A method for preparing a nano-ceramic coating on the surface of marine aluminum alloy
By preparing a nano-ceramic coating on the surface of aluminum alloy, which combines carbon nanotube composite material with silica sol, the problems of hardness, wear resistance and corrosion resistance of aluminum alloy materials in marine environments were solved, and a nano-ceramic coating with high hardness and good wear resistance was achieved.
Patent Information
- Application Number
- CN202311297243.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-09
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-10-09
AI Technical Summary
Existing technologies are insufficient to effectively improve the hardness, wear resistance, and corrosion resistance of aluminum alloy materials in marine environments.
A nano-ceramic coating with high hardness, wear resistance, and corrosion resistance is formed by combining carbon nanotube composite materials with silica sol to prepare a nano-ceramic coating on the surface of aluminum alloy. The specific steps include pretreatment, functionalization of carbon nanotubes, zinc oxide sol composite, preparation of silica composite sol and coating and curing.
The prepared nano-ceramic coating has a hardness of up to 640-730 Hv, excellent wear resistance, good corrosion resistance, and a corrosion rate of 0.02-0.05 g/cm2, which significantly improves the overall performance of aluminum alloy.
Smart Images

Figure CN117463588B_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The application belongs to the technical field of alloy surface ceramic coating, and particularly relates to a marine aluminum alloy surface nano ceramic coating preparation method. BACKGROUND
[0002] The metal surface ceramic coating is a multifunctional inorganic nonmetal ceramic coating coated on the metal surface, which can change the metal surface performance and has the performance of inorganic ceramic compared with the traditional organic coating, metal and alloy coating.
[0003] At present, the metal-based ceramic coating has been greatly applied in the fields of aerospace, navigation, power electronics, mechanization and chemical industry. The ceramic coating has the excellent performance of inorganic ceramic, high hardness, strong wear resistance and corrosion resistance, and low manufacturing cost. The technology is an important means of material surface treatment, and after a small amount of inorganic material is added, the performance is improved, the processing cost is reduced, the product quality is controlled, the energy is saved, and the significance is great. The research and development of the metal surface ceramic coating combines the excellent performance of metal materials and ceramic materials, does not affect the excellent performance of the metal material such as electric conductivity and thermal conductivity, obtains the excellent corrosion resistance and wear resistance of the inorganic ceramic material, meets the needs of the product on the structure performance and environmental performance, and even special functions such as infrared radiation, wavelength absorption, heat sensitivity, light sensitivity and the like, and endows the material with quite ideal comprehensive performance. Therefore, the metal surface ceramic coating becomes one of the most realistic technologies for solving the poor heat resistance, poor wear resistance and easy corrosion of the metal material, and is paid more and more attention by people. SUMMARY
[0004] The application aims to provide a marine aluminum alloy surface nano ceramic coating preparation method with high hardness, good wear resistance and good corrosion resistance.
[0005] The technical scheme adopted by the application to achieve the above object is: The application discloses a marine aluminum alloy surface nano ceramic coating preparation method, which comprises the following steps: performing pretreatment on the surface of an aluminum alloy base material to remove a surface layer to obtain a pretreated aluminum alloy base material; performing dip coating on the pretreated aluminum alloy base material in a silicon oxide composite sol and performing solidification treatment to obtain an aluminum alloy surface nano ceramic coating; and the silicon oxide composite sol contains a carbon nanotube composite material, the carbon nanotube composite material is prepared by adding functionalized carbon nanotubes into a zinc oxide sol, and the functionalized carbon nanotubes are generated by the reaction of carboxylated carbon nanotubes and ethanolamine phosphate. After the functionalized carbon nanotubes are prepared, the carbon nanotube composite material is prepared by the reaction of the functionalized carbon nanotubes and the zinc oxide sol, the carbon nanotube composite material is reacted with tetraethyl orthosilicate in a glycerol solution, a polyvinyl alcohol solution and an ethanol solution to prepare the silicon oxide composite sol, and after the dip coating and the nano ceramic coating are formed, it is found that the nano ceramic coating prepared by the above method has high hardness and good wear resistance and corrosion resistance.
[0006] Preferably, the pretreatment comprises wet grinding by sandpaper, alkaline washing by an alkaline solution and acid washing by an acidic solution.
[0007] Preferably, the zinc oxide sol contains 0.3-0.8wt% of zinc reagent.
