A water-soluble alicyclic amine curing agent and preparation method thereof

By using a small amount of N,N-dimethyl tertiary amine fatty amine and epoxy resin in aqueous epoxy resin, the problem of insufficient performance of alicyclic amine in aqueous curing agents is solved, and high performance is achieved The preparation of water-soluble alicyclic amine curing agent simplifies the process and expands the scope of application.

CN117487136BActive Publication Date: 2024-11-01JIANGSU FUQISEN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311448634.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-02
Publication Date
2024-11-01
Estimated Expiration
2043-11-02

AI Technical Summary

Technical Problem

When using alicyclic amines in existing aqueous epoxy resin curing agents, it is difficult to fully reflect their performance characteristics, and the preparation process is complex and costly, resulting in low physical stability of the curing agent and limited application fields.

Method used

A small amount of N,N-dimethyl tertiary amine is used to combine with ethoxy group-containing epoxy resin and ethoxy group-free biepoxy compound through specific reaction steps and cosolvents and additives. The proportion is to improve the content and curing properties of alicyclic amines, and form a water-soluble alicyclic amine curing agent.

Benefits of technology

It realizes the maximum hydrophobicity, high gloss, high hardness, high toughness and high media resistance of alicyclic amines while ensuring water solubility and storage stability, simplifies the preparation process and improves the performance of the curing agent. and versatile.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004528307610000021
    Figure BDA0004528307610000021
  • Figure BDA0004528307610000051
    Figure BDA0004528307610000051
  • Figure BDA0004528307610000111
    Figure BDA0004528307610000111
Patent Text Reader

Abstract

The present invention relates to the technical field of waterborne epoxy resin curing agents, and in particular to a water-soluble alicyclic amine curing agent and a preparation method thereof. The curing agent uses alicyclic amine as a main raw material, and is matched with a monoepoxy compound or a diepoxy compound containing at least one ethoxy group in the molecular structure as epoxy resin A, a tertiary amino fatty amine, a diepoxy compound having no less than 10 carbon atoms and no ethoxy group as epoxy resin B, a cosolvent, a neutralizer and water to prepare a water-soluble alicyclic amine curing agent that retains the performance characteristics of alicyclic amine to the greatest extent. The curing agent greatly increases the content of alicyclic amine in the curing agent while ensuring good water solubility and storage stability, and has the characteristics of hydrophobicity, high gloss, high hardness, high toughness, high medium resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of waterborne epoxy resin curing agents, in particular to a water-soluble alicyclic amine curing agent and a preparation method thereof. Background Art

[0002] Small-molecule base amines commonly used to modify epoxy resin curing agents can be divided into three main categories based on their chemical structure: aliphatic amines, cycloaliphatic amines, and aromatic amines. Aromatic amines have weak reactivity, dark color, and high toxicity, making them less commonly used in water-based products. Aliphatic amines are fast, low-cost, and most commonly used. Their high water solubility facilitates the preparation of water-based products, but their curing performance is less pronounced. Cycloaliphatic amines, on the other hand, possess a unique molecular structure. Compared to aliphatic amines when curing epoxy resins, cycloaliphatic amines exhibit moderate reactivity, high gloss, low chroma (yellowing resistance), high mechanical strength, and excellent media resistance. With the recent increase in aliphatic amine production capacity and reduction in costs, cycloaliphatic amine epoxy curing agents have gained increasing market attention.

[0003] Currently, using alicyclic amines as the primary raw material to create water-based curing agents presents the following difficulties: 1) The alicyclic amine molecule contains at least one six-membered carbon ring. The high number of carbon atoms and steric hindrance result in poor hydrophilicity of the amine adduct. To prepare stable water-soluble curing agents, those skilled in the art typically incorporate a high proportion of hydrophilic fatty amines, such as diethylenetriamine and triethylenetetramine, into their formulations and modify them with nonionic hydrophilic groups. This method results in a high proportion of polyvalent fatty amines in the curing agent, resulting in a large number of active hydrogen atoms provided by the fatty amines participating in the curing process, making it difficult to fully realize the performance characteristics of the alicyclic amines. Furthermore, the reactivity of alicyclic amines differs significantly from that of fatty amines. Mixing the two makes the modification process complex and prone to uneven reaction and high viscosity. To better utilize alicyclic amines, the alicyclic amines can be first prepared as hydrophobic amine adducts, which are then mixed with an emulsifier to create an emulsion-type water-based curing agent. However, emulsion curing agents also have disadvantages such as complex processes and high production costs. In addition, compared with water-soluble curing agents, emulsion curing agents have low physical stability and limited application areas.

