A kind of ferrous sulfide cleaning passivation agent and preparation method thereof

By using ferrous sulfide cleaning passivating agent composed of oxidizing agents, composite dispersants, chelating agents and modified agents in oil refining equipment, the spontaneous combustion and pollution problems caused by ferrous sulfide accumulation are solved, and the efficient removal of ferrous sulfide scale and harmfulness is achieved. The effect of gas improves the safety and environmental protection of equipment.

CN117488293BActive Publication Date: 2024-11-05SHANDONG BINHE NEW MATERIALS CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202311475583.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-08
Publication Date
2024-11-05
Estimated Expiration
2043-11-08

AI Technical Summary

Technical Problem

During the oil refining process, the accumulation of ferrous sulfide in the equipment can easily lead to spontaneous combustion accidents, and contaminate odors such as hydrogen sulfide, which poses safety hazards and environmental hazards.

Method used

Using a ferrous sulfide cleaning passivation agent composed of oxidant, composite dispersant, chelating agent and modification agent, the ferrous sulfide scale in the equipment is efficiently removed and prevented by spontaneous combustion. and reduce the release of hydrogen sulfide and ammonia nitrogen.

Benefits of technology

Effectively prevent ferrous sulfide spontaneous combustion, improve equipment operation efficiency and safety, remove harmful gases such as hydrogen sulfide and ammonia nitrogen, and reduce environmental and human harm. It has the characteristics of efficiency, safety and environmental protection.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of chemical passivators, and specifically relates to a ferrous sulfide cleaning passivator and a preparation method thereof. The ferrous sulfide cleaning passivator provided by the present invention comprises the following components and their weight proportions: 5 to 10 parts of an oxidant, 1 to 3 parts of a composite dispersant, 0.5 to 1.5 parts of a chelating agent, 1 to 3 parts of an improver, and 79 to 90 parts of water. The ferrous sulfide cleaning passivator provided by the present invention can efficiently clean and passivate the ferrous sulfide scale deposited on a petrochemical device through the combined action of a reasonable ratio of an oxidant, a composite dispersant, a chelating agent and an improver, effectively preventing the occurrence of ferrous sulfide spontaneous combustion, and at the same time, can also remove harmful gases such as hydrogen sulfide and ammonia nitrogen in the device, reducing harm to the environment and human body, and has the characteristics of high efficiency, safety, and environmental protection, and can be widely used in the cleaning of petroleum refining production devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical passivators, and in particular relates to a ferrous sulfide cleaning passivator and a preparation method thereof. Background Art

[0002] In the oil refining process, elemental iron is ubiquitous in pipeline equipment, which causes a series of chemical reactions between various active sulfur and elemental iron in the crude oil processing process, and finally accumulates in large space, low flow rate towers and containers in the form of ferrous sulfide. The distribution of ferrous sulfide in process equipment generally follows this rule: the higher the sulfur content in the medium, the more ferrous sulfide corrosion products it produces. However, when the equipment with a sulfur content of only a few parts per million in the medium is turned on, ferrous sulfide will also spontaneously combust. The reason is not the high sulfur content in the medium, but the fine ferrous sulfide corrosion products will continue to transfer from upstream to downstream with the material, and continue to gather and settle in a relatively low speed area. For tower equipment, the material flow rate in the device is low, and the corrosion products of ferrous sulfide are easy to deposit in some local areas, especially in packed towers. In addition to the function of fractionation, the packing also has a high-efficiency filtering function, and the ferrous sulfide carried from the upstream is easily intercepted. At the same time, metal packing has a large specific surface area and a large contact area with the material, so it will corrode the packing even if the sulfur content in the material is very low. Since the material flow rate in the packed tower is low, the ferrous sulfide generated by the corrosion of the packing surface is difficult to be carried away by the material. Therefore, in a packed tower that is operated continuously for a large load, a long period, or multiple periods, a certain amount of ferrous sulfide will accumulate in the tower.

[0003] During downtime such as maintenance, these ferrous sulfides react with oxygen in the air to produce exothermic chemical reactions. If the heat released cannot be released and transmitted in time, it will generate high temperatures and damage the equipment. Especially in towers and containers with many internal components such as packings and trays, the accumulation of ferrous sulfide is large, which is very likely to cause spontaneous combustion accidents.