[0008] More preferably, the zinc reagent is zinc acetate.
[0009] Preferably, the amount of the functionalized carbon nanotubes is 20-100wt% of the zinc oxide sol.
[0010] Preferably, the silicon oxide composite sol is prepared by mixing a tetraethyl orthosilicate solution, a polyvinyl alcohol solution, the carbon nanotube composite material and an alcohol solution.
[0011] More preferably, the tetraethyl orthosilicate solution contains 50-70wt% of tetraethyl orthosilicate, and the polyvinyl alcohol solution contains 6-14wt% of polyvinyl alcohol.
[0012] More preferably, the amount of the glycerol is 20-40wt% of the tetraethyl orthosilicate solution, and the amount of the polyvinyl alcohol solution is 20-40wt% of the tetraethyl orthosilicate solution.
[0013] More preferably, the amount of the carbon nanotube composite material is 2-6wt% of the tetraethyl orthosilicate solution.
[0014] More preferably, the alcohol solution contains ethanol and glycerol.
[0015] Preferably, in the pretreatment of the aluminum alloy substrate, the surface layer of the substrate is removed by wet sanding with sandpaper, then washed with ethanol, and after washing and drying, it is alkaline washed with an alkaline solution at a temperature of 60-80°C for 20-60 minutes. After alkaline washing, it is washed with deionized water until neutral, and then acid-washed with an acidic solution at a temperature of 20-40°C for 20-60 minutes. After acid washing, it is washed with deionized water until neutral, rinsed with acetone, and then dried to obtain the pretreated aluminum alloy substrate.
[0016] More preferably, in the pretreatment of the aluminum alloy substrate, the alkaline solution is sodium hydroxide with a mass fraction of 1-3 wt%.
[0017] More preferably, in the pretreatment of the aluminum alloy substrate, the acidic solution is nitric acid with a mass fraction of 4-12 wt%.
[0018] Preferably, in the preparation of carboxylated carbon nanotubes, carbon nanotubes are added to a mixed acid solution, ultrasonically treated for 20-60 min, and then stirred at 50-80℃ for 0.5-4 h. After removing the carbon nanotubes, they are washed with anhydrous ethanol, then washed with deionized water until neutral, dried, and ground to obtain carboxylated carbon nanotubes.
[0019] More preferably, in the preparation of carboxylated carbon nanotubes, the mixed acid solution is a mixture of concentrated sulfuric acid and concentrated nitric acid, and the amount of concentrated nitric acid used in the mixed acid solution is 20-40 wt% of the amount of concentrated sulfuric acid.
[0020] More preferably, in the preparation of carboxylated carbon nanotubes, the amount of carbon nanotubes used is 0.1-0.5 wt% of the mixed acid solution.
[0021] Preferably, in the preparation of functionalized carbon nanotubes, carboxylated carbon nanotubes and ethanolamine phosphate are added to DMF, stirred and mixed under nitrogen protection for 20-60 min, DCC solution is added, and the reaction is carried out at 20-40℃ for 48-96 h. After the reaction is completed, the mixture is filtered, washed, dried, and ground to obtain functionalized carbon nanotubes.
[0022] More preferably, in the preparation of functionalized carbon nanotubes, the amount of carboxylated carbon nanotubes used is 0.2-0.6 wt% of DMF.
[0023] More preferably, in the preparation of functionalized carbon nanotubes, the amount of ethanolamine phosphate used is 1-4 wt% of the carboxylated carbon nanotubes.
[0024] More preferably, in the preparation of functionalized carbon nanotubes, the DCC solution is obtained by dissolving DCC in THF, and the DCC solution contains 12-18 wt% DCC.
[0025] More preferably, in the preparation of functionalized carbon nanotubes, the amount of DCC solution used is 20-40 wt% of DMF.
[0026] Preferably, in the preparation of the carbon nanotube composite material, zinc reagent and deionized water are added to diethylene glycol and stirred at 160-180°C for 3-10 min. Then, the mixture is allowed to stand at 20-40°C for 1-4 h to obtain zinc oxide sol. Functionalized carbon nanotubes are added and ultrasonically mixed to obtain a carbon nanotube composite liquid. The liquid is stirred at 170-190°C for 1-5 h. After cooling to room temperature, the supernatant is removed by centrifugation. The mixture is then washed, dried, and ground to obtain the carbon nanotube composite material.
