A PPA / PI / LCP alloy, preparation method and application thereof

By mixing polyphthalamide, glass fiber, PI resin and thermogenic liquid crystal polymer in an extruder, the problem of difficulty in blending PPA and PI is solved, and PPA/PI/LCP alloy with excellent performance is prepared , achieving low water absorption, high heat resistance and high electrical performance, and is suitable for high-precision processing of new energy vehicles and electronic appliances.

CN117511198BActive Publication Date: 2024-11-05PULIMEI (JINGYANG) MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410017534.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-05
Publication Date
2024-11-05
Estimated Expiration
2044-01-05

AI Technical Summary

Technical Problem

PPA and polyimide resins (PI) are difficult to blend and compatible, resulting in high water absorption, poor dimensional stability and electrical performance, poor heat resistance and low temperature impact strength, which cannot meet the high-precision processing needs of some industries. .

Method used

Using PPA/PI/LCP alloy, the alloy is prepared by mixing polyphthalamide, glass fiber, PI resin, thermogenic liquid crystal polymer and antioxidant in the extruder to control the temperature and pressure, and the alloy is prepared by using The orientation and heterogeneous nucleation of thermogenic liquid crystal polymers improve fluidity and flame retardancy, and improve heat resistance and processability.

Benefits of technology

Prepare alloy materials with low water absorption, high load thermal deformation temperature, high impact strength and high tensile modulus, which have excellent mechanical properties, heat resistance and electrical properties, and can be completed through traditional extrusion molding processes. In the fields of new energy vehicles, electronics and electrical appliances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117511198B_ABST
    Figure CN117511198B_ABST
Patent Text Reader

Abstract

The present application discloses a PPA / PI / LCP alloy, a preparation method and its application. The preparation method comprises: (1) preparing PI resin; (2) mixing polyphthalamide, glass fiber, PI resin, thermotropic liquid crystal polymer, antioxidant and internal release agent uniformly to obtain a mixture; (3) putting the mixture into an extruder for mixing and extrusion; (4) cooling, drying and pelletizing the extruded material to obtain a PPA / PI / LCP alloy material. The present application comprises the following components in parts by weight: 40-50 parts of polyphthalamide; 40-50 parts of glass fiber; 1-5 parts of thermotropic liquid crystal polymer; 5-10 parts of PI resin; 0.1-0.5 parts of antioxidant; The present application provides a PPA / PI / LCP alloy with excellent mechanical properties, heat resistance and electrical properties, and improves the processability of the material on the basis of ensuring the material properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a PPA / PI / LCP alloy, a preparation method and application thereof, and belongs to the technical field of modified plastics. Background Art

[0002] PPA is the most widely used type of engineering plastics, which has the following characteristics: excellent mechanical strength, good toughness, stress cracking resistance, good wear resistance and corrosion resistance, and good molding processability, etc. As an engineering plastic, its disadvantages are high water absorption, poor dimensional stability and electrical properties, poor heat resistance and low-temperature impact strength. Therefore, it cannot meet the needs of some industries that require environmental resistance, stress resistance and high processing precision.

[0003] Polyimide resin (PI) is a type of high molecular weight polymer containing imide groups in the main chain. Their unique temperature resistance and mechanical properties provide prospects for the application of polyimide resin in the field of high-end plastic technology.

[0004] However, how to achieve processing feasibility while maintaining the excellent properties of PPA and polyimide resin (PI) is one of the main directions for developing new materials by alloying PPA and polyimide resin (PI) in the current polymer field. Summary of the invention

[0005] In view of this, the present application provides a PPA / PI / LCP alloy, which solves the problem that PPA and PI are difficult to blend and compatibility, and provides an alloy material with low water absorption, high load heat deformation temperature, high impact strength, and high tensile modulus. The specific solution is:

[0006] A method for preparing a PPA / PI / LCP alloy, characterized in that the preparation method comprises the following steps:

[0007] (1) Preparation of PI resin;

[0008] (2) polyphthalamide, glass fiber, PI resin, thermotropic liquid crystal polymer, antioxidant and internal release agent are uniformly mixed to obtain a mixture;

[0009] (3) Putting the mixed material into an extruder for mixing and extrusion;

[0010] (4) Cooling, drying and pelletizing the extruded material to obtain PPA / PI / LCP alloy material;

[0011] The weight proportions of the polyphthalamide, glass fiber, PI resin, thermotropic liquid crystal polymer, antioxidant and internal release agent are as follows:

[0012] 40-50 parts of polyphthalamide;

[0013] 40~50 parts of glass fiber;

[0014] 1-5 parts of thermotropic liquid crystal polymer;

[0015] PI resin 5-10 parts;

[0016] 0.1~0.5 parts of antioxidant;

[0017] The temperature of the first zone of the extruder is 220°C to 250°C, the temperature of the second zone is 260°C to 290°C, the temperature of the third zone is 300°C to 310°C, the temperature of the fourth zone is 320°C to 350°C, and the temperature of the fifth zone is 290°C to 300°C;

[0018] The extruder residence time is 2-5 min, the main engine speed is 200-500 rpm, and the pressure is 10-18 MPa.

[0019] Preferably, the temperature of the extruder is set as follows: the temperature of zone 1 of the extruder is 250°C, the temperature of zone 2 is 290°C, the temperature of zone 3 is 310°C, the temperature of zone 4 is 350°C, and the temperature of zone 5 is 300°C.

[0020] Preferably, the extruder residence time is 5 min, the main engine speed is 500 rpm, and the pressure is 18 MPa.

[0021] Preferably, the intrinsic viscosity of the PI resin is 0.68 dL / g.

[0022] According to another aspect of the present application, a PPA / PI / LCP is provided, comprising the following components in parts by weight:

[0023] Polyphthalamide 40~50;

[0024] 40~50 parts of glass fiber;

[0025] 1-5 parts of thermotropic liquid crystal polymer;

[0026] PI resin 5-10 parts;

[0027] Antioxidant 0.1~0.5 parts.

[0028] Preferably, the antioxidant is one or more of N, N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, and 3,5-di-tert-butyl-4-hydroxyphenylpropionate.

[0029] According to another aspect of the present application, there is provided an application of the PPA / PI / LCP alloy in new energy vehicles, electronic appliances, and household appliances.

[0030] The beneficial effects of this application include:

[0031] The PPA / PI / LCP alloy described in the present application uses PPA (i.e., polyphthalamide) and PI resin as matrix materials, wherein PPA is the main matrix material and glass fiber is the reinforcing material. The heat resistance of PPA is improved by introducing PI resin, and the alloy has excellent electrical properties through PPA, and is not prone to static electricity accumulation during use; the alloy has excellent mechanical properties through glass fiber;

[0032] By introducing LCP (liquid crystal polymer), utilizing the good orientation and heterogeneous nucleation of LCP, the fluidity of the resin is greatly improved, and the processing performance of the alloy is improved. LCP is selected as a thermotropic liquid crystal polymer, and the flame retardancy of the alloy is improved by utilizing the excellent heat resistance and self-flammability of the thermotropic liquid crystal polymer. Since the melt viscosity of the thermotropic liquid crystal polymer is low and the fluidity is good, only a small amount of thermotropic liquid crystal polymer needs to be added to ensure the excellent performance of PPA and PI themselves, and the blending and fusion of PPA and PI can be achieved without the need to add any additional compatibilizer. At the same time, the application adopts a thermotropic liquid crystal polymer to avoid the defects of the low melting point of ordinary LCP and the mismatch between the melting points of PPA and PI, easy phase separation and poor heat resistance during processing, and easy decomposition and inability to fuse during processing, thereby improving the processability of the material while ensuring the performance of the material.