[0004] In order to better apply alicyclic amines to environmentally friendly water-based products, the art urgently needs a water-soluble alicyclic amine curing agent that uses alicyclic amines as a main raw material and can highlight its performance characteristics. Summary of the Invention

[0005] The purpose of the present invention is to provide a water-soluble alicyclic amine curing agent and a preparation method thereof, thereby reducing the use of fatty amines in the preparation of the alicyclic amine curing agent and maximizing the functional properties of the alicyclic amine itself.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] A water-soluble alicyclic amine curing agent is prepared from the following raw materials in parts by weight:

[0008]

[0009] The epoxy resin A is a monoepoxy compound or a diepoxy compound containing at least one ethoxy group in its molecular structure;

[0010] The epoxy resin B is a diepoxy compound having no less than 10 carbon atoms and no ethoxy group.

[0011] Optionally, the chemical structure of the alicyclic amine contains at least one cyclohexyl group and at least two primary amine groups, and at least one primary amine group is directly connected to the cyclohexyl group;

[0012] The epoxy equivalent of the epoxy resin A is 100 to 800 g / eq;

[0013] The tertiary amino fatty amine is an aliphatic amine containing at least one N,N-dimethyl group in its molecular structure; the aliphatic amine contains 2 to 8 carbon atoms and 1 to 2 active hydrogen atoms;

[0014] The epoxy equivalent of the epoxy resin B is 100 to 350 g / eq;

[0015] The cosolvent is a monohydric alcohol or alcohol ether compound that is miscible with water in any proportion; the boiling point of the cosolvent is greater than 80°C;

[0016] The neutralizing agent is a monocarboxylic acid with a carbon number not greater than 4.

[0017] Optionally, the alicyclic amine includes at least one of menthanediamine, isophoronediamine, 1,2-cyclohexanediamine, methylcyclohexanediamine, 4,4-diaminodicyclohexylmethane, and 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane.

[0018] Optionally, the epoxy resin A comprises at least one of methoxy polyethylene glycol glycidyl ether, ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, triethylene glycol diglycidyl ether and polyethylene glycol diglycidyl ether.

[0019] Optionally, the tertiary amino fatty amine includes at least one of N,N-dimethylethylenediamine, N,N-dimethyl-1,3-propylenediamine, and 3,3'-iminobis(N,N-dimethylpropylamine).

[0020] Optionally, the epoxy resin B comprises at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,2-cyclohexanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, dipropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether and dimer acid diglycidyl ether.

[0021] Optionally, the cosolvent comprises at least one of isopropyl alcohol, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether, propylene glycol methyl ether, and dipropylene glycol methyl ether;

[0022] The neutralizing agent comprises at least one of formic acid, acetic acid, propionic acid, n-butyric acid, glycolic acid, and lactic acid.

[0023] The present invention also provides a method for preparing a water-soluble alicyclic amine curing agent, comprising the following steps:

[0024] 1). Mix tertiary amino fatty amine and epoxy resin A to obtain an intermediate,

[0025] 2) Adding alicyclic amine and cosolvent to the intermediate obtained in step 1) as the bottom liquid;

[0026] 3) The epoxy resin B was added dropwise to the bottom of the kettle liquid obtained in step 2), and the reaction was continued after the addition was completed;

[0027] 4). After the reaction in step 3) is completed, a neutralizing agent and water are added to obtain the water-soluble alicyclic amine curing agent.

[0028] Optionally, the reaction temperature in step 1) is 40-70° C., and the reaction time is 0.5-2 h;

[0029] Step 3) the dripping time is 2 to 4 hours, the reaction temperature is 60 to 90° C., and the reaction time is 1 to 4 hours;

[0030] After adding the neutralizing agent and water in step 4), the mixture needs to be dispersed at 30-60° C. for 1-3 hours.

[0031] Optionally, in step 3), before the epoxy resin B is dripped into the kettle bottom liquid obtained in step 2), the temperature of the kettle bottom liquid is 60-90° C., and the temperature of the epoxy resin B is 20-40° C.;

[0032] In step 4), the reaction product of step 3) needs to be cooled to 40-70° C. before adding the neutralizing agent and water.