[0004] How to prevent ferrous sulfide from spontaneous combustion and hydrogen sulfide odor pollution, and ensure the safety of personnel and equipment during the overhaul of refining equipment is of great significance. Therefore, a technical problem that needs to be solved is to provide an environmentally friendly and efficient ferrous sulfide passivation agent that can quickly passivate ferrous sulfide, effectively prevent ferrous sulfide from spontaneous combustion, and at the same time have a good cleaning effect on odorous substances such as hydrogen sulfide. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide a ferrous sulfide cleaning passivation agent and a preparation method thereof. The ferrous sulfide cleaning passivation agent provided by the present invention can efficiently clean and passivate the ferrous sulfide scale deposited on the petrochemical device, effectively prevent the occurrence of ferrous sulfide spontaneous combustion, and can also remove harmful gases such as hydrogen sulfide and ammonia nitrogen in the device, reducing the harm to the environment and human body, and has the characteristics of high efficiency, safety, environmental protection, etc., and can be widely used in the cleaning of petroleum refining production equipment.

[0006] The technical solution of the present invention is:

[0007] A ferrous sulfide cleaning passivation agent, comprising the following components and their weight proportions:

[0008] 5-10 parts of oxidant, 1-3 parts of composite dispersant, 0.5-1.5 parts of chelating agent, 1-3 parts of improver, and 79-90 parts of water.

[0009] Preferably, the ferrous sulfide cleaning passivation agent is composed of the following components and their weight proportions:

[0010] 7 parts of oxidant, 2 parts of composite dispersant, 1 part of chelating agent, 2 parts of improver, and 85 parts of water.

[0011] Preferably, the oxidant is potassium permanganate.

[0012] Preferably, the composite dispersant is composed of sodium sulfate, triethanolamine oleate soap and octylphenol polyoxyethylene ether in a weight ratio of 1 to 3:5 to 8:3.

[0013] Preferably, the CAS number of the triethanolamine oleic acid soap is 10277-04-0; the CAS number of the octylphenol polyoxyethylene ether is 9036-19-5.

[0014] Further preferably, the composite dispersant is composed of sodium sulfate, triethanolamine oleate soap and octylphenol polyoxyethylene ether in a weight ratio of 2:7:3.

[0015] Preferably, the chelating agent is at least two of tetrasodium ethylenediaminetetraacetate, sodium diethyldithiophosphate, sodium hexametaphosphate, and sodium tartrate.

[0016] Preferably, the CAS number of the tetrasodium ethylenediaminetetraacetate is 64-02-8; the CAS number of the sodium diethyl dithiophosphate is 3338-24-7; the CAS number of the sodium hexametaphosphate is 10124-56-8; and the CAS number of the sodium tartrate is 6106-24-7.

[0017] Preferably, the improver is composed of sodium carbonate, disodium hydrogen phosphate and N-methyldiethanolamine in a weight ratio of 0.5-2:0.5-2:3-5.

[0018] Preferably, the improver consists of sodium carbonate, disodium hydrogen phosphate and N-methyldiethanolamine in a weight ratio of 1:1:4.

[0019] In addition, the present invention also provides a method for preparing a ferrous sulfide cleaning passivation agent, comprising the following steps:

[0020] S1. Turn on the stirrer and slowly add the composite dispersant and oxidant into the water for 20 to 35 minutes to obtain a mixed solution I;

[0021] S2, slowly stirring and adding the improver to the mixed solution I obtained in step S1, controlling the reaction temperature during the feeding process to be less than 65° C., and the time required for the entire feeding process is 20 to 35 minutes, to obtain a mixed solution II;

[0022] S3, slowly stirring and adding the chelating agent to the mixed solution II obtained in step S2, controlling the reaction temperature during the feeding process to be less than 65° C., and the time required for the entire feeding process is 20 to 30 minutes, to obtain the product.

[0023] The stirring speed in step S1 is 100-150 r / min; the stirring speed in step S2 is 150-300 r / min; and the stirring time in step S3 is 150-200 r / min.

