Polylactide resin compositions with excellent crystallinity and half-life and their preparation methods

By incorporating nucleating agents with uracil and lactide monomer oligomer structures into polylactide resin, the problem of slow crystallization rate of polylactide resin was solved, achieving efficient crystallization and excellent crystallinity, thereby improving production efficiency and transparency.

CN117500871BActive Publication Date: 2026-11-17LG CHEM LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380012053.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-03-22
Filing Date
2023-02-27
Publication Date
2026-11-17
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

Existing polylactide resins have a slow crystallization rate, resulting in long molding cycles. Furthermore, traditional nucleating agents may increase the resin's specific gravity and reduce its transparency. In addition, there are dispersion problems between traditional nucleating agents and PLA resins.

Method used

A polylactide resin composition was prepared by melt blending a combination of bio-based uracil as the first nucleating agent and a second nucleating agent containing lactide monomer oligomer structure with polylactide resin, thereby improving the crystallization half-life and crystallinity.

Benefits of technology

At crystallization temperatures of 100°C to 130°C, the crystallization half-life of the polylactide resin composition is significantly shortened to less than 5 minutes, while maintaining excellent crystallinity and transparency, thus improving production efficiency and physical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117500871B_ABST
    Figure CN117500871B_ABST
Patent Text Reader

Abstract

This disclosure relates to polylactide resin compositions used in combination with specific nucleating agents, the polylactide resin compositions having excellent crystallization half-life and crystallinity, thus being able to retain the inherent properties of the polylactide resin according to this disclosure, while having excellent processability.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] Cross-references to related applications

[0002] This application claims the benefit of Korean Patent Application No. 10-2022-0035552, filed with the Korean Intellectual Property Office on March 22, 2022, the disclosure of which is incorporated herein by reference in its entirety.

[0003] This invention relates to polylactide resin compositions with excellent crystallization half-life and methods for preparing the same. [Background Technology]

[0004] Polylactide (or polylactic acid; PLA) resin is made from biomass materials and is an environmentally friendly material. Its production process releases relatively little carbon dioxide, a global warming gas, and it degrades through specific temperatures and composting facilities. In recent years, as one of the materials that can replace existing crude oil-based resins, it has also received attention as a means of upgrading and recycling waste plastics and regulating carbon emissions.

[0005] In addition, polylactide resin has the advantages of being cheaper than other biodegradable polymers and having high tensile strength and modulus properties.

[0006] However, polylactide resins have the following problems: the rigid polymer backbone repeats with short units, the crystallization rate is slow due to slow chain mobility, and the molding cycle is long, thus reducing productivity. Therefore, in order to improve these problems, much research is underway to introduce materials such as nucleating agents to improve productivity and heat resistance.

[0007] Typically, the materials used as nucleating agents are mainly inorganic nucleating agents, and materials such as talc, mica and nanoclay have been reported to be used, and some of them are added during PLA molding to improve heat resistance and strength.

[0008] However, excessive addition of this nucleating agent leads to increased resin density and decreased transparency. On the other hand, organic nucleating agents such as LAK301 (an aromatic sulfonate derivative), sodium benzoate, N-aminophthalimide, phthalohydrazide, and cadmium phenylmalonate are used to improve crystallinity and transparency. However, these materials are not bio-based and exhibit dispersion problems with PLA resin.

[0009] Therefore, there is a need to introduce bio-based organic nucleating agents that can be prepared in environmentally friendly products without compromising transparency. Furthermore, there is a need to introduce nucleating agents that have fewer dispersion problems with polylactide resins to further improve the crystallization half-life and crystallinity of polylactide resins. [Summary of the Invention]

[0010] [Technical Issues]

[0011] The purpose of this disclosure is to provide polylactide resin compositions that have excellent crystallization half-life when used in combination with specific nucleating agents.

[0012] Another object of this disclosure is to provide a method for preparing polylactide resin compositions.

[0013] [Technical Solution]

[0014] To achieve the above objectives, the following polylactide resin composition is provided according to this disclosure:

[0015] A polylactide resin composition comprising polylactide resin; a first nucleating agent; and a second nucleating agent.

[0016] The polylactide resin composition has a crystallization half-life of less than 2 minutes at a crystallization temperature of 100°C to 130°C.