[0033] Existing water-soluble alicyclic amine curing agent formulations achieve good water solubility through the use of large amounts of fatty amines. However, the performance of the curing agent prepared with this formulation deviates from the original characteristics of the alicyclic amines, and the preparation method is relatively complex. The formulation provided by the present invention increases the content of alicyclic amines in the curing agent raw materials, requiring only a small amount of aliphatic amine containing N,N-dimethyl tertiary amine groups as an auxiliary raw material. Due to the alkyl electron-donating effect and low steric hindrance, the N,N-dimethyl tertiary amine group has a strong hydration ability and provides strong hydrophilicity to the curing agent in combination with a small amount of acid salt and a small amount of ethoxylated compound. The content of alicyclic amine in the curing agent can be greatly increased while ensuring good water solubility and storage stability, so that the water-based curing agent prepared by the present invention can maximize the retention of the hydrophobicity, high gloss, high hardness, high toughness, and high media resistance characteristics of the alicyclic amines. The tertiary amine group can also promote the curing of the alicyclic amine and epoxy resin, having a catalytic effect.

[0034] In the raw materials for preparing the curing agent of the present invention, the amount of tertiary amino fatty amine is small and the number of active hydrogen atoms therein is small. Therefore, in the water-based alicyclic amine curing agent prepared by the present invention, the active hydrogen atoms that can be used for curing are almost all provided by the alicyclic amine.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) Increase the amount of alicyclic amine in the curing agent and reduce the use of fatty amine, fully reflect the performance characteristics of alicyclic amine, and the preparation process is simple and controllable.

[0037] (2) When the curing agent prepared by the present invention is used for curing, the performance of the obtained cured product is close to that of the unmodified raw material alicyclic amine.

[0038] (3) The water-soluble alicyclic amine curing agent obtained by the present invention is suitable for various water-based epoxy resins (emulsion type, solution type) on the market, and can also directly emulsify unmodified standard liquid epoxy resins, and has a wide range of uses.

[0039] (4) The water-soluble alicyclic amine curing agent obtained by the present invention has the curing performance characteristics of the alicyclic amine raw material, and can also be used as an auxiliary component to be used in combination with other types of water-based amine curing agents to enhance their performance.

[0040] In summary, the water-soluble alicyclic amine curing agent provided by the present invention possesses all the performance advantages of the raw alicyclic amine. It can also be used with various modified or unmodified epoxy resins and as a co-curing agent mixed with other water-based amine curing agents to achieve diverse performance. This curing agent has a wide range of applications and can significantly promote the application of high-performance alicyclic amines in the field of water-based resins, thus possessing high market value. Furthermore, the preparation process of the water-soluble alicyclic amine curing agent is simple, making it amenable to industrial production. DETAILED DESCRIPTION

[0041] The present invention provides a water-soluble alicyclic amine curing agent, which is prepared from the following raw materials in parts by weight:

[0042]

[0043] The epoxy resin A is a monoepoxy compound or a diepoxy compound containing at least one ethoxy group in its molecular structure;

[0044] The epoxy resin B is a diepoxy compound having no less than 10 carbon atoms and no ethoxy group.

[0045] In the present invention, the weight portion of the alicyclic amine in the raw material is 15 to 35 parts, preferably 18 to 32 parts, more preferably 22 to 30 parts, and even more preferably 24 to 28 parts;

[0046] The chemical structure of the alicyclic amine contains at least one cyclohexyl group and at least two primary amine groups, and at least one primary amine group is directly connected to the cyclohexyl group; the alicyclic amine contains at least one of menthane diamine, isophorone diamine, 1,2-cyclohexane diamine, methylcyclohexane diamine, 4,4-diaminodicyclohexylmethane, and 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane.

[0047] In the present invention, the weight portion of epoxy resin A in the raw materials is 2 to 12 parts, preferably 4 to 10 parts, more preferably 5 to 8 parts, and even more preferably 6 to 7 parts;

[0048] The epoxy equivalent weight of the epoxy resin A is 100 to 800 g / eq, preferably 150 to 600 g / eq, more preferably 200 to 400 g / eq, and even more preferably 260 to 300 g / eq;

[0049] The epoxy resin A comprises at least one of methoxy polyethylene glycol glycidyl ether, ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, triethylene glycol diglycidyl ether and polyethylene glycol diglycidyl ether.

