Low-temperature-resistant modified PC material and production process thereof
By introducing core-shell structured low-temperature toughening agents and UV absorbers into PC materials, the problems of embrittlement and UV damage of polycarbonate at low temperatures are solved, and the material achieves high toughness and UV resistance at extreme low temperatures.
Patent Information
- Application Number
- CN202411329950.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polycarbonate materials exhibit a significant decrease in toughness at extreme low temperatures, making them prone to embrittlement and cracking. Additionally, under ultraviolet radiation, the material surface shows cracks and photoaging phenomena, and traditional coatings exhibit poor stability.
PC materials are modified with low-temperature toughening agents and ultraviolet absorbers. By synthesizing intermediates containing isocyanate groups and core-shell toughening agents with Si-O bonds, and combining them with benzotriazole intermediates and ultraviolet absorbers with sulfone groups, the low-temperature toughness and ultraviolet resistance of the materials are enhanced.
It improves the toughness and impact resistance of PC materials at extreme low temperatures, reduces UV damage, and extends service life.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a low-temperature resistant modified PC material and a production process thereof. Background Art
[0002] With the rapid progress of science and technology and the vigorous development of industry, polycarbonate (PC), as a thermoplastic engineering plastic with excellent comprehensive performance, has shown increasingly extensive application potential in many fields such as automobile manufacturing, electronic equipment, and medical equipment. With the growth of demand in extreme low temperature environments, the development of low-temperature resistant PC materials has important practical significance and application value.
[0003] Polycarbonate has high transparency, good toughness and weather resistance at room temperature due to the carbonate-based structure in the molecular chain. However, as the temperature decreases, the molecular chain activity of polycarbonate is restricted, and the PC material will change from a highly elastic state to a glassy state, resulting in a significant decrease in the toughness of the material, and it is prone to embrittlement and cracking, which limits its application under low temperature conditions. At the same time, traditional PC materials are prone to molecular chain breakage or structural changes under ultraviolet irradiation, resulting in cracks and light aging on the surface of the material, causing serious losses. At present, the method used to make PC materials resistant to ultraviolet rays is surface coating, but it has poor stability and is easy to scratch. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a low-temperature resistant modified PC material and a production process thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions: A low-temperature resistant modified PC material, comprising the following raw materials in parts by weight: 90-100 parts of PC base, 4-8 parts of low-temperature resistant toughening agent, 0.8-1.2 parts of ultraviolet absorber, 0.3-0.5 parts of antioxidant, and 0.3-0.5 parts of lubricant; The PC-based material is bisphenol A polycarbonate with a melt flow rate of 10-20 g / 10 min; The antioxidant is antioxidant 412S; The lubricant is pentaerythritol stearate.
[0006] The low temperature resistant toughening agent is prepared by the following method: Step A1: Evenly mix pentamethyldisiloxane and vinyl isocyanate, heat to 60-80°C, add chloroplatinic acid and stir evenly, heat to 115°C under nitrogen protection, react for 7h, reduce pressure and distill to obtain an intermediate. The reaction route can be expressed as follows:
[0007] Further, the molar ratio of pentamethyldisiloxane, vinyl isocyanate, and chloroplatinic acid is 1:1.2:0.5; Step A2: Mix dodecylbenzenesulfonic acid and water, raise the temperature to 45°C, stir evenly, then add decamethylcyclopentasiloxane, 3-trimethoxysilane acrylate and the intermediate, mix evenly, and react for 3h to obtain product a. The reaction route can be expressed as follows:
[0008] Further, the amount ratio of decamethylcyclopentasiloxane, water, 3-trimethoxysilane acrylate, and the intermediate is 3-5 mol: 45 mL: 5-7 mol: 5-7 mol, and the amount of dodecylbenzenesulfonic acid accounts for 1.4% of the total amount of water in the system; Step A3: Ethyl acrylate, butylene glycol dimethacrylate, dodecanethiol and product a are mixed, nitrogen is passed through to protect, the pH is adjusted to 7-8, 1 / 2 potassium persulfate is added, the reaction is performed for 1-2 hours, methyl methacrylate and 1 / 2 potassium persulfate are added, the reaction is performed for 2.5 hours, and the mixture is frozen, thawed, demulsified, washed, filtered, and dried at 80°C to obtain a low-temperature resistant toughening agent; Furthermore, the mass ratio of ethyl acrylate, butylene glycol dimethacrylate, dodecanethiol, product a, total amount of potassium persulfate, and methyl methacrylate is 120-200:45-60:3-4:90-120:10:45-60.