[0027] More preferably, in the preparation of carbon nanotube composite materials, the zinc reagent is zinc acetate, and the zinc oxide sol contains 0.3-0.8 wt% zinc reagent.
[0028] More preferably, in the preparation of carbon nanotube composite materials, the amount of deionized water used is 800-1200 wt% of zinc reagent.
[0029] More preferably, in the preparation of carbon nanotube composite materials, the amount of functionalized carbon nanotubes used is 20-100 wt% of zinc oxide sol.
[0030] Preferably, in the preparation of the silica composite sol, an ethanol solution and an orthosilicate solution are mixed, glycerol is added, the pH of the solution is adjusted to 2-3, and the mixture is stirred for 20-60 min. Then, a polyvinyl alcohol solution is added, and the mixture is stirred at 60-80°C for 6-12 h. Finally, carbon nanotube composite material is added, and the mixture is stirred at 60-80°C for 6-12 h. The mixture is then aged at 20-40°C for more than 24 h to obtain the silica composite sol.
[0031] More preferably, in the preparation of silica composite sol, the ethanol solution contains 70-90 wt% ethanol.
[0032] More preferably, in the preparation of the silica composite sol, the tetraethyl orthosilicate solution is obtained by adding tetraethyl orthosilicate to deionized water, and the tetraethyl orthosilicate solution contains 50-70 wt% tetraethyl orthosilicate.
[0033] More preferably, in the preparation of silica composite sol, the amount of ethanol solution used is 150-300 wt% of tetraethyl orthosilicate.
[0034] More preferably, in the preparation of silica composite sol, the amount of glycerol used is 20-40 wt% of the tetraethyl orthosilicate solution.
[0035] More preferably, in the preparation of the silica composite sol, the polyvinyl alcohol solution contains 6-14 wt% polyvinyl alcohol, and the amount of polyvinyl alcohol solution used is 20-40 wt% of the tetraethyl orthosilicate solution.
[0036] More preferably, in the preparation of silica composite sol, the amount of carbon nanotube composite material used is 2-6 wt% of tetraethyl orthosilicate solution.
[0037] Preferably, aluminum dihydrogen phosphate can be added during the preparation of the silica composite sol, with the amount of aluminum dihydrogen phosphate being 0.6-2 wt% of the tetraethyl orthosilicate solution. After adding aluminum dihydrogen phosphate to the silica composite sol for preparing the nano-ceramic coating, the performance of the prepared nano-ceramic coating is improved in the presence of the carbon nanotube composite material, with enhanced hardness, wear resistance, and corrosion resistance.
[0038] Preferably, in the sol coating process, the pretreated aluminum alloy is immersed in the silica composite sol and coated at least 3 times. The first coating time is 60-120s, the remaining coating time is 15-45s, the interval between each coating is 30-120min, and the coating speed is 3-10cm / min.
[0039] Preferably, in the preparation of the nano-ceramic coating on the aluminum alloy surface, the aluminum alloy coated with silica composite sol is treated at a temperature of 90-120℃ for 30-120 min, and then cured at a temperature of 200-400℃ to obtain an aluminum alloy with a nano-ceramic coating on the surface.
[0040] This invention utilizes the reaction of carboxylated carbon nanotubes with ethanolamine phosphate to prepare functionalized carbon nanotubes, then adds these functionalized carbon nanotubes to zinc oxide sol to prepare a carbon nanotube composite material, and finally uses this composite material to prepare a silica composite sol. After coating and high-temperature curing, a nano-ceramic coating is obtained. Therefore, this invention offers the following advantages: the nano-ceramic coating prepared by this invention has high hardness (640-730 Hv); good wear resistance; and good corrosion resistance (0.02-0.05 g / cm³). 2 Therefore, this invention provides a method for preparing a nano-ceramic coating on the surface of marine aluminum alloys, which exhibits high hardness, good wear resistance, and good corrosion resistance. Attached Figure Description
[0041] Figure 1 Infrared spectrum of functionalized carbon nanotubes; Figure 2 Hardness diagram of nano-ceramic coating; Figure 3 This is a diagram showing the wear of the nano-ceramic coating. Figure 4 This is a graph showing the corrosion rate of the nano-ceramic coating. Detailed Implementation
[0042] The technical solution of the present invention will be further described in detail below with reference to specific embodiments and accompanying drawings: Example 1: A method for preparing a nano-ceramic coating on the surface of marine aluminum alloys. Pretreatment of the aluminum alloy substrate: The surface layer of the substrate was removed by wet sanding with sandpaper, followed by washing with ethanol. After washing and drying with ethanol, the substrate was alkaline-washed with an alkaline solution at 80°C for 40 minutes. After alkaline washing, it was washed with deionized water until neutral. Then, it was acid-washed with an acidic solution at 30°C for 40 minutes. After acid washing, it was washed with deionized water until neutral. After rinsing with acetone, it was dried to obtain the pretreated aluminum alloy substrate. The alkaline solution was 2 wt% sodium hydroxide, and the acidic solution was 8 wt% nitric acid.