[0033] By adding antioxidants, the mechanical properties of the alloy are increased while the CTI and thermal insulation strength of the alloy are significantly improved, thereby preparing a PPA / PI / LCP alloy with excellent mechanical properties, heat resistance and electrical properties;

[0034] At the same time, the PPA / PI / LCP alloy described in the present application does not require optimization, improvement or special processes for molding process to be molded. The preparation of the alloy material can be completed only through the traditional extrusion molding process, and the molding is simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A structural diagram of a polyimide resin in an embodiment of the present invention;

[0036] Figure 2 is an infrared spectrum of the polyimide resin in the embodiment of the present invention;

[0037] Figure 3 This is a thermal gravimetric test diagram of the PPA / PI / LCP alloy prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0038] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0039] The preparation process of PI resin (polyimide resin) is:

[0040] Step 1: prepare a polyamic acid solution, and the specific preparation process is as follows:

[0041] At room temperature, 200 g of 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, 10 g of phthalic anhydride and 230 g of 4,4'-diaminodiphenyl ether were added to a 5 L reactor containing 2 L of N-methylpyrrolidone, and the mixture was stirred and reacted for 12 hours under nitrogen to obtain a polyamic acid solution.

[0042] Step 2: prepare polyimide resin, the specific preparation process is:

[0043] Add 1.5L of xylene to the polyamic acid solution prepared in step 1, heat to 160°C under nitrogen protection, stir and reflux, and precipitate yellow powder after 4 hours. After 8 hours of reflux reaction, distill and recover xylene. After distilling out xylene, cool and centrifuge to collect filter cake, wash the filter cake with ethanol 3 times and water 5 times. Dry the powder after centrifugation in an 85°C forced air drying oven for 36 hours, then heat treat at 350°C under vacuum for 4 hours, and crush and subdivide to obtain a yellow polyimide resin. The structure of the polyimide resin is shown in the attached figure. Figure 1 The infrared spectrum of polyimide resin is shown in the attached figure. Figure 2 As shown, from Figure 2 It can be seen that 1780cm -1 The absorption peak at 1720 cm is the asymmetric stretching vibration absorption peak of the carbonyl group in aromatic imide. -1 The carbonyl symmetric stretching vibration absorption peak is 1380cm -1 The carbon-nitrogen bond stretching vibration absorption peak is 725 cm -1 It is the carbonyl bending vibration absorption peak, from which we know that the resin prepared in step 2 is polyimide resin.

[0044] The characteristic viscosity of the prepared polyimide resin is 0.68 dL / g (tested at 30°C with concentrated sulfuric acid as solvent).

[0045] Step three, preparing PPA / PI / LCP alloy. The preparation of PPA / PI / LCP alloy is completed by the following embodiment.

[0046] Embodiment 1:

[0047] 40 parts of PPA (i.e., polyphthalamide), 50 parts of glass fiber, 5 parts of PI resin, 4.4 parts of thermotropic liquid crystal polymer, 0.1 part of antioxidant and 0.5 part of internal release agent were mixed evenly and added into a twin-screw extruder. The temperature of the first zone from the feed port to the die head was 250°C, the temperature of the second zone was 290°C, the temperature of the third zone was 310°C, the temperature of the fourth zone was 350°C, the temperature of the fifth zone was 300°C, the residence time was 5 min, the main engine speed was 500 rpm, the pressure was 18 MPa, and finally, after extrusion cooling, drying and pelletizing, a PPA / PI / LCP alloy material was obtained.

[0048] Embodiment 2:

[0049] 50 parts of PPA (i.e., polyphthalamide), 40 parts of glass fiber, 7.5 parts of PI resin, 1 part of thermotropic liquid crystal polymer, 0.5 parts of antioxidant and 1 part of internal release agent were mixed evenly and added into a twin-screw extruder. The temperature of the first zone from the feed port to the die head was 220°C, the temperature of the second zone was 260°C, the temperature of the third zone was 300°C, the temperature of the fourth zone was 320°C, the temperature of the fifth zone was 290°C, the residence time was 2 min, the main engine speed was 200 rpm, the pressure was 10 MPa, and finally, after extrusion cooling, drying and pelletizing, the PPA / PI / LCP alloy material was obtained.