[0050] In the present invention, the weight portion of the tertiary amino fatty amine in the raw material is 1 to 5 parts, preferably 1 to 4 parts, and more preferably 2 to 3 parts;

[0051] The tertiary amino fatty amine is an aliphatic amine containing at least one N,N-dimethyl group in its molecular structure; the aliphatic amine contains 1 to 8 carbon atoms and 1 to 2 active hydrogen atoms; the aliphatic amine preferably contains 2 to 6 carbon atoms, more preferably 2 to 4 carbon atoms;

[0052] The tertiary amino fatty amine includes at least one of N,N-dimethylethylenediamine, N,N-dimethyl-1,3-propylenediamine, and 3,3'-iminobis(N,N-dimethylpropylamine).

[0053] In the present invention, the weight portion of epoxy resin B in the raw materials is 10 to 32 parts, preferably 16 to 30 parts, more preferably 20 to 28 parts, and even more preferably 22 to 26 parts;

[0054] The epoxy equivalent weight of the epoxy resin B is 100 to 350 g / eq, preferably 120 to 320 g / eq, more preferably 150 to 300 g / eq, and even more preferably 180 to 220 g / eq;

[0055] The epoxy resin B comprises at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,2-cyclohexanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, dipropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether and dimer acid diglycidyl ether.

[0056] In the present invention, the weight portion of the cosolvent in the raw material is 5 to 15 parts, preferably 6 to 12 parts, more preferably 7 to 11 parts, and even more preferably 8 to 10 parts;

[0057] The cosolvent is a monohydric alcohol or alcohol ether compound that is miscible with water in any proportion; the boiling point of the cosolvent is greater than 80°C, preferably greater than 100°C, more preferably 120°C, and even more preferably 130°C;

[0058] The cosolvent comprises at least one of isopropyl alcohol, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether, propylene glycol methyl ether, and dipropylene glycol methyl ether. Adding the cosolvent to the reaction can adjust the viscosity of the curing agent during preparation and improve its affinity with water.

[0059] In the present invention, the weight portion of the neutralizing agent in the raw material is 0 to 5 parts, preferably 0 to 4 parts, more preferably 0 to 3 parts, and even more preferably 1 to 2 parts;

[0060] The neutralizing agent is a monocarboxylic acid having no more than 4 carbon atoms; the carbon number of the carboxylic acid is preferably no more than 3, more preferably no more than 2;

[0061] The neutralizing agent comprises at least one of formic acid, acetic acid, propionic acid, n-butyric acid, glycolic acid, and lactic acid. The neutralizing agent can enhance the water solubility of the prepared curing agent.

[0062] In the present invention, the weight portion of water in the raw material is 10 to 40 parts, preferably 20 to 35 parts, more preferably 25 to 34 parts, and even more preferably 30 to 33 parts. The addition of water can adjust the viscosity of the obtained curing agent.

[0063] The present invention also provides a method for preparing a water-soluble alicyclic amine curing agent, comprising the following steps:

[0064] 1). Mix tertiary amino fatty amine and epoxy resin A to obtain an intermediate,

[0065] 2) Adding alicyclic amine and cosolvent to the intermediate obtained in step 1) as the bottom liquid;

[0066] 3) The epoxy resin B was added dropwise to the bottom of the kettle liquid obtained in step 2), and the reaction was continued after the addition was completed;

[0067] 4). After the reaction in step 3) is completed, a neutralizing agent and water are added to obtain the water-soluble alicyclic amine curing agent.

[0068] In the present invention, the reaction temperature in step 1) is 40-70°C, preferably 45-65°C, more preferably 50-60°C; the reaction time is 0.5-2h, preferably 0.75-1.5h, more preferably 1-1.25h;

[0069] In the present invention, before the epoxy resin B is dripped into the kettle bottom liquid obtained in step 2) in step 3), the temperature of the kettle bottom liquid is 60-90°C, preferably 65-85°C, more preferably 70-80°C, and even more preferably 75-80°C;

[0070] The temperature of epoxy resin B is 20-40°C, preferably 25-40°C, more preferably 30-35°C; the addition time;

[0071] Step 3) the dripping time is 2 to 4 hours, preferably 2.25 to 3.75 hours, more preferably 2.5 to 3.5 hours, and even more preferably 3 to 3.25 hours;