[0017] As used herein, the term "polylactide resin" is defined broadly as a homopolymer or copolymer comprising repeating units represented by the following chemical formula.

[0018]

[0019] Polylactide resin can be prepared by a method including the step of forming the aforementioned repeating units through ring-opening polymerization of lactide monomers. The polymer obtained after completing this ring-opening polymerization and forming the repeating units can be called "polylactide resin".

[0020] At this point, the term "lactide monomer" can be defined as follows. Generally, lactides can be classified into L-lactides composed of L-lactic acid, D-lactides composed of D-lactic acid, and meso-lactides composed of both L- and D-type lactides. Similarly, a mixture of L-lactides and D-lactides in a 50:50 ratio is called D,L-lactides or racemic lactides. Among these lactides, polymerization processes using only L-lactides and D-lactides with high levels of optical purity are known to produce L- or D-polylactides (PLLA or PDLA) with high levels of stereoregularity. These polylactides exhibit faster crystallization rates and higher crystallinity compared to polylactides with lower levels of optical purity. However, the term "lactide monomer" is defined to include all types of lactides, regardless of the differences in properties depending on the type of lactide and the resulting polylactide resin.

[0021] Meanwhile, as an example, the polylactide resin composition according to this disclosure has a weight-average molecular weight of 70,000 to 400,000.

[0022] The present disclosure is characterized by the use of polylactide resin in combination with a first nucleating agent and a second nucleating agent, thereby improving the crystallization half-life of the polylactide resin.

[0023] Specifically, the polylactide resin composition is characterized by a crystallization half-life of 5 minutes or less at a crystallization temperature of 100°C to 130°C. Preferably, the crystallization half-life is 1.9 minutes or less, 1.8 minutes or less, 1.7 minutes or less, 1.6 minutes or less, 1.5 minutes or less, 1.4 minutes or less, 1.3 minutes or less, 1.2 minutes or less, 1.1 minutes or less, or 1.0 minute or less. Furthermore, the crystallization half-life is 0.1 minutes or more, 0.2 minutes or more, 0.3 minutes or more, 0.4 minutes or more, or 0.5 minutes or more.

[0024] The term "crystallization half-life" used in this article is "crystallization half-life (t)". 1 / 2 "50% crystallization" refers to the time (in minutes) required to achieve 50% crystallization and is a useful indicator for evaluating the relative crystallization rate. To determine the crystallization half-life, the relative crystallinity is first measured. Relative crystallinity is the ratio of the total area of ​​the exothermic peak over time during isothermal crystallization to the area at time t. After converting this to relative crystallinity over time, the time when the relative crystallinity reaches 0.5 can be determined as the crystallization half-life. Figure 1 The process is illustrated schematically, and more detailed measurement methods can be shown in the embodiments described later.

[0025] As used herein, the term "crystallization temperature" refers to the temperature at which polylactide resin is melted to a predetermined temperature and then cooled to measure its crystallization half-life. For example, when polylactide resin is melted at 200°C and then cooled to 120°C at a cooling rate of 40°C / min to 100°C / min, 120°C is referred to as the "crystallization temperature." In this disclosure, the crystallization temperature is 100 to 130°C, for example, 100°C, 110°C, 120°C, or 130°C. Specific methods for measuring the crystallization half-life based on the crystallization temperature can be illustrated in the following examples.

[0026] Preferably, the polylactide resin composition according to the invention has a crystallinity of 35% or more at a crystallization temperature of 100 to 130°C. As described above, the polylactide resin composition according to the invention is characterized by having not only an excellent crystallization half-life but also an excellent crystallinity. Preferably, the crystallinity is 40% or more, 45% or more, or 50% or more. A method for measuring crystallinity can be illustrated in the following examples.

[0027] Meanwhile, the first nucleating agent is uracil. The first nucleating agent is a bio-based organic material, which is added to polylactide resin to act as a nucleation site and induce crystal nucleation at high temperature, thereby improving the crystallization half-life and crystallinity.

[0028] Preferably, the content of the first nucleating agent is 0.1 to 5% by weight, based on the total weight of the polylactide resin composition. If the content is less than 0.1% by weight, the effect of using the first nucleating agent is not significant, while if the content exceeds 5% by weight, there is a risk of impairing the inherent physical properties of the polylactide resin. More preferably, the content of the first nucleating agent is 0.2% by weight or more, 0.3% by weight or more, 0.4% by weight or more, or 0.5% by weight or more; and less than 4.5% by weight, less than 4.0% by weight, or less than 3.5% by weight.