[0043] Preparation of carboxylated carbon nanotubes: Carbon nanotubes were added to a mixed acid solution and sonicated for 40 min, then stirred at 60 °C for 2 h. After removing the carbon nanotubes, they were washed with anhydrous ethanol, then washed with deionized water until neutral, dried, and ground to obtain carboxylated carbon nanotubes. The mixed acid solution was a mixture of concentrated sulfuric acid and concentrated nitric acid, with the amount of concentrated nitric acid in the mixed acid solution being 30 wt% of the amount of concentrated sulfuric acid, and the amount of carbon nanotubes being 0.3 wt% of the mixed acid solution.
[0044] Preparation of functionalized carbon nanotubes: Carboxylated carbon nanotubes and ethanolamine phosphate were added to DMF and stirred for 40 min under nitrogen protection. DCC solution was then added, and the mixture was reacted at 30 °C for 72 h. After the reaction was complete, the mixture was filtered, washed, dried, and ground to obtain functionalized carbon nanotubes. The amount of carboxylated carbon nanotubes used was 0.4 wt% of DMF, and the amount of ethanolamine phosphate used was 3 wt% of carboxylated carbon nanotubes. The DCC solution was obtained by dissolving DCC in THF, and the DCC solution contained 15 wt% DCC. The amount of DCC solution used was 30 wt% of DMF.
[0045] Preparation of carbon nanotube composite materials: Zinc reagent and deionized water were added to diethylene glycol and stirred at 160-180℃ for 5 min. The mixture was then allowed to stand at 30℃ for 2 h to obtain a zinc oxide sol. Functionalized carbon nanotubes were added and ultrasonically mixed to obtain a carbon nanotube composite solution. The solution was stirred at 180℃ for 3 h, cooled to room temperature, centrifuged to remove the supernatant, washed, dried, and ground to obtain the carbon nanotube composite material. The zinc reagent was zinc acetate, the zinc oxide sol contained 0.5 wt% zinc reagent, the amount of deionized water was 1000 wt% of the zinc reagent, and the amount of functionalized carbon nanotubes was 80 wt% of the zinc oxide sol.
[0046] Preparation of silica composite sol: An ethanol solution and a tetraethyl orthosilicate solution were mixed, glycerol was added, the pH of the solution was adjusted to 2, and the mixture was stirred for 40 min. A polyvinyl alcohol solution was then added, and the mixture was stirred at 80 °C for 9 h. Carbon nanotube composite material was then added, and the mixture was stirred at 80 °C for 9 h. The mixture was then aged at 30 °C for 24 h to obtain the silica composite sol. The ethanol solution contained 80 wt% ethanol. The tetraethyl orthosilicate solution was obtained by adding tetraethyl orthosilicate to deionized water and contained 60 wt% tetraethyl orthosilicate. The amount of ethanol used was 200 wt% of the tetraethyl orthosilicate solution, the amount of glycerol used was 30 wt% of the tetraethyl orthosilicate solution, the amount of polyvinyl alcohol used was 12 wt% of polyvinyl alcohol used was 30 wt% of the tetraethyl orthosilicate solution, and the amount of carbon nanotube composite material used was 2.6 wt% of the tetraethyl orthosilicate solution.
[0047] Sol coating: The pretreated aluminum alloy was immersed in silica composite sol and coated 5 times. The first coating time was 100s, and the subsequent coating times were 40s. The interval between each coating was 60min. The coating speed was 5cm / min.
[0048] Preparation of nano-ceramic coating on aluminum alloy surface: The aluminum alloy coated with silica composite sol was treated at 100℃ for 60 min and then cured at 300℃ to obtain an aluminum alloy with nano-ceramic coating on the surface.