[0072] The temperature for continuing the reaction is 60-90°C, preferably 65-85°C, more preferably 70-80°C, and even more preferably 75-75°C;

[0073] The reaction time is 1 to 4 hours, preferably 1.5 to 3.5 hours, more preferably 2 to 3.5 hours, and even more preferably 2.5 to 3 hours;

[0074] In the present invention, in step 4), the reaction product of step 3) needs to be cooled to 40-70°C, preferably 45-70°C, more preferably 50-65°C, and even more preferably 55-60°C before adding the neutralizing agent and water;

[0075] After adding the neutralizing agent and water in step 4), the mixture needs to be dispersed at 30-60°C for 30-90 minutes; the dispersion temperature is preferably 35-55°C, more preferably 40-55°C, and even more preferably 45-50°C;

[0076] The dispersion time is preferably 1 to 3 hours, more preferably 1.5 to 2.5 hours, and more preferably 2 hours.

[0077] The technical solutions provided by the present invention are described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0078] Example 1

[0079] 1) Add 5 parts by weight of polyethylene glycol diglycidyl ether with an epoxy equivalent of 280g / eq and 2 parts by weight of N,N-dimethyl-1,3-propylenediamine to the reactor and mix evenly. Then heat to 60°C and keep warm for 1h. After the end of the heat preservation, add 20 parts by weight of 1,2-cyclohexanediamine and 10 parts by weight of propylene glycol methyl ether and mix evenly. Heat to 70°C as the bottom liquid for later use.

[0080] 2) Mix and dissolve 8 parts by weight of 1,6-hexanediol diglycidyl ether, 18 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189, and 6 parts by weight of polypropylene glycol diglycidyl ether with an epoxy equivalent of 320 at 30°C, pour into a constant pressure dropping funnel, and add dropwise the bottom liquid obtained in step 1) for 3 hours. Maintain the temperature of the material in the kettle at 70°C during the addition process. After the addition is completed, raise the temperature of the material in the kettle to 80°C and continue the reaction for 2 hours.

[0081] 3). After the reaction in step 2) was completed, stirring was maintained, 1 part by weight of acetic acid and 30 parts by weight of pure water were added, the temperature was lowered to 50°C and stirred for 2h to obtain a water-soluble alicyclic amine curing agent A with a solid content of 60wt% and an active hydrogen equivalent of 189g / eq.

[0082] 37.5 parts by weight of curing agent A, 37.5 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189, and 25 parts by weight of pure water were mixed in a container. After standing for 10 minutes, a 100 μm wire rod was used to apply the coating on polished tinplate to test the coating performance. The results are shown in Table 1.

[0083] Example 2

[0084] 1) Add 6 parts by weight of polyethylene glycol diglycidyl ether with an epoxy equivalent of 280g / eq and 4 parts by weight of 3,3'-iminobis(N,N-dimethylpropylamine) to the reactor and mix well. Then heat to 60°C and keep warm for 1h. After the end of the heat preservation, add 20 parts by weight of 1,2-cyclohexanediamine and 5 parts by weight of propylene glycol methyl ether and mix well. Heat to 70°C as the bottom liquid for later use.

[0085] 2) Mix and dissolve 11 parts by weight of 1,6-hexanediol diglycidyl ether and 19 parts by weight of bisphenol A epoxy resin with an epoxy equivalent weight of 189 at 30°C, pour into a constant pressure dropping funnel, and add dropwise the bottom liquid obtained in step 1) for 3 hours. Maintain the temperature of the material in the kettle at 70°C during the addition process. After the addition is completed, raise the temperature of the material in the kettle to 80°C and continue the reaction for 2 hours.

[0086] 3) After the reaction in step 2) is completed, stirring is maintained, 35 parts by weight of pure water is added, the temperature is lowered to 50 ° C and stirred for 2h to obtain a water-soluble alicyclic amine curing agent B with a solid content of 60wt% and an active hydrogen equivalent of 186g / eq.

[0087] 37.8 parts by weight of curing agent B, 37.2 parts by weight of bisphenol A epoxy resin with an epoxy equivalent weight of 189, and 25 parts by weight of pure water were mixed in a container. After standing for 10 minutes, a 100 μm wire rod was used to apply the coating on polished tinplate to test the coating performance. The results are shown in Table 1.