[0009] The ultraviolet absorber is prepared by the following method: Step B1: o-aminophenol, sodium nitrite, copper sulfate pentahydrate and concentrated hydrochloric acid are mixed, stirred in an ice-salt bath at 0-5°C, the pH is adjusted to 7-8, m-phenylenediamine is added, the temperature is raised to 25°C, the reaction is performed for 2h, filtered, and finally 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole and dioxane are added, the mixture is stirred, filtered, decompressed and distilled to obtain a benzotriazole intermediate; Further, the dosage ratio of o-aminophenol, sodium nitrite, copper sulfate pentahydrate, concentrated hydrochloric acid, m-phenylenediamine, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, and dioxane is: 1-1.5 g: 0.69 g: 1.05-1.19 g: 3 mL: 6.0 g: 3.51-4.05 g: 10-20 mL; Step B2: Mix 4,6-diisopentyloxy-1,3-benzenedisulfonyl chloride, benzotriazole intermediate, acetone and triethylamine, stir at room temperature for 2-3 hours, rotary evaporate, wash and dry to obtain a UV absorber; Furthermore, the usage ratio of 4,6-diisopentyloxy-1,3-benzenedisulfonyl chloride, benzotriazole intermediate, acetone and triethylamine is 0.854-0.935 g: 0.580 g: 20 mL: 0.5-0.6 mL.
[0010] A production process of low temperature resistant modified PC material, specifically comprising the following steps: Step S1: adding the PC substrate into a mixer, adding dispersing oil, and stirring evenly to obtain a pre-dispersed mixture; Step S2: adding a low temperature resistant toughening agent, an antioxidant, an ultraviolet absorber and a lubricant to the pre-dispersed mixture and continuing to stir evenly to obtain a mixed base material; Step S3: placing the mixed base material in a twin-screw extruder at 200°C-240°C for extrusion granulation, the extruder screw speed is 120r / min, and then drying at 120°C for 4h to obtain a low-temperature resistant modified PC material; Furthermore, in step S1, the dispersing oil is methyl silicone oil.
[0011] Beneficial effects of the present invention: The low temperature resistant toughening agent prepared by the present invention is firstly prepared by adding Si-H of pentamethyldisiloxane and carbon-carbon double bond of vinyl isocyanate under the action of chloroplatinic acid as a catalyst to synthesize an intermediate containing an isocyanate group; secondly, dodecylbenzenesulfonic acid is used to ionize H + , the decamethylcyclopentasiloxane is ring-opened to form a growth chain, which is then condensed with hydrolyzable 3-trimethoxysilane acrylate, and finally grafted to synthesize a core-shell structure low-temperature toughening agent with product a as the core layer, ethyl acrylate as the transition layer, and methyl methacrylate as the shell layer. The isocyanate group in the low-temperature toughening agent has good reactivity due to its highly unsaturated characteristics. It can react with the ester group to make the molecules tightly bonded, increase internal cohesion, thereby reducing crack formation, and further improving toughness and impact resistance; the Si-O bond contained therein can remain stable at low temperatures due to its high bond energy and long bond length, and is not easy to break, giving the toughening agent good low-temperature resistance; the polyacrylate contained in it lacks cross-linking between molecules due to the increase in temperature, is easy to slide and become sticky, and has good bonding properties. Therefore, the low-temperature toughening agent formed by the combination not only has good low-temperature resistance and crack resistance, but also has good low-temperature toughness and impact resistance.