[0049] Example 2: A method for preparing a nano-ceramic coating on the surface of marine aluminum alloys. The only difference between this embodiment and Example 1 is that the amount of carbon nanotube composite material used is 5.4 wt% of tetraethyl orthosilicate solution.
[0050] Example 3: A method for preparing a nano-ceramic coating on the surface of marine aluminum alloys. Pretreatment of the aluminum alloy substrate: The surface layer of the substrate was removed by wet sanding with sandpaper, followed by washing with ethanol. After washing and drying with ethanol, the substrate was alkaline-washed with an alkaline solution at 80°C for 40 minutes. After alkaline washing, it was washed with deionized water until neutral. Then, it was acid-washed with an acidic solution at 30°C for 40 minutes. After acid washing, it was washed with deionized water until neutral. After rinsing with acetone, it was dried to obtain the pretreated aluminum alloy substrate. The alkaline solution was 2 wt% sodium hydroxide, and the acidic solution was 8 wt% nitric acid.
[0051] Preparation of carboxylated carbon nanotubes: Carbon nanotubes were added to a mixed acid solution and sonicated for 40 min, then stirred at 60 °C for 2 h. After removing the carbon nanotubes, they were washed with anhydrous ethanol, then washed with deionized water until neutral, dried, and ground to obtain carboxylated carbon nanotubes. The mixed acid solution was a mixture of concentrated sulfuric acid and concentrated nitric acid, with the amount of concentrated nitric acid in the mixed acid solution being 30 wt% of the amount of concentrated sulfuric acid, and the amount of carbon nanotubes being 0.3 wt% of the mixed acid solution.
[0052] Preparation of functionalized carbon nanotubes: Carboxylated carbon nanotubes and ethanolamine phosphate were added to DMF and stirred for 40 min under nitrogen protection. DCC solution was then added, and the mixture was reacted at 30 °C for 72 h. After the reaction was complete, the mixture was filtered, washed, dried, and ground to obtain functionalized carbon nanotubes. The amount of carboxylated carbon nanotubes used was 0.4 wt% of DMF, and the amount of ethanolamine phosphate used was 3 wt% of carboxylated carbon nanotubes. The DCC solution was obtained by dissolving DCC in THF, and the DCC solution contained 15 wt% DCC. The amount of DCC solution used was 30 wt% of DMF.
[0053] Preparation of carbon nanotube composite materials: Zinc reagent and deionized water were added to diethylene glycol and stirred at 160-180℃ for 5 min. The mixture was then allowed to stand at 30℃ for 2 h to obtain a zinc oxide sol. Functionalized carbon nanotubes were added and ultrasonically mixed to obtain a carbon nanotube composite solution. The solution was stirred at 180℃ for 3 h, cooled to room temperature, centrifuged to remove the supernatant, washed, dried, and ground to obtain the carbon nanotube composite material. The zinc reagent was zinc acetate, the zinc oxide sol contained 0.5 wt% zinc reagent, the amount of deionized water was 1000 wt% of the zinc reagent, and the amount of functionalized carbon nanotubes was 80 wt% of the zinc oxide sol.
[0054] Preparation of silica composite sol: An ethanol solution and a tetraethyl orthosilicate solution were mixed, glycerol was added, the pH of the solution was adjusted to 2, and the mixture was stirred for 40 min. A polyvinyl alcohol solution was then added, and the mixture was stirred at 80 °C for 9 h. Carbon nanotube composite material and aluminum dihydrogen phosphate were then added, and the mixture was stirred at 80 °C for 9 h. The mixture was then aged at 30 °C for 24 h to obtain the silica composite sol. The ethanol solution contained 80 wt% ethanol. The tetraethyl orthosilicate solution was obtained by adding tetraethyl orthosilicate to deionized water and contained 60 wt% tetraethyl orthosilicate. The amount of ethanol used was 200 wt% of the tetraethyl orthosilicate solution, the amount of glycerol used was 30 wt% of the tetraethyl orthosilicate solution, the amount of polyvinyl alcohol used was 12 wt% of polyvinyl alcohol used was 30 wt% of the tetraethyl orthosilicate solution, the amount of carbon nanotube composite material used was 2.6 wt% of the tetraethyl orthosilicate solution, and the amount of aluminum dihydrogen phosphate used was 1.2 wt% of the tetraethyl orthosilicate solution.