[0050] Embodiment 3:

[0051] 42 parts of (i.e., polyphthalamide), 42 parts of glass fiber, 10 parts of PI resin, 5 parts of thermotropic liquid crystal polymer, 0.3 parts of antioxidant and 0.7 parts of internal release agent were mixed evenly and added into a twin-screw extruder. The temperature of the first zone from the feed port to the die head was 230°C, the temperature of the second zone was 270°C, the temperature of the third zone was 305°C, the temperature of the fourth zone was 340°C, the temperature of the fifth zone was 295°C, the residence time was 3 min, the main engine speed was 300 rpm, the pressure was 15 MPa, and finally, after extrusion cooling, drying and pelletizing, a PPA / PI / LCP alloy material was obtained.

[0052] In order to verify the properties of the PPA / PI / LCP alloy material prepared in this application, this application conducted a thermal gravimetric test on the PPA / PI / LCP alloy prepared in Example 2. The thermal gravimetric test graph obtained is shown in the attached figure. Figure 3 As shown in the attached Figure 3 It can be seen that the alloy material has three main decomposition peaks, namely: 600℃, 700℃ and 800℃, which correspond to the main decomposition temperatures of PPA, LCP and PI materials respectively, which proves that the prepared product is PPA / PI / LCP alloy material.

[0053] In order to verify the performance of the PPA / PI / LCP alloy material prepared in the present application, the physical properties, mechanical properties, thermal properties and electrical properties of the PPA, PI material and the PPA / PI / LCP alloy material prepared in Example 2 of the present application were tested respectively. The specific test data are shown below.

[0054] The specific test results of the physical properties, mechanical properties, thermal properties and electrical properties of the PPA / PI / LCP alloy material prepared in Example 2 of the present application are shown in Tables 1 to 4, respectively.

[0055]

[0056]

[0057]

[0058]

[0059] The flame retardancy of the PPA / PI / LCP alloy material prepared in the present application is tested using the UL94 test standard, and the flame retardancy can reach the fire protection level, data V-0.

[0060] Comparative Example 1

[0061] The test data of PI physical properties, mechanical properties, thermal properties and electrical properties under the same test standard as the PPA / PI / LCP alloy material prepared in Example 2 of the present application are shown in Tables 5-8.

[0062]

[0063]

[0064]

[0065]

[0066] The test data of physical properties, mechanical properties, thermal properties and electrical properties of PPA under the same test standard as the PPA / PI / LCP alloy material prepared in Example 2 of the present application are shown in Tables 9-12.

[0067]

[0068]

[0069]

[0070]

[0071] From the above test data, it can be seen that the density of the PPA / PI / LCP alloy material prepared in Example 2 of the present application is 1.55 g / cm 3 , greater than the density of PI 1.35g / cm 3 The density of PPA is 1.3g / cm 3 ;

[0072] The 24-hour water absorption rate of the PPA / PI / LCP alloy material is 0.29%, which is lower than the 24-hour water absorption rate of PI (0.3%) and the 24-hour water absorption rate of PPA (0.5%), and has low water absorption.

[0073] The Rockwell hardness of the PPA / PI / LCP alloy material is 95, which is greater than the Rockwell hardness of PI (68) and the Rockwell hardness of PPA (56).

[0074] The tensile strength of the PPA / PI / LCP alloy material is 155MPa, which is greater than 70MPa of PI and 87MPa of PPA, and has high tensile strength;

[0075] The linear expansion coefficient flow value of PPA / PI / LCP alloy material is 1.50E-05cm / cm / ℃, PI is 1.60E-05cm / cm / ℃, and PPA is 1.70E-05cm / cm / ℃;

[0076] The CTI value of the PPA / PI / LCP alloy material is 600V, which is the same as the CTI value of PI of 600V and greater than the CTI value of PPA of 500V.

