. Furthermore, the optical thin film material does not contain halogen atoms or added metal oxide nanoparticles, thus avoiding the phenomenon of being restricted in use due to toxicity and corrosive gases generated during combustion, and eliminating the adverse effects of nanoparticles on light scattering.
[0039] Specifically, the Lorentz-Lorenz equation can be used to predict the refractive index of polymers, and the equation is as follows:
[0040]
[0041] And after conversion, we get:
[0042]
[0043] In the above formula, the refractive index (n) is expressed using the molecular refractive index (R), molecular weight (M), and molecular volume (V) of the polymer repeating unit. R / M can be further referred to as the molar refractive index (Rm). M M / V is the sum of the refractive indices of the atoms and groups of the components that make up the repeating unit of a polymer. Similarly, M / V can be expressed as molar volume (V0). M The reciprocal of ). And after verification, the molar refractive index R of each group is obtained in Table 1 below. M .
[0044] Table 1: Comparison of Molar Refractive Indices
[0045]
[0046]
[0047] As can be seen from the table above, aromatic rings, halogen atoms other than fluorine, and sulfur atoms can all effectively improve the refractive index of polymers. Therefore, embodiments of the present invention provide an optical thin film material, which includes at least one compound represented by the following general formula.
[0048]
[0049] One of R1 and R2 includes an aromatic ring and / or a sulfur atom, and the other includes at least one of an acryloyloxy group, an aromatic ring, and a sulfur atom.
[0050] It is understood that the embodiments of the present invention effectively improve the molar refractive index of the optical thin film material by forming aromatic rings and / or sulfur atoms with high molar refractive index in the compound, thereby effectively improving the refractive index of the optical thin film made using the optical thin film material. Furthermore, the embodiments of the present invention avoid the use of halogen atoms, thereby avoiding the phenomenon of being restricted in use due to toxicity and corrosive gases generated during combustion.
[0051] Furthermore, the compounds provided in the embodiments of the present invention may also include acryloyloxy groups, and the acryloyloxy groups can undergo cross-linking polymerization reactions to increase the degree of cross-linking.
[0052] In one embodiment, both R1 and R2 include an acryloxy group, which can effectively increase the degree of crosslinking of the polymer during the polymerization reaction in the process of forming the optical thin film material, thereby improving the mechanical properties and stability of the optical thin film made using the optical thin film material, and improving its resistance to high and low temperatures, high temperature and high humidity, and thermal shock.
[0053] In this embodiment of the invention, the optical thin film material may include at least one of a first compound, a second compound, and a third compound. Specifically, the structural formula of the first compound is shown below:
[0054]
[0055] In one embodiment, R1 can be R2 can be
[0056] In the first compound, both R1 and R2 contain a large number of sulfur atoms and aromatic rings, resulting in a high molar refractive index. This can effectively improve the refractive index of optical films made using this optical thin film material.
[0057] The structural formula of the second compound is shown below:
[0058]
[0059] In one embodiment, R1 can be R2 can be
[0060] In the second compound, the number of aromatic rings in R1 and R2 is greater than that in the first compound. Similarly, the second compound also has a higher molar refractive index, which can effectively improve the refractive index of optical films made using this optical thin film material.
[0061] The structural formula of the third compound is shown below:
[0062]
[0063] In one embodiment, R1 can be R2 can be
[0064] In the third compound, R1 contains an aromatic ring and a sulfur atom, which increases the refractive index of the optical film made from this optical film material. In addition, both R1 and R2 contain a large number of acryloyloxy groups, which can undergo cross-linking polymerization to increase the degree of cross-linking. Thus, during the polymerization reaction that occurs in the formation of the optical film, the degree of cross-linking of the optical film can be effectively increased, thereby improving the mechanical properties and stability of the optical film made from this optical film material, and enhancing its resistance to high and low temperatures, high temperature and high humidity, and thermal shock.