[0012] The ultraviolet absorber prepared by the present invention is prepared by reacting a compound synthesized from o-aminophenol, sodium nitrite and m-phenylenediamine with 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole to obtain a benzotriazole intermediate, and then the hydroxyl group of the benzotriazole intermediate reacts with the chlorine of 4,6-diisopentyloxy-1,3-benzenedisulfonyl chloride to synthesize the ultraviolet absorber. The ultraviolet absorber has a sulfone structure, which, as an electron-donating and withdrawing group, can promote charge transfer within the molecule, so that electrons in the material molecule can flow and thus absorb light. At the same time, 4,6-diisopentyloxy-1,3-benzenedisulfonyl chloride forms a larger conjugated system with a benzene ring, thereby increasing the light absorption capacity. In addition, the conjugated double bonds and aromatic rings of the benzotriazole intermediate can efficiently absorb ultraviolet rays in different wavelength ranges, and convert ultraviolet energy into heat energy or light energy, thereby reducing the damage of ultraviolet rays to PC materials.
[0013] The low-temperature resistant modified PC material prepared by the present invention not only has excellent low-temperature toughness and impact resistance, but also can reduce the loss caused by ultraviolet rays, extend the service life of the product, and still maintain good toughness in extreme low-temperature environments, providing strong support for the innovation and development of various industries, making it have broad application prospects in the fields of automobiles, electronics, and medical treatment. DETAILED DESCRIPTION
[0014] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0015] A production process of low temperature resistant modified PC material, specifically comprising the following steps: Step S1: adding the PC substrate into a mixer, adding dispersing oil, and stirring evenly to obtain a pre-dispersed mixture; Step S2: adding a low temperature resistant toughening agent, an antioxidant, an ultraviolet absorber and a lubricant to the pre-dispersed mixture and continuing to stir evenly to obtain a mixed base material; Step S3: placing the mixed base material in a twin-screw extruder at 200° C. for granulation, with the extruder screw speed being 120 r / min, and then drying at 120° C. for 4 h to obtain a low-temperature resistant modified PC material; The low temperature resistant toughening agent is prepared by the following method: Step A1: 1 mol of pentamethyldisiloxane and 1.2 mol of vinyl isocyanate are mixed evenly, the temperature is raised to 60-80°C, 0.5 mol of chloroplatinic acid is added and stirred evenly, the temperature is raised to 115°C under nitrogen protection, the reaction is carried out for 7 hours, the pressure is reduced, and distillation is performed to obtain an intermediate; Step A2: Mix dodecylbenzenesulfonic acid and 45 mL of water, raise the temperature to 45°C, stir evenly, then add 3 mol of decamethylcyclopentasiloxane, 5 mol of 3-trimethoxysilane acrylate and 5 mol of the intermediate, mix evenly, and react for 3 hours to obtain product a. The amount of dodecylbenzenesulfonic acid used accounts for 1.4% of the total amount of water in the system; Step A3: 120g of ethyl acrylate, 45g of butylene glycol dimethacrylate, 3g of dodecanethiol and 90g of product a are mixed, nitrogen is passed through, the pH is adjusted to 7-8, 5g of potassium persulfate is added, and the reaction is carried out for 1-2h, and 45g of methyl methacrylate and 5g of potassium persulfate are added, and the reaction is carried out for 2.5h, and the mixture is frozen, thawed, demulsified, washed, filtered, and dried at 80°C to obtain a low-temperature resistant toughening agent; The ultraviolet absorber is prepared by the following method: Step B1: 1 g of o-aminophenol, 0.69 g of sodium nitrite, 1.05 g of copper sulfate pentahydrate and 3 mL of concentrated hydrochloric acid were mixed, stirred in an ice-salt bath at 0-5°C, the pH was adjusted to 7-8, 6.0 g of m-phenylenediamine was added, the temperature was raised to 25°C, the reaction was performed for 2 h, and the mixture was filtered. Finally, 3.51 g of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole and 10 mL of dioxane were added, the mixture was stirred, filtered, decompressed and distilled to obtain a benzotriazole intermediate; Step B2: Mix 0.854 g of 4,6-diisopentyloxy-1,3-benzenedisulfonyl chloride, 0.580 g of benzotriazole intermediate, 20 mL of acetone and 0.5 mL of triethylamine, stir at room temperature for 2-3 h, rotary evaporate, wash and dry to obtain a UV absorber. Example 2