[0088] Example 3

[0089] 1) Add 8 parts by weight of polyethylene glycol diglycidyl ether with an epoxy equivalent of 280g / eq and 3 parts by weight of N,N-dimethyl-1,3-propylenediamine to the reactor and mix well. Then heat to 60°C and keep warm for 1h. After the end of the heat preservation, add 20 parts by weight of isophorone diamine and 10 parts by weight of propylene glycol methyl ether and mix well. Heat to 75°C as the bottom liquid for standby use.

[0090] 2) Mix and dissolve 14 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 and 14 parts by weight of polypropylene glycol diglycidyl ether with an epoxy equivalent of 320 at 30°C, pour into a constant pressure dropping funnel, and add dropwise the bottom solution obtained in step 1) for 3 hours. Maintain the temperature of the contents in the kettle at 75°C during the addition process. After the addition is complete, raise the temperature of the contents in the kettle to 80°C and continue the reaction for 3 hours.

[0091] 3). After the reaction in step 2) was completed, stirring was maintained, 31 parts by weight of pure water was added, the temperature was lowered to 50°C and stirred for 2h to obtain a water-soluble alicyclic amine curing agent C with a solid content of 60wt% and an active hydrogen equivalent of 262g / eq.

[0092] 45.4 parts by weight of curing agent C, 32.6 parts by weight of bisphenol A epoxy resin with an epoxy equivalent weight of 189, and 22 parts by weight of pure water were mixed in a container. After standing for 10 minutes, a 100 μm wire rod was used to apply the coating on polished tinplate to test the coating performance. The results are shown in Table 1.

[0093] Example 4

[0094] 1) Add 5 parts by weight of polyethylene glycol diglycidyl ether with an epoxy equivalent of 280g / eq and 3 parts by weight of 3,3'-iminobis(N,N-dimethylpropylamine) to the reactor and mix well. Then heat to 60°C and keep warm for 1h. After the end of the heat preservation, add 26 parts by weight of isophorone diamine and 6 parts by weight of propylene glycol methyl ether and mix well. Heat to 75°C as the bottom liquid for later use.

[0095] 2) Mix and dissolve 10 parts by weight of 1,6-hexanediol diglycidyl ether and 16 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 at 30°C, pour into a constant pressure dropping funnel, and add dropwise the bottom liquid obtained in step 1) for 3 hours. Maintain the temperature of the material in the kettle at 75°C during the addition process. After the addition is completed, raise the temperature of the material in the kettle to 80°C and continue the reaction for 3 hours.

[0096] 3). After the reaction in step 2) was completed, stirring was maintained, 34 parts by weight of pure water was added, the temperature was lowered to 50°C and stirred for 2h to obtain a water-soluble alicyclic amine curing agent D with a solid content of 60wt% and an active hydrogen equivalent of 218g / eq.

[0097] 41 parts by weight of curing agent D, 35.5 parts by weight of bisphenol A epoxy resin with an epoxy equivalent weight of 189, and 23.5 parts by weight of pure water were mixed in a container. After standing for 10 minutes, the coating was scraped on polished tinplate using a 100 μm wire rod to test the coating properties. The results are shown in Table 1.

[0098] Example 5

[0099] 1) Add 12 parts by weight of polyethylene glycol diglycidyl ether with an epoxy equivalent of 280 g / eq and 3 parts by weight of N,N-dimethyl-1,3-propylenediamine to the reactor and mix evenly. Then heat to 60 ° C and keep warm for 1 hour. After the end of the heat preservation, add 22 parts by weight of 4,4-diaminodicyclohexylmethane and 7 parts by weight of propylene glycol methyl ether and mix evenly. Heat to 75 ° C as the bottom liquid for later use.

[0100] 2) Mix and dissolve 4 parts by weight of 1,6-hexanediol diglycidyl ether, 8 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189, and 9 parts by weight of polypropylene glycol diglycidyl ether with an epoxy equivalent of 320 at 30°C, pour into a constant pressure dropping funnel, and add dropwise the bottom liquid obtained in step 1) for 3 hours. Maintain the temperature of the material in the kettle at 75°C during the addition process. After the addition is completed, raise the temperature of the material in the kettle to 80°C and continue the reaction for 3 hours.

[0101] 3). After the reaction in step 2) was completed, stirring was maintained, 2 parts by weight of propionic acid and 33 parts by weight of pure water were added, the temperature was lowered to 50°C and stirred for 2h to obtain a water-soluble alicyclic amine curing agent E with a solid content of 60wt% and an active hydrogen equivalent of 296g / eq.