[0065] Furthermore, the optical thin film material may include 50 to 100 parts by mass of a first compound, 0 to 50 parts by mass of a second compound, and 0 to 50 parts by mass of a third compound. For example, the mass parts of the first compound may be 50, 60, 70, 80, 90, or 100, the mass parts of the second compound may be 0, 10, 20, 30, 40, or 50, and the mass parts of the third compound may be 0, 10, 20, 30, 40, or 50. The above values are examples of the first, second, and third compounds within their respective mass part ranges and are not limited thereto; they may also be any values within the corresponding mass part ranges.
[0066] In addition, the optical film material is a photocurable material, and the optical film material also includes a photoinitiator. In order to adjust the viscosity of the optical film material, the optical film material also includes an active diluent.
[0067] In one embodiment, the reactive diluent includes a reactive diluent containing a monofunctional group or a reactive diluent containing a difunctional group. For example, monofunctional reactive diluents include hydroxyethyl (meth)acrylate, isobornyl (meth)acrylate, 2-phenoxyethyl acrylate, lauryl acrylate, tetrahydrofuran acrylate, etc.; difunctional reactive diluents include diethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol diacrylate, dipropylene glycol diacrylate, dipropylene glycol diacrylate, tricyclodecanedimethyl diacrylate, neopentyl glycol diacrylate, 1,6-hexanediol diacrylate, etc.
[0068] Photoinitiators include type I photoinitiators and / or type II photoinitiators. Type I photoinitiators generate free radicals through molecular decomposition due to differences in chemical structure or molecular binding energy. Type II (hydrogen-abstracting) photoinitiators introduce a tertiary amine as a co-initiator. Specifically, type I photoinitiators can include acetophenone-based photoinitiators and benzoin-based photoinitiators. For example, acetophenone-based photoinitiators can include 4-phenoxydichloroacetophenone, 4-tert-butyldichloroacetophenone, 4-tert-butyltrichloroacetophenone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylacetone, 1(4-isopropylphenyl)-2-hydroxy-2-methylacetone, 1(4-dodecylphenyl)-2-hydroxy-2-methylacetone, 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl) ketone, 1-hydroxycyclohexylphenyl ketone, etc.; benzoin-based photoinitiators can include benzoin methyl ether, benzoin ethyl ether, benzyl dimethyl ketal, etc.; type I photoinitiators can also include acylphosphine oxides and titanium ether compounds. Type II photoinitiators can include benzophenone-based photoinitiators and thioxanone-based photoinitiators. For example, benzophenone-based photoinitiators can include benzophenone, benzoylbenzoic acid, benzoylbenzoic acid methyl ether, 4-phenylbenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3'-dimethyl-4-methoxybenzophenone, etc.; thioxanone-based photoinitiators can include thioxanone, 2-chlorothioxanone, 2-methylthioxanone, 2,4-dimethylthioxanone, isopropylthioxanone, etc. Furthermore, the photoinitiator can be at least one of the above-mentioned photoinitiators.
[0069] In this invention, the optical thin film material comprises 10 to 30 parts by mass of an active diluent and 1 to 10 parts by mass of a photoinitiator. For example, the active diluent may be 10, 20, or 30 parts by mass, and the photoinitiator may be 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass. The above values are examples of the active diluent and photoinitiator within their respective mass part ranges, and are not limited thereto. They may also be any value within the corresponding mass part range.
[0070] As described above, the embodiments of the present invention form aromatic rings and / or sulfur atoms in the optical thin film material. Both aromatic rings and sulfur atoms can effectively increase the refractive index of the polymer. Therefore, the optical thin film material provided by the embodiments of the present invention can form an optical thin film with a high refractive index. Furthermore, the optical thin film material does not contain halogen atoms or added metal oxide nanoparticles, thus avoiding the phenomenon of being restricted in use due to toxicity and corrosive gases generated during combustion, and eliminating the adverse effects of nanoparticles on light scattering.
[0071] In addition, this invention also provides a method for preparing an optical thin film using the optical thin film material described in the above embodiments. Please refer to [link / reference needed]. Figure 1 The method for preparing this optical thin film includes the following steps:
[0072] S10. Providing an optical thin film material, the optical thin film material comprising at least one compound represented by the following general formula; One of R1 and R2 includes an aromatic ring and / or a sulfur atom, and the other includes at least one of an acryloyloxy group, an aromatic ring, and a sulfur atom.