[0055] Sol coating: The pretreated aluminum alloy was immersed in silica composite sol and coated 5 times. The first coating time was 100s, and the subsequent coating times were 40s. The interval between each coating was 60min. The coating speed was 5cm / min.
[0056] Preparation of nano-ceramic coating on aluminum alloy surface: The aluminum alloy coated with silica composite sol was treated at 100℃ for 60 min and then cured at 300℃ to obtain an aluminum alloy with nano-ceramic coating on the surface.
[0057] Comparative Example 1: A method for preparing a nano-ceramic coating on the surface of marine aluminum alloys. The only difference between this comparative example and Example 2 is that, in the preparation of the carbon nanotube composite material, the functionalized carbon nanotubes are replaced with carboxylated carbon nanotubes.
[0058] Experimental example: 1. Infrared characterization Test sample: Functionalized carbon nanotubes prepared in Example 1.
[0059] The infrared spectra of functionalized carbon nanotubes were determined by total reflectance method after mixing potassium bromide with the test sample and pressing the mixture into a pellet.
[0060] The infrared spectrum of the functionalized carbon nanotubes prepared by this invention is as follows: Figure 1 As shown, at 3425cm -1 The infrared absorption peak at 3351 cm⁻¹ is the hydroxyl group on the carbon nanotube. -1 The infrared absorption peaks for nitrogen and hydrogen are located at 2874 cm⁻¹. -1 The infrared absorption of the methylene group is at 1712 cm⁻¹. -1 The infrared absorption peak at 1289 cm⁻¹ represents the carbon-oxygen double bond. -1 The infrared absorption peak at 1138 cm⁻¹ represents the phosphorus-oxygen double bond. -1 The presence of infrared absorption peaks for carbon, oxygen, and carbon indicates the formation of functionalized carbon nanotubes obtained from ethanolamine phosphate and carboxylated carbon nanotubes.
[0061] 2. Hardness test Test samples: Aluminum alloys with nano-ceramic coatings on the surface prepared in each embodiment and comparative example.
[0062] The hardness of the test sample was tested and analyzed using a microhardness tester. The indenter was 300g and the loading time was 30s.
[0063] The hardness test results of the nano-ceramic coating on the aluminum alloy surface prepared by this invention are as follows: Figure 2As shown, A represents Example 1, B represents Example 2, C represents Example 3, and D represents Comparative Example 1. The hardness of the nano-ceramic coating on the aluminum alloy surface prepared in Example 1 is 658 Hv, the hardness of the nano-ceramic coating on the aluminum alloy surface prepared in Example 2 is 684 Hv, and the hardness of the nano-ceramic coating on the aluminum alloy surface prepared in Comparative Example 1 is 582 Hv. Compared with Comparative Example 1, Example 2 involves acidifying carbon nanotubes to obtain carboxylated carbon nanotubes, then reacting the carboxylated carbon nanotubes with ethanolamine phosphate to obtain functionalized carbon nanotubes, and then combining the functionalized carbon nanotubes with zinc reagent to form a carbon nanotube composite material. This carbon nanotube composite material is used to prepare a silica composite sol. The aluminum alloy is dip-coated in the silica composite sol, dried, and then cured at high temperature to obtain a nano-ceramic coating attached to the surface of the aluminum alloy. When replacing functionalized carbon nanotubes with carboxylated carbon nanotubes in the preparation of composite materials, the hardness of the nano-ceramic coating obtained by replacing functionalized carbon nanotubes with carboxylated carbon nanotubes was not as high as that obtained by using functionalized carbon nanotubes. This indicates that using functionalized carbon nanotubes obtained by reacting carboxylated carbon nanotubes with ethanolamine phosphate has an effect on improving the hardness of the nano-ceramic coating. Compared with Comparative Example 1, the hardness of the nano-ceramic coating prepared in Example 2 increased by 17.53%. The hardness of the nano-ceramic coating on the aluminum alloy surface prepared in Example 3 was 713 Hv. Compared with Example 2, Example 3 shows that when preparing silica composite sol, under the condition of using functionalized carbon nanotubes, the addition of aluminum dihydrogen phosphate has an enhancing effect on the hardness of the nano-ceramic coating on the aluminum alloy surface. Compared with Example 2, the hardness of the nano-ceramic coating prepared in Example 3 increased by 4.24%.