[0029] The second nucleating agent is a nucleating agent containing an oligomer structure of lactide monomer. Due to the oligomer structure of lactide monomer, it has high compatibility with polylactide resin and is added to polylactide resin to act as a plasticizer. Therefore, it can form free volumes in polylactide resin, thereby enhancing the chain mobility of polylactide resin and increasing the crystallization half-life.

[0030] Preferably, the second nucleating agent is a compound represented by the following chemical formula 1:

[0031] [Chemical Formula 1]

[0032]

[0033] In chemical formula 1,

[0034] L is:

[0035]

[0036] in,

[0037] n1 is an integer from 1 to 30.

[0038] R is a substituent represented by the following chemical formula 2.

[0039] [Chemical Formula 2]

[0040]

[0041] in,

[0042] n represents the number of repeating units, and

[0043] R' is hydrogen or acetyl.

[0044] The weight-average molecular weight of the second nucleating agent can be adjusted according to the number of each lactide repeating unit. Preferably, the weight-average molecular weight of the second nucleating agent is from 1,000 to 50,000. More preferably, the weight-average molecular weight of the second nucleating agent is 1,100 or more, 1,200 or more, 1,300 or more, 1,400 or more, or 1,500 or more; and 40,000 or less, 30,000 or less, 20,000 or less, 10,000 or less, 9,000 or less, or 8,000 or less.

[0045] Preferably, the content of the second nucleating agent is 3 to 25% by weight, based on the total weight of the polylactide resin composition. If the content is less than 3% by weight, the effect of using the second nucleating agent is not significant, while if the content exceeds 25% by weight, there is a risk of impairing the inherent physical properties of the polylactide resin. More preferably, the content of the second nucleating agent is 3.5% by weight or more, 4.0% by weight or more, or 4.5% by weight or more; and less than 24% by weight, less than 23% by weight, less than 22% by weight, or less than 21% by weight.

[0046] Furthermore, the method for preparing the polylactide resin composition according to this disclosure is not particularly limited, as long as it involves mixing the polylactide resin, the first nucleating agent, and the second nucleating agent. In one example, the above components can be prepared by melt blending.

[0047] [Beneficial Effects]

[0048] The polylactide resin composition according to this disclosure has excellent crystallization half-life and crystallinity. Therefore, the polylactide resin composition according to this disclosure can retain the inherent properties of the polylactide resin according to this disclosure, while having excellent processability. [Image Description]

[0049] Figure 1 The meaning of the crystallization half-life according to this disclosure is illustrated schematically. [Detailed Implementation]

[0050] The embodiments of this disclosure will now be described in more detail with reference to examples. However, the following examples are for illustrative purposes only and are not intended to limit the scope of this disclosure.

[0051] Preparation Example 1: Preparation of the Second Nucleating Agent (P10-A-002)

[0052] Oligomers were prepared using PEG-1000 (P10) as an initiator. Specifically, lactide and P10 were added to a 20 mL vial at a molar ratio of 8:1, resulting in a total volume of 4.5 g. Sn(Oct)2 catalyst was added in an amount of 0.1 to 0.2 wt%, and the reaction was carried out at 130 °C for 4 hours. After adjusting the temperature to 120 °C, acetic anhydride (4 equivalents relative to the terminal OH groups) was added, and the reaction was further carried out for 12 hours. After the reaction was complete, acetic acid and residual acetic anhydride, which were byproducts, were removed by vacuum drying to prepare a second nucleating agent having a structure in which the terminal groups were substituted with acetyl groups. This agent was named P10-A-002, and its weight-average molecular weight is shown in Table 1 below.

[0053] Examples and Comparative Examples

[0054] Melt blending was performed using a Haake mixer. Specifically, 65 g of PLA granules (4032D from Natureworks; weight average molecular weight approximately 200,000) were added, along with the first and second nucleating agents shown in Table 1 below, according to their respective contents. The nucleating agent in powder form was mixed with the PLA granules and added thereto. The nucleating agent, with a melting point below the process operating temperature (180°C), was blended for 5 minutes (until the PLA was completely dissolved), and then added to the hopper. The operation was carried out at 180°C, 60 rpm, and 10 minutes. The resulting PLA resin was subjected to isothermal DSC analysis as described below to confirm the crystallization behavior at each crystallization temperature.