[0073] S20. An optical thin film is prepared using optical thin film materials.
[0074] Specifically, in step S10, the optical thin film material may include at least one of a first compound, a second compound, and a third compound. Specifically, the structural formula of the first compound is shown below:
[0075]
[0076] In one embodiment, R1 can be R2 can be
[0077] The preparation process of the first compound includes: adding 10g of methyl ethyl ketone, 20g of 4′,4-dimercaptodiphenylthionine, and 8.8g of isophorone diisocyanate to a three-necked flask, stirring at 60°C for 10 min, then adding 0.1g of dibutyltin dilaurate catalyst, and reacting at 60°C for 4 h to obtain a sulfhydryl-terminated prepolymer; the specific reaction process is shown below:
[0078]
[0079] Next, 10g of methyl ethyl ketone, 20g of the thiol-terminated prepolymer of the above reaction product, and 13g of ethyl isocyanate methacrylate were added to a three-necked flask. The mixture was stirred at 60°C for 10 min, and then 0.1g of dibutyltin dilaurate catalyst was added. The reaction was carried out at 60°C for 4 h to obtain the first compound with acryloyloxy group termination. The specific reaction process is as follows:
[0080]
[0081] In the first compound, both R1 and R2 contain a large number of sulfur atoms and aromatic rings, resulting in a high molar refractive index. This can effectively improve the refractive index of optical films made using this optical thin film material.
[0082] The structural formula of the second compound is shown below:
[0083]
[0084] In one embodiment, R1 can be R2 can be
[0085] The preparation process of the second compound includes: adding 10g of toluene, 20g of 9′,9-di(4-hydroxyphenyl)fluorene, and 5g of isophorone diisocyanate to a three-necked flask, stirring at 60°C for 10 min, then adding 0.1g of dibutyltin dilaurate catalyst, and reacting at 60°C for 4 h to obtain the hydroxyl-terminated prepolymer; the specific reaction process is shown below:
[0086]
[0087] Next, 10g of toluene, 20g of the hydroxyl-terminated prepolymer from the above reaction, and 2.4g of ethyl isocyanate methacrylate were added to a three-necked flask. The mixture was stirred at 60°C for 10 min, and then 0.1g of dibutyltin dilaurate catalyst was added. The reaction was carried out at 60°C for 4 h to obtain the second compound with acryloyloxy groups at the end of its reaction. The specific reaction process is as follows:
[0088]
[0089] In the second compound, the number of aromatic rings in R1 and R2 is greater than that in the first compound. Similarly, the second compound also has a higher molar refractive index, which can effectively improve the refractive index of optical films made using this optical thin film material.
[0090] The structural formula of the third compound is shown below:
[0091]
[0092] In one embodiment, R1 can be R2 can be
[0093] The preparation process of the third compound includes: adding 10g of methyl ethyl ketone, 20g of 4′,4-dimercaptodiphenylthionine, and 35g of isophorone diisocyanate to a three-necked flask, stirring at 60°C for 10 min, then adding 0.1g of dibutyltin dilaurate catalyst, and reacting at 60°C for 4 h to obtain the isocyanate-terminated prepolymer; the specific reaction process is shown below:
[0094]
[0095] Next, 10g of methyl ethyl ketone, 20g of the isocyanate-terminated prepolymer of the above reaction product, and 25g of dipentaerythritol pentaacrylate were added to a three-necked flask. The mixture was stirred at 60°C for 10 min, and then 0.1g of dibutyltin dilaurate catalyst was added. The reaction was carried out at 60°C for 4 h to obtain the acryloyloxy-terminated third compound. The specific reaction process is as follows:
[0096]
[0097] In the third compound, R1 contains an aromatic ring and a sulfur atom, which increases the refractive index of the optical film made from this optical film material. In addition, both R1 and R2 contain a large number of acryloyloxy groups, which can effectively increase the degree of crosslinking of the polymer during the polymerization reaction in the formation of the optical film material. This improves the mechanical properties and stability of the optical film made from this optical film material, as well as its resistance to high and low temperatures, high temperatures and high humidity, and thermal shock.