[0024] The ferrous sulfide cleaning and passivating agent provided by the present invention forms a water-soluble cleaning and passivating agent by adding an oxidant, a composite dispersant, a chelating agent and an improver in appropriate proportions. The cleaning and passivating agent can be applied to the cleaning of petroleum refining production equipment and the cleaning of sediments on petrochemical equipment. The principle is mainly to efficiently remove ferrous sulfide scale in the equipment through the wetting, dispersion, oxidation and chelation effects of the cleaning and passivating agent on the equipment.

[0025] The added oxidant is potassium permanganate, which can form a crystal protective film on the metal surface of the production equipment while oxidizing the ferrous sulfide, thereby effectively preventing the sulfide from contacting the metal to react and produce ferrous sulfide again, thereby protecting the equipment. The chelating agent (selected from at least two of tetrasodium ethylenediaminetetraacetic acid, sodium diethyl dithiophosphate, sodium hexametaphosphate, and sodium tartrate) added by the present invention can convert ferrous sulfide into soluble iron oxide and sulfur, thereby preventing ferrous sulfide from directly contacting the air and spontaneous combustion, and is also conducive to improving the removal efficiency of ferrous sulfide and sulfide, reducing the release of hydrogen sulfide gas, and reducing the generation of secondary pollution.

[0026] Furthermore, the dispersant added by the present invention, which is composed of sodium sulfate, triethanolamine oleic acid soap and octylphenol polyoxyethylene ether in a specific ratio, can effectively enhance the penetration of the oxidant and the chelating agent in the dirt layer, separate the formed dirt, thoroughly contact and clean the attached matter, thereby facilitating the removal of deep-layer ferrous sulfide.

[0027] At the same time, the added modifier can assist in enhancing the passivation effect of the oxidant and the complexing agent on ferrous sulfide, thereby effectively improving the passivation efficiency of ferrous sulfide, reducing and facilitating the formation of an oxide film on the surface of metal equipment, effectively inhibiting the oxidation of the metal, reducing the corrosion to the equipment, and reducing the release of harmful gases such as hydrogen sulfide and ammonia.

[0028] Compared with the prior art, the ferrous sulfide cleaning passivation agent provided by the present invention has the following advantages:

[0029] (1) The ferrous sulfide cleaning and passivation agent provided by the present invention can efficiently clean and passivate the ferrous sulfide scale deposited on the petrochemical equipment through the combined action of a reasonable ratio of an oxidant, a composite dispersant, a chelating agent and a modifier, effectively preventing the occurrence of spontaneous combustion of ferrous sulfide, improving the operating efficiency and safety of the equipment, having the characteristics of high efficiency, safety and environmental protection, and can be widely used in the cleaning of petroleum refining production equipment.

[0030] (2) The ferrous sulfide cleaning passivation agent provided by the present invention can also remove harmful gases such as hydrogen sulfide and ammonia nitrogen in petrochemical equipment, thereby reducing harm to the environment and human body. DETAILED DESCRIPTION

[0031] The present invention is further illustrated below through the description of specific implementation methods, but this is not a limitation of the present invention. Those skilled in the art can make various modifications or improvements based on the basic idea of ​​the present invention, but as long as they do not deviate from the basic idea of ​​the present invention, they are all within the protection scope of the present invention.

[0032] In the following examples and comparative examples, reagents not otherwise specified are conventional reagents and can be purchased from conventional reagent production and sales companies. The methods used are all prior art unless otherwise specified.

[0033] Example 1

[0034] A ferrous sulfide cleaning passivation agent, comprising the following components and their weight proportions:

[0035] 5kg potassium permanganate, 1kg composite dispersant, 0.5kg chelating agent, 1kg improver, 79kg water.

[0036] The composite dispersant is composed of sodium sulfate, triethanolamine oleic acid soap and octylphenol polyoxyethylene ether in a weight ratio of 1:8:3.

[0037] The chelating agent is composed of tetrasodium ethylenediaminetetraacetate and sodium hexametaphosphate in a weight ratio of 1:1.

[0038] The improver is composed of sodium carbonate, disodium hydrogen phosphate and N-methyldiethanolamine in a weight ratio of 0.5:2:5.