[0102] 48.4 parts by weight of curing agent E, 31 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189, and 20.6 parts by weight of pure water were mixed in a container. After standing for 10 minutes, a 100 μm wire rod was used to apply the coating on polished tinplate to test the coating performance. The results are shown in Table 1.

[0103] Example 6

[0104] 1) Add 8 parts by weight of polyethylene glycol diglycidyl ether with an epoxy equivalent of 280g / eq and 3 parts by weight of 3,3'-iminobis(N,N-dimethylpropylamine) to the reactor and mix well. Then heat to 60°C and keep warm for 1h. After the end of the heat preservation, add 28 parts by weight of 4,4-diaminodicyclohexylmethane and 10 parts by weight of propylene glycol methyl ether and mix well. Heat to 75°C as the bottom liquid for later use.

[0105] 2) Mix and dissolve 11 parts by weight of 1,6-hexanediol diglycidyl ether and 9 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189 at 30°C, pour into a constant pressure dropping funnel, and add dropwise the bottom liquid obtained in step 1) for 3 hours. Maintain the temperature of the material in the kettle at 75°C during the addition process. After the addition is completed, raise the temperature of the material in the kettle to 80°C and continue the reaction for 3 hours.

[0106] 3). After the reaction in step 2) was completed, stirring was maintained, 1 part by weight of acetic acid and 30 parts by weight of pure water were added, the temperature was lowered to 50°C and stirred for 2h to obtain a water-soluble alicyclic amine curing agent F with a solid content of 60wt% and an active hydrogen equivalent of 246g / eq.

[0107] 43.8 parts by weight of curing agent F, 33.7 parts by weight of bisphenol A epoxy resin with an epoxy equivalent weight of 189, and 22.5 parts by weight of pure water were mixed in a container. After standing for 10 minutes, a 100 μm wire rod was used to apply the coating on polished tinplate to test the coating performance. The results are shown in Table 1.

[0108] Comparative Example 1

[0109] 7.9 parts by weight of 1,2-cyclohexanediamine, 52.1 parts by weight of bisphenol A epoxy resin with an epoxy equivalent weight of 189, and 40 parts by weight of propylene glycol methyl ether were mixed in a container. After standing for 10 minutes, the coating was scraped onto polished tinplate using a 100 μm wire rod to test the coating properties. The results are shown in Table 1.

[0110] Comparative Example 2

[0111] 11 parts by weight of isophorone diamine, 49 parts by weight of bisphenol A epoxy resin with an epoxy equivalent weight of 189, and 40 parts by weight of propylene glycol methyl ether were mixed in a container and allowed to stand for 10 minutes before being scraped onto polished tinplate using a 100 μm wire rod to test the coating properties; the results are shown in Table 1.

[0112] Comparative Example 3

[0113] 13.1 parts by weight of 4,4-diaminodicyclohexylmethane, 46.9 parts by weight of bisphenol A epoxy resin with an epoxy equivalent of 189, and 40 parts by weight of propylene glycol methyl ether were mixed in a container. After standing for 10 minutes, the coating was scraped onto polished tinplate using a 100 μm wire rod to test the coating properties. The results are shown in Table 1.

[0114] The performance test includes five indicators: gloss, pencil hardness, flexibility, water resistance, and acid resistance of the coating. The coating gloss test refers to the national standard GB / T 9754-2007; the coating pencil hardness test refers to the national standard GB / T 6739-2006; the coating flexibility test refers to the national standard GB / T 1731-1993; the coating water resistance test refers to the national standard GB / T 1733-1993; and the coating acid resistance test refers to the national standard GB / T9274-1988 Method A. All tinplate samples were cured at 50°C for 1 hour and then at 80°C for 2 hours. The test results are shown in Table 1:

[0115] Table 1: Curing properties of water-based alicyclic amine curing agents

[0116]

[0117]

[0118] As is well known to those skilled in the art, the performance of water-based curing agents is generally inferior to that of oil-based curing agents. The above examples demonstrate that the performance of the water-soluble alicyclic amine curing agent prepared in the present invention is extremely close to that of the unmodified oil-based amine curing agent prepared in the comparative example. Furthermore, it possesses the high gloss, high hardness, and good media resistance expected of alicyclic amines. This demonstrates that the present invention addresses the difficulties associated with water-based curing of alicyclic amines, or the difficulty in maintaining the original properties of the raw materials during the water-based curing process. Furthermore, the present invention introduces a toughening chemical structure during the curing agent modification process, significantly improving the coating's flexibility and making it more practical.