[0098] Furthermore, the optical thin film material may include 50 to 100 parts by mass of a first compound, 0 to 50 parts by mass of a second compound, and 0 to 50 parts by mass of a third compound.
[0099] In addition, the optical film material is a photocurable material, and the optical film material also includes a photoinitiator. In order to adjust the viscosity of the optical film material, the optical film material also includes an active diluent.
[0100] In one embodiment, the reactive diluent includes a reactive diluent containing a monofunctional group or a reactive diluent containing a difunctional group. For example, monofunctional reactive diluents include hydroxyethyl (meth)acrylate, isobornyl (meth)acrylate, 2-phenoxyethyl acrylate, lauryl acrylate, tetrahydrofuran acrylate, etc.; difunctional reactive diluents include diethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol diacrylate, dipropylene glycol diacrylate, dipropylene glycol diacrylate, tricyclodecanedimethyl diacrylate, neopentyl glycol diacrylate, 1,6-hexanediol diacrylate, etc.
[0101] Photoinitiators include type I photoinitiators and / or type II photoinitiators. Type I photoinitiators generate free radicals through molecular decomposition due to differences in chemical structure or molecular binding energy. Type II (hydrogen-abstracting) photoinitiators introduce a tertiary amine as a co-initiator. Specifically, type I photoinitiators can include acetophenone-based photoinitiators and benzoin-based photoinitiators. For example, acetophenone-based photoinitiators can include 4-phenoxydichloroacetophenone, 4-tert-butyldichloroacetophenone, 4-tert-butyltrichloroacetophenone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylacetone, 1(4-isopropylphenyl)-2-hydroxy-2-methylacetone, 1(4-dodecylphenyl)-2-hydroxy-2-methylacetone, 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl) ketone, 1-hydroxycyclohexylphenyl ketone, etc.; benzoin-based photoinitiators can include benzoin methyl ether, benzoin ethyl ether, benzyl dimethyl ketal, etc.; type I photoinitiators can also include acylphosphine oxides and titanium ether compounds. Type II photoinitiators can include benzophenone-based photoinitiators and thioxanone-based photoinitiators. For example, benzophenone-based photoinitiators can include benzophenone, benzoylbenzoic acid, benzoylbenzoic acid methyl ether, 4-phenylbenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3'-dimethyl-4-methoxybenzophenone, etc.; thioxanone-based photoinitiators can include thioxanone, 2-chlorothioxanone, 2-methylthioxanone, 2,4-dimethylthioxanone, isopropylthioxanone, etc. Furthermore, the photoinitiator can be at least one of the above-mentioned photoinitiators.
[0102] In this invention, the optical thin film material comprises 10 to 30 parts by mass of an active diluent and 1 to 10 parts by mass of a photoinitiator.
[0103] In step S20, the optical thin film materials are mixed to form a mixture.
[0104] Then, the above mixture is used for coating to obtain an intermediate film; specifically, roller coating, such as micro-grooving roller coating, can be used.
[0105] Next, the intermediate film is cured to obtain the optical film. Specifically, ultraviolet light curing can be used for film formation, and the energy of the ultraviolet light can be 500–1000 mJ / cm. 2 .
[0106] It is understood that during the curing process described above, the first compound, the second compound, and the third compound can undergo cross-linking polymerization to obtain a polymer, which is then cured to form an optical film.
[0107] In the embodiments of the present invention, the first and second compounds have more aromatic rings and / or sulfur atoms, which can significantly improve the refractive index of the optical film. The third compound contains aromatic rings, which can improve the refractive index of the optical film to a certain extent. In addition, the third compound has more acryloyloxy groups, which can improve the crosslinking degree of the polymer in the optical film, thereby improving the stability and durability of the optical film.
[0108] In this embodiment of the invention, the refractive index of the optical thin film can be greater than or equal to 1.5 and less than or equal to 1.8.
[0109] Furthermore, in this embodiment of the invention, the components of the optical thin film material are selected, and the refractive index of the prepared optical thin film is verified using the above preparation method, so as to obtain 7 embodiments as shown in Table 2 below.