[0039] The preparation method of the ferrous sulfide cleaning passivation agent comprises the following steps:

[0040] S1, turn on the stirrer, add the composite dispersant and potassium permanganate into the water at a stirring speed of 100r / min, and the feeding time is 35min to obtain a mixed solution I;

[0041] S2, adding the improver to the mixed solution I obtained in step S1 at a stirring speed of 150 r / min, controlling the reaction temperature during the feeding process to be less than 65° C., and the time required for the entire feeding process is 35 min, to obtain a mixed solution II;

[0042] S3, adding a chelating agent to the mixed solution II obtained in step S2 at a stirring speed of 150 r / min, controlling the reaction temperature during the feeding process to be less than 65° C., and the time required for the entire feeding process is 30 min.

[0043] Example 2

[0044] A ferrous sulfide cleaning passivation agent, comprising the following components and their weight proportions:

[0045] Potassium permanganate 7kg, composite dispersant 2kg, chelating agent 1kg, improver 2kg, water 85kg.

[0046] The composite dispersant is composed of sodium sulfate, triethanolamine oleic acid soap and octylphenol polyoxyethylene ether in a weight ratio of 2:7:3.

[0047] The chelating agent is composed of sodium diethyl dithiophosphate, sodium hexametaphosphate and sodium tartrate in a weight ratio of 3:1:1.

[0048] The improver is composed of sodium carbonate, disodium hydrogen phosphate and N-methyldiethanolamine in a weight ratio of 1:1:4.

[0049] The preparation method of the ferrous sulfide cleaning passivation agent comprises the following steps:

[0050] S1, turn on the stirrer, add the composite dispersant and potassium permanganate into the water at a stirring speed of 120r / min, and the feeding time is 30min to obtain a mixed solution I;

[0051] S2, adding the improver to the mixed solution I obtained in step S1 at a stirring speed of 250 r / min, controlling the reaction temperature during the feeding process to be less than 65° C., and the time required for the entire feeding process is 30 min, to obtain a mixed solution II;

[0052] S3, adding a chelating agent to the mixed solution II obtained in step S2 at a stirring speed of 180 r / min, controlling the reaction temperature during the feeding process to be less than 65° C., and the time required for the entire feeding process is 25 min.

[0053] Example 3

[0054] A ferrous sulfide cleaning passivation agent, comprising the following components and their weight proportions:

[0055] 10kg potassium permanganate, 3kg composite dispersant, 1.5kg chelating agent, 3kg improver, 90kg water.

[0056] The composite dispersant is composed of sodium sulfate, triethanolamine oleic acid soap and octylphenol polyoxyethylene ether in a weight ratio of 3:5:3.

[0057] The chelating agent is composed of tetrasodium ethylenediaminetetraacetate, sodium diethyldithiophosphate, sodium hexametaphosphate and sodium tartrate in a weight ratio of 1:1:1:1.

[0058] The improver is composed of sodium carbonate, disodium hydrogen phosphate and N-methyldiethanolamine in a weight ratio of 2:0.5:3.

[0059] The preparation method of the ferrous sulfide cleaning passivation agent comprises the following steps:

[0060] S1, turn on the stirrer, add the composite dispersant and potassium permanganate into the water at a stirring speed of 150r / min, and the feeding time is 20min to obtain a mixed solution I;

[0061] S2, adding the improver to the mixed solution I obtained in step S1 at a stirring speed of 300 r / min, controlling the reaction temperature during the feeding process to be less than 65° C., and the time required for the entire feeding process is 20 min, to obtain a mixed solution II;

[0062] S3, adding a chelating agent to the mixed solution II obtained in step S2 at a stirring speed of 200 r / min, controlling the reaction temperature during the feeding process to be less than 65° C., and the time required for the entire feeding process is 20 min.

[0063] Comparative Example 1

[0064] Compared with Example 2, the difference of Comparative Example 1 is that potassium permanganate is replaced by potassium ferrate, and other components and preparation methods are the same as those of Example 2.

[0065] Comparative Example 2

[0066] Compared with Example 2, the difference of Comparative Example 2 is that the octylphenol polyoxyethylene ether in the composite dispersant is replaced with lauryl alcohol polyoxyethylene ether (CAS No. 9002-92-0), that is, the composite dispersant is composed of sodium sulfate, triethanolamine oleic acid soap and lauryl alcohol polyoxyethylene ether in a weight ratio of 2:7:3. Other components and preparation methods are the same as those in Example 2.