[0016] A production process of low temperature resistant modified PC material, specifically comprising the following steps: Step S1: adding the PC substrate into a mixer, adding dispersing oil, and stirring evenly to obtain a pre-dispersed mixture; Step S2: adding a low temperature resistant toughening agent, an antioxidant, an ultraviolet absorber and a lubricant to the pre-dispersed mixture and continuing to stir evenly to obtain a mixed base material; Step S3: placing the mixed base material in a twin-screw extruder at 220° C. for granulation, with the extruder screw speed being 120 r / min, and then drying at 120° C. for 4 h to obtain a low-temperature resistant modified PC material; The low temperature resistant toughening agent is prepared by the following method: Step A1: 1 mol of pentamethyldisiloxane and 1.2 mol of vinyl isocyanate are mixed evenly, the temperature is raised to 60-80°C, 0.5 mol of chloroplatinic acid is added and stirred evenly, the temperature is raised to 115°C under nitrogen protection, the reaction is carried out for 7 hours, the pressure is reduced, and distillation is performed to obtain an intermediate; Step A2: Mix dodecylbenzenesulfonic acid and 45 mL of water, raise the temperature to 45°C, stir evenly, then add 4 mol of decamethylcyclopentasiloxane, 6 mol of 3-trimethoxysilane acrylate and 6 mol of the intermediate, mix evenly, and react for 3 hours to obtain product a. The amount of dodecylbenzenesulfonic acid used accounts for 1.4% of the total amount of water in the system; Step A3: 160g of ethyl acrylate, 52g of butylene glycol dimethacrylate, 3.5g of dodecanethiol and 105g of product a are mixed, nitrogen is passed through, the pH is adjusted to 7-8, 5g of potassium persulfate is added, and the reaction is carried out for 1-2h, and 52g of methyl methacrylate and 5g of potassium persulfate are added, and the reaction is carried out for 2.5h, and the mixture is frozen, thawed, demulsified, washed, filtered, and dried at 80°C to obtain a low-temperature resistant toughening agent; The ultraviolet absorber is prepared by the following method: Step B1: 1.25 g of o-aminophenol, 0.69 g of sodium nitrite, 1.12 g of copper sulfate pentahydrate and 3 mL of concentrated hydrochloric acid were mixed, stirred in an ice-salt bath at 0-5°C, the pH was adjusted to 7-8, 6.0 g of m-phenylenediamine was added, the temperature was raised to 25°C, the reaction was performed for 2 h, and the mixture was filtered. Finally, 3.78 g of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole and 10-20 mL of dioxane were added, the mixture was stirred, filtered, decompressed and distilled to obtain a benzotriazole intermediate; Step B2: Mix 0.894 g of 4,6-diisopentyloxy-1,3-benzenedisulfonyl chloride, 0.580 g of benzotriazole intermediate, 20 mL of acetone and 0.55 mL of triethylamine, stir at room temperature for 2-3 h, rotary evaporate, wash and dry to obtain a UV absorber. Example 3
[0017] A production process of low temperature resistant modified PC material, specifically comprising the following steps: Step S1: adding the PC substrate into a mixer, adding dispersing oil, and stirring evenly to obtain a pre-dispersed mixture; Step S2: adding a low temperature resistant toughening agent, an antioxidant, an ultraviolet absorber and a lubricant to the pre-dispersed mixture and continuing to stir evenly to obtain a mixed base material; Step S3: placing the mixed base material in a twin-screw extruder at 240° C. for granulation, with the extruder screw speed being 120 r / min, and then drying at 120° C. for 4 h to obtain a low-temperature resistant modified PC material; The low temperature resistant toughening agent is prepared by the following method: Step A1: 1 mol of pentamethyldisiloxane and 1.2 mol of vinyl isocyanate are mixed evenly, the temperature is raised to 60-80°C, 0.5 mol of chloroplatinic acid is added and stirred evenly, the temperature is raised to 115°C under nitrogen protection, the reaction is carried out for 7 hours, the pressure is reduced, and distillation is performed to