[0110] Table 2: Refractive Index Verification Results
[0111]
[0112] As can be seen from the seven embodiments in Table 2, the optical thin film material provided by the embodiments of the present invention can effectively improve the refractive index of the optical thin film to obtain an optical thin film with a high refractive index.
[0113] In addition, embodiments of the present invention also provide a display panel, the display panel including an optical thin film, and the optical thin film is an optical thin film prepared by the optical thin film preparation method described in the above embodiments.
[0114] The display panel can be an organic light-emitting diode (OLED) display panel.
[0115] In one embodiment, the display panel includes an encapsulation layer, which includes the optical film. The optical film can improve the light extraction effect inside the organic light-emitting device and can also be reused as an encapsulation film layer.
[0116] In one embodiment, please refer to Figure 2 The display panel 10 includes an anti-reflection and anti-reflection film 12 disposed on the light-emitting surface of the panel body 11. The anti-reflection and anti-reflection film 12 includes a substrate layer 121 disposed on the light-emitting surface of the panel body 11, an optical film 122 disposed on the side of the substrate layer 121 away from the panel body 11, and a low refractive index layer 123 disposed on the side of the optical film 122 away from the substrate layer 121. The optical film 122 has a higher refractive index, while the refractive index of the low refractive index layer 123 is lower than that of the optical film 122.
[0117] In summary, the embodiments of the present invention form aromatic rings and / or sulfur atoms in the optical thin film material. Both aromatic rings and sulfur atoms can effectively increase the refractive index of the polymer. Therefore, the optical thin film material provided by the embodiments of the present invention can form an optical thin film with a high refractive index. Furthermore, the optical thin film material does not contain halogen atoms or added metal oxide nanoparticles, thus avoiding the phenomenon of being restricted in use due to toxicity and corrosive gases generated during combustion, and eliminating the adverse effects of nanoparticles on light scattering.
[0118] In the above embodiments, the descriptions of each embodiment have different focuses. For parts not described in detail in a certain embodiment, please refer to the relevant descriptions in other embodiments.
[0119] The foregoing has provided a detailed description of an optical thin film material, a method for preparing an optical thin film, and a display panel provided by the embodiments of the present invention. Specific examples have been used to illustrate the principles and implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the technical solutions and core ideas of the present invention. Those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. These modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An optical thin film material, characterized in that, The optical thin film material comprises 50-100 parts by mass of a first compound, 0-50 parts by mass of a second compound, 0-50 parts by mass of a third compound, 10-30 parts by mass of an active diluent, and 1-10 parts by mass of a photoinitiator. The optical thin film material does not contain halogen atoms or metal oxide nanoparticles. The structural formula of the first compound is shown below: ; The structural formula of the second compound is shown below: ; The structural formula of the third compound is shown below: 。 2. The optical thin film material according to claim 1, characterized in that, The reactive diluent includes a reactive diluent containing a monofunctional group or a reactive diluent containing a difunctional group, and the photoinitiator includes a type I photoinitiator and / or a type II photoinitiator.
3. A method for preparing an optical thin film, characterized in that, The optical thin film is prepared using the optical thin film material as described in claim 1 or 2, and the preparation method includes the following steps: Provide the optical thin film material; The optical thin film materials are mixed to form a mixture; The mixture is used for coating to obtain an intermediate film; The intermediate film is cured to obtain the optical film.
4. The method for preparing an optical thin film according to claim 3, characterized in that, The refractive index of the optical thin film is greater than or equal to 1.5 and less than or equal to 1.
8.
5. A display panel, characterized in that, The display panel includes an optical thin film, which is prepared by the optical thin film preparation method as described in any one of claims 3 to 4.
Citation Information
Patent Citations
Compound, polymerizable composition, polymer, holographic recording medium, optical material, and optical member
CN114616228A
High-refraction UV light-cured polyurethane acrylate resin and preparation method thereof
CN114685748A
Triazine ring-containing polymer
JP2014169463A
Optical resin composition
US7473754B1