[0119] In summary, the present invention provides a water-soluble alicyclic amine curing agent and a preparation method thereof, which uses alicyclic amine as a main raw material and retains the performance characteristics of alicyclic amine to the greatest extent. The performance of the water-soluble alicyclic amine curing agent meets the technical requirements of the industry.

[0120] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A water-soluble alicyclic amine curing agent, characterized in that Made from the following raw materials in parts by weight: The epoxy resin A is a monoepoxy compound or a diepoxy compound containing at least one ethoxy group in its molecular structure; The epoxy resin B is a diepoxy compound having no less than 10 carbon atoms and no ethoxy group; The alicyclic amine comprises at least one of menthanediamine, 1,2-cyclohexanediamine, methylcyclohexanediamine, 4,4-diaminodicyclohexylmethane, and 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane; The tertiary amino fatty amine includes at least one of N,N-dimethylethylenediamine, N,N-dimethyl-1,3-propylenediamine, and 3,3'-iminobis(N,N-dimethylpropylamine).

2. The water-soluble alicyclic amine curing agent according to claim 1, characterized in that The chemical structure of the alicyclic amine contains at least one cyclohexyl group and at least two primary amine groups, and at least one primary amine group is directly connected to the cyclohexyl group; The epoxy equivalent of the epoxy resin A is 100 to 800 g / eq; The tertiary amino fatty amine is an aliphatic amine containing at least one N,N-dimethyl group in its molecular structure; the aliphatic amine contains 2 to 8 carbon atoms and 1 to 2 active hydrogen atoms; The epoxy equivalent of the epoxy resin B is 100 to 350 g / eq; The cosolvent is a monohydric alcohol or alcohol ether compound that is miscible with water in any proportion; the boiling point of the cosolvent is greater than 80°C; The neutralizing agent is a monocarboxylic acid having no more than 4 carbon atoms.

3. The water-soluble alicyclic amine curing agent according to claim 1 or 2, characterized in that: The epoxy resin A comprises at least one of methoxy polyethylene glycol glycidyl ether, ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, triethylene glycol diglycidyl ether and polyethylene glycol diglycidyl ether.

4. The water-soluble alicyclic amine curing agent according to claim 1 or 2, characterized in that: The epoxy resin B comprises at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,2-cyclohexanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, dipropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether and dimer acid diglycidyl ether.

5. The water-soluble alicyclic amine curing agent according to claim 1 or 2, characterized in that: The cosolvent comprises at least one of isopropanol, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether, propylene glycol methyl ether, and dipropylene glycol methyl ether; The neutralizing agent comprises at least one of formic acid, acetic acid, propionic acid, n-butyric acid, glycolic acid, and lactic acid.

6. The method for preparing the water-soluble alicyclic amine curing agent according to any one of claims 1 to 5, characterized in that: The following steps are included: 1). Mix tertiary amino fatty amine and epoxy resin A to obtain an intermediate. 2) Add alicyclic amine and co-solvent to the intermediate obtained in step 1) as the bottom liquid; 3). Add epoxy resin B dropwise into the bottom liquid of the kettle obtained in step 2), and continue the reaction after the addition is completed; 4). After the reaction in step 3) is completed, a neutralizing agent and water are added to obtain the water-soluble alicyclic amine curing agent.

7. The preparation method according to claim 6, characterized in that: The reaction temperature in step 1) is 40-70°C and the reaction time is 0.5-2h; Step 3) the dripping time is 2 to 4 hours, the temperature for continuing the reaction is 60 to 90° C., and the time for continuing the reaction is 1 to 4 hours; After adding the neutralizing agent and water in step 4), the mixture needs to be dispersed at 30-60° C. for 1-3 hours.

8. The preparation method according to claim 7, characterized in that: In step 3), before the epoxy resin B is dripped into the kettle bottom liquid obtained in step 2), the temperature of the kettle bottom liquid is 60-90°C, and the temperature of the epoxy resin B is 20-40°C; In step 4), the reaction product of step 3) needs to be cooled to 40-70° C. before adding the neutralizing agent and water.