[0055] Experimental Example

[0056] The physical properties of the first nucleating agent, the second nucleating agent, and the polylactide resin composition prepared above were measured using the following methods.

[0057] 1) Weight-average molecular weight

[0058] The number-average molecular weight (Mn) and weight-average molecular weight (Mw) were calculated using a GPC (gel permeation chromatography) apparatus, and the molecular weight distribution of oligomers (Mw / Mn) was measured under the following specific measurement conditions.

[0059] - Column: PL gel mixture E x 2

[0060] Solvent: THF

[0061] - Flow rate: 0.7 mL / min

[0062] - Sample concentration: 3.0 mg / mL

[0063] Injection volume: 100μl

[0064] - Column temperature: 40℃

[0065] - Detector: Waters 2414RID

[0066] -Standard: PS (Polystyrene)

[0067] 2) DSC (Differential Scanning Calorimetry)

[0068] The PLA resins prepared in the examples and comparative examples were completely melted at 200°C for 20 minutes during the first heating to eliminate thermal history. Then, after cooling to the respective crystallization temperatures (100 to 130°C) as quickly as possible at 100°C / min, heat flow was observed while maintaining the temperature at each crystallization temperature, and the crystallization half-life was measured. Furthermore, the crystallinity X was calculated using the following equation (100% crystalline PLA ΔHm = 93 J / g).

[0069] - Crystallinity: (Area of ​​the exothermic peak during cooling, ΔHc) / (ΔHm of 100% crystalline PLA)

[0070] The results are shown in Table 1 below.

[0071] [Table 1]

[0072]

[0073] As shown in Table 1, it was confirmed that in the examples where the first nucleating agent and the second nucleating agent were used simultaneously according to this disclosure, the crystallinity was equal to or similar to that of the comparative example, but the crystallization half-life was significantly shorter.

Claims

1. A polylactide resin composition comprising polylactide resin; a first nucleating agent; and a second nucleating agent. in, The polylactide resin composition has a crystallization half-life of less than 2 minutes at a crystallization temperature of 100°C to 130°C. The first nucleating agent is uracil, and the content of the first nucleating agent is from 0.1% to 5% by weight based on the total weight of the polylactide resin composition. The second nucleating agent is a compound containing a lactide oligomer structure, and the content of the second nucleating agent is from 3% to 25% by weight based on the total weight of the polylactide resin composition.

2. The polylactide resin composition of claim 1, wherein: The polylactide resin composition has a crystallization half-life of less than 1.3 minutes at a crystallization temperature of 100°C to 130°C.

3. The polylactide resin composition according to claim 1, wherein: The polylactide resin composition has a crystallinity of more than 35% at a crystallization temperature of 100°C to 130°C.

4. The polylactide resin composition of claim 1, wherein: Based on the total weight of the polylactide resin composition, the content of the first nucleating agent is from 0.2% to 4.5% by weight.

5. The polylactide resin composition of claim 1, wherein: The second nucleating agent is a compound represented by the following chemical formula 1: [Chemical Formula 1] In chemical formula 1, L is: in, n1 is an integer from 1 to 30, and R is a substituent represented by the following chemical formula 2. [Chemical Formula 2] in, n represents the number of repeating units, and R' is hydrogen or acetyl.

6. The polylactide resin composition of claim 1, wherein: Based on the total weight of the polylactide resin composition, the content of the second nucleating agent is from 3.5% to 24% by weight.

7. The polylactide resin composition of claim 1, wherein: The weight-average molecular weight of the second nucleating agent is between 1,000 and 50,000.

8. The polylactide resin composition of claim 1, wherein: The weight-average molecular weight of the polylactide resin is between 70,000 and 400,000.

Citation Information

Patent Citations

  • Partition with heating function

    KR1020220035552A

  • Polylactic acid resin composition and molded body thereof

    CN101495572A

  • Biomass reinforced polylactic acid composite material and preparation method thereof

    CN109401249A

  • Biodegradable resin composition

    JP2008115372A