AI Technical Summary
TPU materials are prone to yellowing when exposed to high temperatures and long-term UV light. Existing antioxidants cannot effectively prevent yellowing, affecting the durability and appearance of shoe materials.
An antioxidant complex is used, including a combination of antioxidants, hindered amine light stabilizers and UV absorbers to improve anti-yellowing and anti-UV aging properties through synergy, and L-polylactic acid is added during the high-temperature injection molding process to Reduce the amount of antioxidant precipitation and prevent surface 'blooming' phenomenon.
Significantly reduces the yellowness of TPU shoe materials under long-term UV irradiation, improves the resistance to high temperature yellowing and UV aging, reduces the 'blooming' phenomenon on the surface of the shoe material, and expands the effectiveness of the antioxidant compound Scope of use.
Smart Images

Figure BDA0004563760920000041 
Figure BDA0004563760920000051 
Figure BDA0004563760920000052
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of antioxidants, and more specifically, to an antioxidant compound for TPU materials and a preparation method thereof. Background Art
[0002] TPU material (polyurethane elastomer) is an elastomer that can be plasticized by heating and dissolved by solvents. Its performance is between that of plastic and rubber. It is oil-resistant, wear-resistant, low-temperature-resistant, aging-resistant, high-hardness and elastic. It is widely used in the shoemaking, medical and other industries.
[0003] With the help of TPU's own characteristics, shoe materials made of TPU have better environmental protection, wear resistance, low-temperature winding, hydrolysis resistance, UV resistance and other properties than other materials, and are easy to process and shape, thus having a wider product processing range.
[0004] The raw materials for the preparation of TPU materials are mainly divided into aliphatic isocyanates and aromatic isocyanates. Aromatic isocyanates are widely used in the manufacture of TPU materials for footwear due to their advantages such as low cost and fast reaction speed. During the preparation process, TPU materials need to be injection molded at high temperatures (150-250°C). However, due to the structural characteristics of aromatic isocyanates themselves, the high-temperature aging resistance of the prepared polyurethane elastomer is poor, resulting in the material being prone to yellowing at high temperatures. Therefore, hindered phenolic high-temperature resistant antioxidants are generally added during injection molding to improve the anti-yellowing performance of the footwear material and improve the above-mentioned problem.
[0005] However, after the shoe materials are prepared and formed, they still need to be tested using the ultraviolet lamp method to determine whether they can pass the ASTM-D1148 test standard. However, the shoe materials are still prone to yellowing under long-term ultraviolet light exposure, indicating that the current antioxidants cannot assist the shoe materials to pass long-term ultraviolet light exposure well, and the performance needs to be improved. Summary of the invention
[0006] In order to further optimize the performance of the antioxidant so that the TPU shoe material is less likely to turn yellow after long-term ultraviolet irradiation, the present application provides an antioxidant compound for TPU material and a preparation method thereof.
[0007] In a first aspect, the present application provides an antioxidant compound for TPU material and a preparation method thereof, using the following technical solution:
[0008] An antioxidant compound for TPU material, comprising the following components by weight:
[0009] 45-55 parts of antioxidant;
[0010] 20-30 parts of hindered amine light stabilizer;
[0011] 20-30 parts of ultraviolet absorber.
[0012] By adopting the above technical solution: the performance test is carried out, and the yellowness YI of the shoe material using the antioxidant compound after being irradiated with ultraviolet light for 40 hours is 40 The yellowness YI of the shoe material using the same amount of antioxidant 1010 is only 4.73. 40 As high as 29.88, the yellowness YI of the shoe material using antioxidant 1010 and hindered amine light stabilizer 40 The yellowness YI of the shoe material using antioxidant 1010 and hindered amine light stabilizer is 24.36. 40 It is 25.52.
[0013] The reason is that the antioxidant gives the composite a certain anti-yellowing effect, the hindered amine light stabilizer mainly has a good inhibitory effect on photo-oxidative degradation reactions by quenching singlet oxygen chromophores and decomposing peroxides, and the ultraviolet absorber can absorb ultraviolet rays, and the molecular structure undergoes thermal vibration, which is converted into heat energy and released. The two complement each other and have a synergistic effect, jointly improving the anti-ultraviolet aging performance of the composite, and at the same time have antioxidant activity during thermal processing and heating processes, so that the combination of the three produces a composite with excellent antioxidant, anti-yellowing and anti-ultraviolet aging properties, which significantly reduces the yellowness of shoe materials under long-term ultraviolet light irradiation.
[0014] Optionally, the following components are included in parts by weight:
[0015] Antioxidant 50 parts;
[0016] 25 parts of hindered amine light stabilizer;
[0017] 25 parts of ultraviolet absorber.