[0067] Comparative Example 3

[0068] Compared with Example 2, the difference of Comparative Example 3 is that octylphenol polyoxyethylene ether is not added to the composite dispersant, and the dosage of the other two components is increased accordingly, that is, the composite dispersant is composed of sodium sulfate and triethanolamine oleic acid soap in a weight ratio of 3:9. The other components and preparation method are the same as those in Example 2.

[0069] Comparative Example 4

[0070] Compared with Example 2, the difference of Comparative Example 4 is that the sodium diethyl dithiophosphate in the chelating agent is replaced with ethylene triamine pentaacetic acid (CAS No. 67-43-6), that is, the chelating agent is composed of ethylene triamine pentaacetic acid, sodium hexametaphosphate and sodium tartrate in a weight ratio of 3:1:1. Other components and preparation methods are the same as those in Example 2.

[0071] Test Example 1: Cleaning Effect Detection

[0072] 1. Test materials: ferrous sulfide passivation cleaning agents prepared in Examples 1 to 3 and Comparative Examples 1 to 4 of the present invention.

[0073] 2. Test method: 1L of the ferrous sulfide passivation cleaning agent prepared in Examples 1 to 3 and Comparative Examples 1 to 4 of the present invention was placed in a beaker, and then 50g of the ferrous sulfide sample was added thereto. After treating for 1 hour, the mixture was filtered, and the residue was weighed after drying to calculate the removal rate (%) of ferrous sulfide. The test results are shown in Table 1.

[0074] Table 1

[0075] Group Ferrous sulfide removal rate (%) Example 1 98.7 Example 2 99.3 Example 3 99.1 Comparative Example 1 89.3 Comparative Example 2 93.9 Comparative Example 3 91.5 Comparative Example 4 95.4

[0076] As can be seen from Table 1, the ferrous sulfide cleaning and passivating agents prepared by Examples 1 to 3 of the present invention have excellent removal effects on ferrous sulfide samples, and the removal rates of ferrous sulfide are all above 98%. Among them, the removal rate of ferrous sulfide in Example 2 is as high as 99.3%, which is the best embodiment of the present invention. In Comparative Examples 1 to 4, when the components of the ferrous sulfide cleaning and passivating agents provided by the present invention are changed, the removal rates of ferrous sulfide have decreased to varying degrees, which fully demonstrates that the components in the ferrous sulfide cleaning and passivating agents provided by the present invention work together, and the synergistic effect is obvious, which can effectively improve the removal rate of ferrous sulfide and prevent the ferrous sulfide in the equipment from contacting with air and spontaneously igniting.

[0077] Test Example 2: Actual Production Application Test

[0078] 1. Test materials: Ferrous sulfide passivation cleaning agents prepared in Example 2 of the present invention and Comparative Examples 1 to 4.

[0079] 2. Test method: (1) The ferrous sulfide cleaning and passivation agents prepared in Example 2 of the present invention and Comparative Examples 1 to 4 were added to the petrochemical equipment in a shutdown state for 6 to 8 hours to complete the one-step cleaning of the ferrous sulfide passivation, deodorization, and degreasing. After the treatment was completed, the cleaning and passivation effect was checked, including the descaling rate of ferrous sulfide (%), the concentration of hydrogen sulfide and ammonia in the equipment after cleaning (mg / m 3 ). The test results are shown in Table 2.

[0080] (2) The concentrations of COD (mg / L) and sulfide (mg / L) in the waste liquid of ferrous sulfide cleaning passivation agent in Example 2 and Comparative Examples 1 to 4 after cleaning in step (1) were respectively tested. The test results are shown in Table 3.