obtain an intermediate; Step A2: Mix dodecylbenzenesulfonic acid and 45 mL of water, raise the temperature to 45°C, stir evenly, then add 5 mol of decamethylcyclopentasiloxane, 7 mol of 3-trimethoxysilane acrylate and 7 mol of the intermediate, mix evenly, and react for 3 hours to obtain product a. The amount of dodecylbenzenesulfonic acid used accounts for 1.4% of the total amount of water in the system; Step A3: 200g of ethyl acrylate, 60g of butylene glycol dimethacrylate, 4g of dodecanethiol and 120g of product a are mixed, nitrogen is passed through, the pH is adjusted to 7-8, 5g of potassium persulfate is added, and the reaction is carried out for 1-2h, and 60g of methyl methacrylate and 5g of potassium persulfate are added, and the reaction is carried out for 2.5h, and the mixture is frozen, thawed, demulsified, washed, filtered, and dried at 80°C to obtain a low-temperature resistant toughening agent; The ultraviolet absorber is prepared by the following method: Step B1: 1.5 g of o-aminophenol, 0.69 g of sodium nitrite, 1.19 g of copper sulfate pentahydrate and 3 mL of concentrated hydrochloric acid were mixed, stirred in an ice-salt bath at 0-5°C, the pH was adjusted to 7-8, 6.0 g of m-phenylenediamine was added, the temperature was raised to 25°C, the reaction was performed for 2 h, and the mixture was filtered. Finally, 4.05 g of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole and 20 mL of dioxane were added, the mixture was stirred, filtered, decompressed and distilled to obtain a benzotriazole intermediate; Step B2: Mix 0.935 g of 4,6-diisopentyloxy-1,3-benzenedisulfonyl chloride, 0.580 g of benzotriazole intermediate, 20 mL of acetone and 0.6 mL of triethylamine, stir at room temperature for 2-3 h, rotary evaporate, wash and dry to obtain a UV absorber.
[0018] Comparative Example 1 This comparative example is a low-temperature resistant modified PC material. The difference from Example 3 is that an equal amount of toughening agent S-2030 is used to replace the low-temperature resistant toughening agent prepared in Example 3, and the rest are the same.
[0019] Comparative Example 2 This comparative example is a low-temperature resistant modified PC material, which differs from Example 3 in that an equal amount of ultraviolet blocker nano barium sulfate is used to replace the ultraviolet absorber prepared in Example 3, and the rest are the same.
[0020] Performance test: The low-temperature resistant modified PC materials prepared in Examples 1-3 and Comparative Examples 1-2 were cut into standard test sizes, and the bending strength test was performed at temperatures of 25°C and -30°C according to ASTM D790-2003; The low-temperature resistant modified PC materials prepared in Examples 1-3 and Comparative Examples 1-2 were cut into standard test sizes, and a UVC-LED disinfection lamp (30W, 254nm wavelength) was used to irradiate for 40 hours at a vertical distance of 10cm, and the color difference before and after UVC-LED irradiation was detected according to CIE1976L*a*b* standard and the impact strength test was performed according to GB104393; the test results are shown in the following table:
[0021] It can be seen from the test data in the table that the low-temperature resistant modified PC material prepared in Example 1 still has a bending strength of more than 80% at room temperature at a temperature of -30°C, and has excellent low-temperature toughness. It can also be seen from the above table that the low-temperature resistant modified PC material prepared by the present invention has good impact resistance and UV resistance.
[0022] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A production process of low temperature resistant modified PC material, characterized in that: The following steps are involved: Step S1: adding the PC substrate into a mixer, adding dispersing oil, and stirring evenly to obtain a pre-dispersed mixture; Step S2: adding a low temperature resistant toughening agent, an antioxidant, an ultraviolet absorber and a lubricant to the pre-dispersed mixture and continuing to stir evenly to obtain a mixed base material; Step S3: placing the mixed base material in a twin-screw extruder at 200°C-240°C for extrusion granulation, with the extruder screw speed being 120r / min, and then drying at 120°C for 4h to obtain a low-temperature resistant modified PC material.