[0018] By adopting the above technical solution: when the dosage of each component of the antioxidant complex is as above, the yellowing resistance test shows that the yellowness of the shoe material YI 40 It dropped from 4.73 to 4.22, and the shoe material has better anti-yellowing performance.
[0019] Optionally, the hindered amine light stabilizer is hindered amine light stabilizer 944.
[0020] Optionally, the antioxidant is one of a hindered phenol antioxidant and a phenol-free phosphite antioxidant.
[0021] By adopting the above technical solution: hindered phenol antioxidants have good antioxidant effect, high thermal stability, low toxicity, and they capture free radicals and simultaneously generate peroxides that are easy to generate free radicals, while hindered phenol light stabilizers can inactivate the peroxides, thereby preventing thermal decomposition or photolysis from generating free radicals, so that hindered phenol antioxidants and hindered amine light stabilizers play a synergistic role. Phenol-free phosphite antioxidants have a good ability to protect color and effectively inhibit the self-oxidation reaction of TPU shoe materials.
[0022] Optionally, the antioxidant is a phenol-free phosphite antioxidant.
[0023] By adopting the above technical solution: the phenol-free phosphite antioxidant itself does not produce chromogenic groups, so it will not turn yellow at high temperatures, thereby improving the problem that shoe materials are prone to yellowing at high temperatures.
[0024] Optionally, the phenol-free phosphite antioxidant is 618.
[0025] By adopting the above technical solution: 618 has a high phosphorus content, is resistant to high temperatures and color change, does not pollute materials, and the shoe material is not easy to yellow after high temperature and ultraviolet light treatment. In addition, 618 has good compatibility with TPU and is not easy to precipitate during the molding process, thereby effectively improving the anti-oxidation, high temperature yellowing and ultraviolet aging effects of the shoe material.
[0026] Optionally, the antioxidant is a hindered phenol antioxidant, and the antioxidant complex further comprises L-polylactic acid.
[0027] By adopting the above technical solution: in actual use, it is found that when using hindered phenol antioxidants (this application only takes 1010 as an example), they precipitate due to poor compatibility with TPU, which not only reduces the protective effect of the antioxidant complex on the material, but also forms a layer of powdery "frost" on the surface of the material, affecting the use of the shoe material.
[0028] Therefore, further improvements were made and it was found that the addition of left-lactic acid (PLLA) could reduce the precipitation problem of antioxidants (not just hindered phenolic antioxidants). Analysis showed that the reason may be that during the high-temperature injection molding process, PLLA crystallized, which increased the crystallinity of TPU, making the shoe material denser, reducing the precipitation problem of antioxidant complexes, and reducing the "frost" phenomenon on the surface of the shoe material.
[0029] A precipitation test was conducted. When the antioxidant complex contained hindered phenolic antioxidant, the precipitation amount of the antioxidant complex in the shoe material was as high as 86.4%. After adding L-polylactic acid, the precipitation amount of the antioxidant complex in the shoe material dropped to 41.2%, indicating that the addition of L-polylactic acid makes the antioxidant complex less likely to precipitate.
[0030] Therefore, after adding L-polylactic acid, the antioxidant compound is not limited to the use of phenol-free phosphite antioxidants. When hindered phenol antioxidants are used, the amount of precipitation is also low, which expands the application range of the antioxidant compound components.
[0031] Optionally, the weight ratio of the added amount of the L-polylactic acid to the hindered phenol antioxidant is (0.2-0.3):1.
[0032] By adopting the above technical solution: when the addition amount of L-polylactic acid is within the above range, the ratio with each component is appropriate, the compounding effect between the components in the prepared antioxidant composite is better, and after precipitation test, the precipitation amount of the antioxidant composite is further reduced to 28.8-35.6%, further improving the precipitation problem of the antioxidant composite.
[0033] In a second aspect, the present application provides a method for preparing an antioxidant compound for TPU material, using the following technical solution:
[0034] A method for preparing the above-mentioned antioxidant compound for TPU material comprises the following steps:
[0035] S1, crushing the antioxidant and L-polylactic acid to obtain a mixture;
[0036] S2. Add hindered amine light stabilizer and ultraviolet absorber into the mixture and mix them to obtain the product.
[0037] By adopting the above technical solution: fewer steps, simple and efficient process, and the antioxidant compound produced is in the form of white powder and granules, clear after dissolution, and the weight loss after heating is within the range of 0-1.0%, which meets the standard. In terms of performance, it can not only significantly improve the anti-yellowing performance of TPU shoe materials, so that TPU shoe materials are not easy to yellow under 40h of ultraviolet irradiation, and have significant anti-ultraviolet aging effect, but also the precipitation amount is low, which effectively protects the shoe materials for a long time and is not easy to "spray frosting".