[0081] Table 2

[0082] Group Ferrous sulfide descaling rate (%) <![CDATA[H2S(mg / m 3 )]]> <![CDATA[NH3(mg / m 3 )]]> Example 2 98.3 0.03 0.5 Comparative Example 1 87.3 1.2 0.9 Comparative Example 2 92.6 3.1 1.6 Comparative Example 3 90.4 3.9 3.2 Comparative Example 4 93.1 6.3 7.9

[0083] Table 3

[0084] Group COD(mg / L) Sulfide (mg / L) Example 2 269 9.2 Comparative Example 1 283 14.3 Comparative Example 2 277 13.2 Comparative Example 3 292 13.9 Comparative Example 4 271 11.6

[0085] As shown in Table 2, after the ferrous sulfide cleaning and passivation agent prepared in Example 2 of the present invention is used to clean the petrochemical equipment, the descaling rate of ferrous sulfide in the equipment can reach 98.3%, and the contents of hydrogen sulfide and ammonia in the equipment after cleaning can meet the emission requirements of GB 14554-93 "Emission Standards for Malodorous Pollutants". It can be seen that the ferrous sulfide cleaning and passivation agent prepared in the present invention can effectively improve the descaling rate of ferrous sulfide while effectively reducing the release of harmful gases such as hydrogen sulfide and ammonia.

[0086] At the same time, it can be seen from Table 3 that after the petrochemical equipment is cleaned by the ferrous sulfide cleaning passivation agent prepared in Example 2 of the present invention, the COD concentration in the treated waste liquid is 269 mg / L, and the sulfide concentration is 9.2 mg / L. The COD and sulfide contents in the waste liquid are low, which can reduce the burden of subsequent sewage treatment, improve treatment efficiency, and be more environmentally friendly.

[0087] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A ferrous sulfide cleaning passivation agent, characterized in that, It includes the following components and their weight parts: 5-10 parts of oxidant, 1-3 parts of composite dispersant, 0.5-1.5 parts of chelating agent, 1-3 parts of improver, 79-90 parts of water; The composite dispersant is composed of sodium sulfate, triethanolamine oleic acid soap and octylphenol polyoxyethylene ether in a weight ratio of 1-3:5-8:3; the chelating agent is at least two of tetrasodium ethylenediaminetetraacetate, sodium diethyl dithiophosphate, sodium hexametaphosphate and sodium tartrate; the improver is composed of sodium carbonate, disodium hydrogen phosphate and N-methyldiethanolamine in a weight ratio of 0.5-2:0.5-2:3-5.

2. The ferrous sulfide cleaning passivation agent according to claim 1, characterized in that: It is composed of the following components and their weight parts: 7 parts of oxidant, 2 parts of composite dispersant, 1 part of chelating agent, 2 parts of improver, and 85 parts of water.

3. The ferrous sulfide cleaning passivation agent according to claim 1, characterized in that: The composite dispersant is composed of sodium sulfate, triethanolamine oleic acid soap and octylphenol polyoxyethylene ether in a weight ratio of 2:7:

3.

4. A method for preparing the ferrous sulfide cleaning passivation agent according to any one of claims 1 to 3, characterized in that: The steps include: S1. Turn on the stirrer and slowly add the composite dispersant and oxidant into the water for 20 to 35 minutes to obtain a mixed solution I; S2, slowly stirring and adding the improver to the mixed solution I obtained in step S1, controlling the reaction temperature during the feeding process to be less than 65° C., and the time required for the entire feeding process is 20 to 35 minutes, to obtain a mixed solution II; S3, slowly stirring and adding the chelating agent to the mixed solution II obtained in step S2, controlling the reaction temperature during the feeding process to be less than 65° C., and the time required for the entire feeding process is 20 to 30 minutes, to obtain the product.

5. The method for preparing the ferrous sulfide cleaning passivating agent according to claim 4, characterized in that: The stirring speed in step S1 is 100-150 r / min; the stirring speed in step S2 is 150-300 r / min; and the stirring time in step S3 is 150-200 r / min.

Citation Information

Patent Citations

  • Chemical cleaning agent for clearing impurities such as ferrous sulfide

    CN102345136A

  • Ferrous sulfide passivation cleaning agent and preparation method and application thereof

    CN102912366A

  • Multi-effect compound antioxidant colloid reducer for gasoline

    CN103351893A

  • Compound chelating agent for stabilizing soil heavy metal

    CN106833669A

  • Hydrogen sulfide cleaning deodorant as well as preparation method and use method thereof

    CN111545034A