[0077] The flame retardant grade of PPA / PI / LCP alloy materials can reach the fireproof grade.

[0078] It can be seen from this that the PPA / PI / LCP alloy material prepared in this application has low water absorption, high load heat deformation temperature, high impact strength, high tensile modulus, and certain flame retardant and antistatic properties. Due to its excellent electrical insulation properties, the PPA / PI / LCP alloy is not easy to accumulate static electricity during use, and will not cause dust absorption, electric shock, or even spark discharge and combustion. Therefore, the PPA / PI / LCP alloy can replace ceramics and be used in new energy vehicles, electronic appliances, household appliances and other fields.

[0079] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for preparing a PPA / PI / LCP alloy, It is characterized in that The preparation method comprises the following steps: (1) preparing PI resin; (2) polyphthalamide, glass fiber, PI resin, thermotropic liquid crystal polymer, antioxidant and internal release agent are uniformly mixed to obtain a mixture; (3) putting the mixed material into an extruder for mixing and extruding; (4) cooling, drying, and pelletizing the extruded material to obtain a PPA / PI / LCP alloy material; The weight proportions of the polyphthalamide, glass fiber, PI resin, thermotropic liquid crystal polymer, antioxidant and internal release agent are as follows: 40-50 parts of polyphthalamide; 40-50 parts of glass fiber; 1-5 parts of thermotropic liquid crystal polymer; PI resin 5-10 parts; 0.1-0.5 parts of antioxidant; The temperature of the first zone of the extruder is 220°C to 250°C, the temperature of the second zone is 260°C to 290°C, the temperature of the third zone is 300°C to 310°C, the temperature of the fourth zone is 320°C to 350°C, and the temperature of the fifth zone is 290°C to 300°C; The extruder residence time is 2 to 5 minutes, the main engine speed is 200 to 500 rpm, and the pressure is 10 to 18 MPa; By introducing thermotropic liquid crystal polymers and utilizing the good orientation and heterogeneous nucleation of LCP, the blending of PPA and PI can be achieved while ensuring the excellent properties of PPA and PI themselves, without the need to add any additional compatibilizers, thereby preparing a PPA / PI / LCP alloy with low water absorption, high load heat deformation temperature, high impact strength and high tensile modulus.

2. A method for preparing a PPA / PI / LCP alloy according to claim 1, It is characterized in that The temperature of the extruder is set as follows: the temperature of zone 1 is 250°C, the temperature of zone 2 is 290°C, the temperature of zone 3 is 310°C, the temperature of zone 4 is 350°C, and the temperature of zone 5 is 300°C.

3. A method for preparing a PPA / PI / LCP alloy according to claim 1, It is characterized in that The extruder residence time is 5 min, the main engine speed is 500 rpm, and the pressure is 18 MPa.

4. A method for preparing a PPA / PI / LCP alloy according to claim 1, It is characterized in that The intrinsic viscosity of the PI resin is 0.68 dL / g.

5. A PPA / PI / LCP alloy, It is characterized in that The PPA / PI / LCP alloy prepared by the method for preparing a PPA / PI / LCP alloy according to any one of claims 1 to 4 comprises the following components in parts by weight: Polyphthalamide 40-50; 40-50 parts of glass fiber; 1-5 parts of thermotropic liquid crystal polymer; PI resin 5-10 parts; 0.1-0.5 parts of antioxidant.

6. A PPA / PI / LCP alloy according to claim 5, It is characterized in that The antioxidant is one or more of N,N-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, and 3,5-di-tert-butyl-4-hydroxyphenylpropionate.

7. Use of the PPA / PI / LCP alloy according to claim 5, It is characterized in that The PPA / PI / LCP alloy is used in the fields of new energy vehicles, electronic appliances, and household appliances.