[0064] The nano-ceramic coating prepared by this invention has high hardness, ranging from 640 to 730 Hv.
[0065] 3. Wear resistance test Test samples: Aluminum alloys with nano-ceramic coatings on the surface prepared in each embodiment and comparative example.
[0066] Wear resistance tests were conducted using a multi-functional friction and wear testing machine. The test load was 20 N, the frequency was 1 Hz, and the running time was 30 min. Si3N4 ceramic balls with a diameter of 9 mm were used for grinding.
[0067] The wear resistance test results of the nano-ceramic coating on the aluminum alloy surface prepared by this invention are as follows: Figure 3 As shown, the unit of wear is 10. -4 mm 3 / Nm, A represents Example 1, B represents Example 2, C represents Example 3, D represents Comparative Example 1. The wear value of the nano-ceramic coating on the aluminum alloy surface prepared in Example 1 is 1.68, the wear value of the nano-ceramic coating on the aluminum alloy surface prepared in Example 2 is 1.54, and the wear value of the nano-ceramic coating on the aluminum alloy surface prepared in Comparative Example 1 is 2.19. Compared with Comparative Example 1, Example 2 involves acidifying carbon nanotubes to obtain carboxylated carbon nanotubes, then reacting the carboxylated carbon nanotubes with ethanolamine phosphate to obtain functionalized carbon nanotubes, and then combining the functionalized carbon nanotubes with zinc reagent to form a carbon nanotube composite material. The above carbon nanotube composite material is used to prepare silica composite sol, and aluminum alloy is dip-coated in silica composite sol. After drying, it is cured at high temperature to obtain a nano-ceramic coating attached to the surface of the aluminum alloy. When preparing the carbon nanotube composite material, the functionalized carbon nanotubes are acidified to obtain carboxylated carbon nanotubes, then reacted with ethanolamine phosphate to obtain functionalized carbon nanotubes, and then reacted with zinc reagent to form a carbon nanotube composite material. After replacing the functionalized carbon nanotubes with carboxylated carbon nanotubes, the wear resistance of the prepared nano-ceramic coating was not as high as that of the nano-ceramic coating obtained using functionalized carbon nanotubes. This indicates that using functionalized carbon nanotubes obtained by reacting carboxylated carbon nanotubes with ethanolamine phosphate has an effect on improving the wear resistance of the nano-ceramic coating. Compared with Comparative Example 1, the wear resistance of the nano-ceramic coating prepared in Example 2 was improved by 29.68%. The wear value of the nano-ceramic coating on the aluminum alloy surface prepared in Example 3 was 1.26. Compared with Example 2, Example 3 shows that when preparing the silica composite sol, under the condition of using functionalized carbon nanotubes, the addition of aluminum dihydrogen phosphate has an enhancing effect on the wear resistance of the nano-ceramic coating on the aluminum alloy surface. Compared with Example 2, the wear resistance of the nano-ceramic coating prepared in Example 3 was improved by 18.18%.
[0068] The nano-ceramic coating prepared by this invention has good wear resistance.
[0069] 4. Corrosion resistance test Test samples: Aluminum alloys with nano-ceramic coatings on the surface prepared in each embodiment and comparative example.
[0070] After weighing the test sample, it was placed in a hydrochloric acid solution for corrosion testing. After 5 hours, it was taken out, cleaned until neutral, dried, weighed, and the corrosion weight loss was calculated.