2. The production process of a low-temperature resistant modified PC material according to claim 1, characterized in that: The low temperature resistant toughening agent is prepared by the following method: Step A1: Evenly mix pentamethyldisiloxane and vinyl isocyanate, heat to 60-80°C, add chloroplatinic acid and stir evenly, heat to 115°C under nitrogen protection, react for 7h, reduce pressure and distill to obtain an intermediate; Step A2: dodecylbenzenesulfonic acid and water are mixed, the temperature is raised to 45°C, and stirred evenly, and then decamethylcyclopentasiloxane, 3-trimethoxysilane acrylate and the intermediate are added and mixed evenly, and the reaction is carried out for 3 hours to obtain product a; Step A3: Ethyl acrylate, butylene glycol dimethacrylate, dodecanethiol and product a are mixed, nitrogen is passed through to protect, the pH is adjusted to 7-8, and then 1 / 2 potassium persulfate is added, and the reaction is carried out for 1-2 hours. Methyl methacrylate and 1 / 2 potassium persulfate are added, and the reaction is carried out for 2.5 hours. The mixture is frozen, thawed, demulsified, washed, filtered, and dried at 80°C to obtain a low-temperature resistant toughening agent.
3. The production process of a low temperature resistant modified PC material according to claim 2, characterized in that: In step A1, the molar ratio of pentamethyldisiloxane, vinyl isocyanate and chloroplatinic acid is 1:1.2:0.
5.
4. The production process of a low temperature resistant modified PC material according to claim 2, characterized in that: In step A2, the usage ratio of decamethylcyclopentasiloxane, water, 3-trimethoxysilane propyl acrylate and the intermediate is 3-5 mol:45 mL:5-7 mol:5-7 mol, and the usage of dodecylbenzenesulfonic acid accounts for 1.4% of the total amount of water in the system.
5. The production process of a low temperature resistant modified PC material according to claim 2, characterized in that: In step A3, the mass ratio of ethyl acrylate, butylene glycol dimethacrylate, dodecanethiol, product a, total amount of potassium persulfate, and methyl methacrylate is 120-200:45-60:3-4:90-120:10:45-60.
6. The production process of a low temperature resistant modified PC material according to claim 1, characterized in that: The ultraviolet absorber is prepared by the following method: Step B1: o-aminophenol, sodium nitrite, copper sulfate pentahydrate and concentrated hydrochloric acid are mixed, stirred in an ice-salt bath at 0-5°C, the pH is adjusted to 7-8, m-phenylenediamine is added, the temperature is raised to 25°C, the reaction is performed for 2h, filtered, and finally 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole and dioxane are added, the mixture is stirred, filtered, decompressed and distilled to obtain a benzotriazole intermediate; Step B2: Mix 4,6-diisopentyloxy-1,3-benzenedisulfonyl chloride, benzotriazole intermediate, acetone and triethylamine, stir at room temperature for 2-3 hours, rotary evaporate, wash and dry to obtain a UV absorber.
7. The production process of a low temperature resistant modified PC material according to claim 6, characterized in that: In step B1, the dosage ratio of o-aminophenol, sodium nitrite, copper sulfate pentahydrate, concentrated hydrochloric acid, m-phenylenediamine, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole and dioxane is: 1-1.5 g: 0.69 g: 1.05-1.19 g: 3 mL: 6.0 g: 3.51-4.05 g: 10-20 mL.
8. The production process of a low temperature resistant modified PC material according to claim 6, characterized in that: In step B2, the usage ratio of 4,6-diisopentyloxy-1,3-benzenedisulfonyl chloride, benzotriazole intermediate, acetone and triethylamine is 0.854-0.935 g: 0.580 g: 20 mL: 0.5-0.6 mL.
9. The production process of a low temperature resistant modified PC material according to claim 1, characterized in that: The antioxidant is antioxidant 412S, and the lubricant is pentaerythritol stearate.
10. A low temperature resistant modified PC material, characterized in that: Prepared according to the production process according to any one of claims 1 to 9.
Citation Information
Patent Citations
Protein reactive ultraviolet absorber and preparation method thereof
CN102619108A
High-transparency low-temperature-impact-resistant flame-retardant polycarbonate composite material and preparation method thereof
CN103788610A
Weather-resistant high-toughness polycarbonate composite material and preparation method thereof
CN114031923A
Anti-ultraviolet radiation-proof fabric and preparation method thereof
CN114592345A
Cited By
Weather-resistant coating for photovoltaic module and preparation method of weather-resistant coating
CN119592156A
Cold-resistant PBT plastic and preparation method thereof
CN119735926A