[0038] In summary, this application has the following beneficial effects:
[0039] 1. In this application, hindered amine light stabilizers, ultraviolet absorbers and antioxidants are compounded to make the prepared antioxidant compound resistant to high temperature yellowing and ultraviolet aging, so that the antioxidant compound can assist the shoe material, reduce the high temperature yellowing of the shoe material during the injection molding process, and the yellowing phenomenon after long-term ultraviolet light exposure;
[0040] 2. In the present application, the phenol-free phosphite antioxidant is preferably used, because it does not produce color-developing groups to pollute the substrate, thereby further reducing the yellowing problem of the shoe material;
[0041] 3. In the present application, by using hindered phenol antioxidants and adding L-polylactic acid, during the injection molding process of the shoe material, the L-polylactic acid crystallizes, which increases the crystallinity of the TPU shoe material and hinders the precipitation of the hindered phenol antioxidant, thereby greatly reducing the precipitation amount of the antioxidant complex, and further reducing the frosting phenomenon on the surface of the shoe material. DETAILED DESCRIPTION
[0042] The present application is further described in detail below with reference to the embodiments.
[0043] Example 1
[0044] An antioxidant compound for TPU material, the components and their corresponding weights are shown in Table 1, and is prepared by the following steps:
[0045] S1. Add the antioxidant into the pulverizer, control the water bath temperature to 25°C, and pulverize at 25°C for 1 hour to obtain a mixture;
[0046] S2. Add hindered amine light stabilizer and ultraviolet absorber to the mixture, stir and mix at 25° C. for 2 hours, take samples for testing, control the content of UV-2908 to be within the range of 25±3% of the total amount of the antioxidant complex, and discharge the material to obtain the product.
[0047] [The antioxidant is hindered phenol antioxidant 1010, the light stabilizer is hindered amine light stabilizer HS-944, and the ultraviolet absorber is UV-2908. ]
[0048] Table 1 Components and their weights in Examples 1-3 and Comparative Examples 1-3 (kg)
[0049]
[0050] Example 4
[0051] An antioxidant compound for TPU material, which is different from Example 2 in that the use of the antioxidant is different, and an equal amount of a phenol-free phosphite antioxidant (AP-618) is used instead of the hindered phenol antioxidant 1010.
[0052] Embodiment 5-8
[0053] An antioxidant compound for TPU material, the components and their corresponding weights are shown in Table 2, and is prepared by the following steps:
[0054] S1, adding antioxidant and L-polylactic acid into a pulverizer, controlling the water bath temperature to 25°C, and pulverizing at 25°C for 1 hour to obtain a mixture;
[0055] S2. Add hindered amine light stabilizer and ultraviolet absorber to the mixture, stir and mix at 25° C. for 2 hours, take samples for testing, control the content of UV-2908 to be within the range of 25±3% of the total amount of the antioxidant complex, and discharge the material to obtain the product.
[0056] [L-polylactic acid was obtained from Shenzhen Boli Biomaterials Co., Ltd., model number is PLLA-05. ]
[0057] Table 2 Components and their weights in Examples 2, 5-8 (kg)
[0058]
[0059] Performance Testing
[0060] Preparation of samples: First, TPU particles were prepared according to the following method: (1) 2 kg of 2-hexyl-3-octyl-4,5-dihydroxyoctylcyclohexane, 3 kg of polybutylene adipate polyol and 0.5 kg of ethylene glycol were mixed and stirred at 100° C. to obtain a premix; (2) 2 kg of 4,4'-diphenylmethane diisocyanate and 0.05 kg of dibutyltin dilaurate were added to storage tank A, and the premix was added to storage tank B. Under stirring conditions, vacuum dehydration was carried out at 100° C., and the mixture was pumped into a twin-screw extruder; (3) The mixture was reacted in a twin-screw extruder at 150° C. and granulated to obtain TPU particles;
[0061] During the injection molding process for shoe materials, when adding TPU particles, the antioxidant compound prepared in the examples and comparative examples was added (the antioxidant compound addition amount was 0.5% of the weight of the TPU particles) to form shoe material samples.
[0062] The prepared shoe material samples were subjected to the following performance tests, and the test results are recorded in Table 3.
[0063] Detection Methods
[0064] 1. Yellowing resistance: Tested according to the UV lamp method in HG / T 3689-2014. After turning on the switch, irradiate the shoe material sample and the control sample under UV light for 40 hours. Take out the sample and use a desktop spectrophotometer (test standard: ASTM E313; light source: D65; angle: 10°) to test the yellowness YI value of the shoe material sample and the control sample, recorded as YI 40 , YI 40 The smaller the value, the better the yellowing resistance of the sample.