[0071] The corrosion resistance test results of the nano-ceramic coating on the aluminum alloy surface prepared by this invention are as follows: Figure 4 As shown, A represents Example 1, B represents Example 2, C represents Example 3, and D represents Comparative Example 1. The corrosion rate of the nano-ceramic coating on the aluminum alloy surface prepared in Example 1 is 0.044 g / cm³. 2The corrosion rate of the nano-ceramic coating on the aluminum alloy surface prepared in Example 2 was 0.038 g / cm³. 2 The corrosion rate of the nano-ceramic coating on the aluminum alloy surface prepared in Comparative Example 1 was 0.064 g / cm³. 2 Compared to Comparative Example 1, Example 2 involved acidifying carbon nanotubes to obtain carboxylated carbon nanotubes, then reacting the carboxylated carbon nanotubes with ethanolamine phosphate to obtain functionalized carbon nanotubes. These functionalized carbon nanotubes were then combined with a zinc reagent to form a carbon nanotube composite material. This composite material was used to prepare a silica composite sol, which was then used to coat aluminum alloy in a pull-coating process. After drying, the coating was cured at high temperature to obtain a nano-ceramic coating attached to the aluminum alloy surface. However, when the functionalized carbon nanotubes were replaced with carboxylated carbon nanotubes in the preparation of the carbon nanotube composite material, the corrosion resistance of the resulting nano-ceramic coating was not as high as that obtained using functionalized carbon nanotubes. This indicates that using carboxylated carbon nanotubes reacted with ethanolamine phosphate to obtain functionalized carbon nanotubes improves the corrosion resistance of the nano-ceramic coating. Compared to Comparative Example 1, the corrosion resistance of the nano-ceramic coating prepared in Example 2 was improved by 40.63%. The corrosion amount of the nano-ceramic coating on the aluminum alloy surface prepared in Example 3 was 0.023 g / cm³. 2 Compared with Example 2, Example 3 shows that when preparing silica composite sol, the addition of aluminum dihydrogen phosphate under the condition of using functionalized carbon nanotubes has an enhanced effect on the corrosion resistance of the nano-ceramic coating on the aluminum alloy surface. Compared with Example 2, the corrosion resistance of the nano-ceramic coating prepared in Example 3 is improved by 39.47%.
[0072] The nano-ceramic coating prepared by this invention exhibits good corrosion resistance, with a corrosion rate of 0.02-0.05 g / cm³. 2 .
[0073] The above embodiments are for illustrative purposes only and are not intended to limit the invention. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the invention. Therefore, all equivalent technical solutions also fall within the scope of this invention, and the patent protection scope of this invention should be defined by the claims.
Claims
1. A method for preparing a nano-ceramic coating on the surface of marine aluminum alloy, comprising: The surface of the aluminum alloy substrate is pretreated to remove the surface layer, resulting in a pretreated aluminum alloy substrate. A nano-ceramic coating on the surface of aluminum alloy is obtained by dip coating in silica composite sol after pretreatment and then curing. Preparation of the silica composite sol: Mix ethanol solution with tetraethyl orthosilicate solution, add glycerol, adjust the pH of the solution to 2-3, stir for 20-60 min, add polyvinyl alcohol solution, stir at 60-80℃ for 6-12 h, add carbon nanotube composite material, stir at 60-80℃ for 6-12 h, and age at 20-40℃ for more than 24 h to obtain silica composite sol; Aluminum dihydrogen phosphate is added during the preparation of the silica composite sol, and the amount of aluminum dihydrogen phosphate used is 0.6-2 wt% of the tetraethyl orthosilicate solution; The silica composite sol contains a carbon nanotube composite material, which is prepared by adding functionalized carbon nanotubes to zinc oxide sol. The functionalized carbon nanotubes are generated by reacting carboxylated carbon nanotubes with ethanolamine phosphate.
2. The method for preparing a nano-ceramic coating on the surface of marine aluminum alloy according to claim 1, characterized in that: The pretreatment process involves wet sanding with sandpaper, followed by alkaline washing with an alkaline solution and acid washing with an acidic solution.
3. The method for preparing a nano-ceramic coating on a marine-grade aluminum alloy surface according to claim 1, characterized in that: The amount of functionalized carbon nanotubes used is 20-100 wt% of zinc oxide sol.
4. The method for preparing a nano-ceramic coating on a marine-grade aluminum alloy surface according to claim 1, characterized in that: The tetraethyl orthosilicate solution contains 50-70 wt% tetraethyl orthosilicate, and the polyvinyl alcohol solution contains 6-14 wt% polyvinyl alcohol.
5. The method for preparing a nano-ceramic coating on a marine-grade aluminum alloy surface according to claim 1, characterized in that: The amount of glycerol used is 20-40 wt% of the tetraethyl orthosilicate solution, and the amount of polyvinyl alcohol used is 20-40 wt% of the tetraethyl orthosilicate solution.
6. The method for preparing a nano-ceramic coating on a marine-grade aluminum alloy surface according to claim 1, characterized in that: The amount of the carbon nanotube composite material used is 2-6 wt% of the tetraethyl orthosilicate solution.
Citation Information
Patent Citations
Preparing method of graphene oxide compound lubricating oil and compound lubricating oil
CN108531246A
Hybrid carbon nanotube reinforced wear-resistant anti-friction ceramic coating and preparation method thereof
CN110305504A