[0065] 2. Precipitation test: Take 1g of each shoe material sample, put it into 100mL ethanol for extraction for 9h, analyze the extract, and detect the extraction amount of the antioxidant complex by HPLC. The extract of the shoe material sample in Comparative Example 1 is used as the control group, and the extraction amount of the antioxidant complex in the control group is detected, which is recorded as a. The amount of the antioxidant complex in the extract of Examples 1-8 and Comparative Examples 2-3 is recorded as b. According to (b / a)*100%, the proportion is calculated. The smaller the proportion, the less likely the antioxidant complex in the embodiment or comparative example is to precipitate.
[0066] Table 3 Performance test results
[0067]
[0068]
[0069] As shown in Table 1, in Example 1, due to the use of the antioxidant compound prepared in Preparation Example 1, the yellowness (YI 40 ) is only 4.73, while in Comparative Example 1, an equal amount of hindered phenolic antioxidant 1010 is used instead of the antioxidant compound, and the YI of the shoe material produced is 40 As high as 29.88, the difference between Comparative Example 2 and Example 1 is that no ultraviolet absorber is added to the composite antioxidant, and the YI of the shoe material produced is 40 As high as 24.36, the difference between Comparative Example 3 and Example 1 is that no hindered amine light stabilizer is added to the composite antioxidant, and the YI of the shoe material produced is 40 Up to 25.52;
[0070] It shows that the antioxidant compound prepared in the present application can significantly improve the anti-yellowing performance of TPU, while the use of only antioxidants or compounding with one of the ultraviolet absorbers and hindered amine light stabilizers cannot effectively improve the anti-yellowing performance of TPU.
[0071] The reason is that hindered amine light stabilizers and UV absorbers have a certain synergistic effect. The combination of the two with hindered phenol antioxidants significantly improves the anti-yellowing effect of TPU, such as high temperature yellowing resistance and UV yellowing resistance.
[0072] The difference between Example 2-3 and Example 1 is that the amounts of the components in the antioxidant compound are different. 40 The value is the lowest, only 4.22, and the anti-yellowing performance of the shoe material is the best.
[0073] The difference between Example 4 and Example 2 is that the use of antioxidants is different. The same amount of phenol-free phosphite antioxidant 618 is used instead of hindered phenol antioxidant 1010. Since 618 does not produce chromophores, the YI of the manufactured shoe material is40 The value dropped significantly to 2.27, and the anti-yellowing performance was better.
[0074] The difference between Example 5-8 and Example 2 is that different amounts of L-polylactic acid are added in step S1 of preparing the antioxidant compound (note, the antioxidant at this time is still 1010, which is consistent with Example 2). The precipitation amount of the antioxidant compound in Example 2 accounts for 86.4%, while the precipitation amount of the antioxidant compound in the shoe material of Examples 5-8 accounts for only 41.2% at most, indicating that the addition of L-polylactic acid significantly reduces the precipitation amount of the antioxidant compound and reduces the "blooming" phenomenon of the shoe material;
[0075] The possible reason is that during the high-temperature injection molding process, L-polylactic acid crystallizes, which increases the crystallinity of TPU and makes the shoe material denser, thereby hindering the precipitation of antioxidant complex components.
[0076] And it can be seen from Table 3 that the precipitation amount of Examples 6-8 accounts for an even lower proportion of 28.8-35.6%, indicating that the amount of L-polylactic acid added should be within the range of Examples 6-8.
[0077] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An antioxidant compound for TPU material, characterized in that: The composition comprises the following components in parts by weight: 45-55 parts of antioxidant; 20-30 parts of hindered amine light stabilizer; 20-30 parts of ultraviolet absorber; Poly(L-lactic acid); The weight ratio of the added amount of L-polylactic acid to the antioxidant is (0.2-0.3):1; The antioxidant is one of a hindered phenol antioxidant and a phenol-free phosphite antioxidant.
2. The antioxidant compound for TPU material according to claim 1, characterized in that: The composition comprises the following components in parts by weight: Antioxidant 50 parts; 25 parts of hindered amine light stabilizer; 25 parts of ultraviolet absorber.
3. The antioxidant compound for TPU material according to claim 1, characterized in that: The hindered amine light stabilizer is hindered amine light stabilizer 944.
4. The antioxidant compound for TPU material according to claim 1, characterized in that: The antioxidant is a phenol-free phosphite antioxidant.
5. The antioxidant compound for TPU material according to claim 4, characterized in that: The phenol-free phosphite antioxidant is antioxidant 618.
6. A method for preparing an antioxidant compound for TPU material according to claim 1, characterized in that: The following steps are involved: S1, crushing the antioxidant and L-polylactic acid to obtain a mixture; S2. Add hindered amine light stabilizer and ultraviolet absorber into the mixture and mix them to obtain the product.