A full-chain integrated method for recovering nickel and cobalt from waste ternary battery powder
Through the full-chain integrated pressure leaching and buffer solution precipitation technology of used ternary battery powder, the problems of high cost and high impurities in the recycling of used ternary lithium batteries are solved, and the purity and low water content of nickel, cobalt, manganese and lithium are efficiently extracted. product.
Patent Information
- Application Number
- CN202380011031.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-09-25
AI Technical Summary
The existing wet recycling process of used ternary lithium batteries has problems such as high cost, high energy consumption, high pollution, and high product impurities, especially the high price and easy decomposition of H2O2 in the inorganic acid leaching system, complex storage conditions, and The problem of large usage of sulfuric acid and high production cost.
Adopting a full-chain integration method, through the mixing of roasted battery powder and unbaked battery powder, pressure leaching, combined with the use of oxidants and buffer solutions, the pH value is adjusted to precipitate nickel, cobalt, manganese, lithium metal, avoid the use of H2O2, and control magnesium hydroxide The solid content and Mg2+ concentration ensure the purity and low water content of nickel cobalt hydroxide.
It achieves efficient extraction of nickel, cobalt, manganese and lithium metal without reducing agents, reduces production costs, improves product purity and particle size, avoids hydrogen generation and local over-alkali, and enhances leaching efficiency and product quality.
Smart Images

Figure CN117529569B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of recycling waste ternary power batteries, and in particular to a full-chain integrated method for recycling nickel and cobalt in waste ternary battery powder. Background Art
[0002] In recent years, with the rapid development of new energy electric vehicles, power lithium batteries generally reach scrap conditions after 5-8 years of use, which also means that the reserves of waste power batteries will continue to rise. The heavy metals in waste batteries have a great impact on environmental pollution, and the content of rare precious metals such as nickel, cobalt, manganese and lithium is extremely high, far exceeding the metal content in ordinary ores, and is one of the typical "urban ores". Therefore, comprehensive recycling of waste power batteries not only has high economic value, but also is conducive to ecological environmental protection.
[0003] At present, the wet recovery process of waste ternary lithium batteries mainly adopts inorganic acid leaching, organic acid leaching, and biological leaching. Among them, the biological leaching method has low cost, low energy consumption, no pollution, and a relatively simple process flow, but the leaching cycle is long, the leaching conditions are difficult to control, and it is still in the laboratory research stage. Organic acid leaching is mainly based on oxalic acid, citric acid, and malic acid, and is mainly used in university research, with low prospects for industrial application. For inorganic acid leaching processes, hydrochloric acid, phosphoric acid, sulfuric acid, etc. are mainly used as the main leaching agents, among which the H2SO4+H2O2 leaching system is the most common, but H2O2 is expensive, easy to decompose, has low utilization rate, and requires high storage conditions. It is a flammable and explosive product, and there are certain constraints in industrial production. At the same time, the amount of sulfuric acid used is large.
[0004] In the existing wet recycling process of waste batteries, the separation process of metal ions in the leachate often uses alkaline substances such as quicklime, sodium carbonate, and sodium hydroxide to adjust the pH of the solution to achieve metal ion precipitation. However, this method usually has the phenomenon of "local over-alkalinity", resulting in high impurity content, high water content, and low metal content in the product. At the same time, it consumes a lot of alkali, and the production cost is high.
[0005] In view of this, the present disclosure is proposed. Summary of the invention
[0006] The purpose of the present disclosure is to provide a full-chain integrated method for recovering nickel and cobalt from waste ternary battery powder, which can realize the efficient extraction of nickel, cobalt, manganese and lithium metal elements without reducing agents, and the nickel and cobalt hydroxide products have low water content and high purity.
[0007] The present disclosure is implemented as follows:
[0008] In a first aspect, the present disclosure provides a method for recovering nickel and cobalt from waste ternary battery powder in a full-chain integrated manner, comprising:
[0009] Mixing and slurrying: Mixing the roasted battery powder and the unroasted battery powder to obtain slurry;
[0010] Pressure leaching: mixing the slurry with acid and leaching under pressure, separating the solid and liquid after leaching to obtain pressure leaching liquid and pressure leaching residue;
[0011] Precipitation and impurity removal: after mixing the pressurized leaching solution with an oxidant, adjusting the solution pH to 4.5-6.0 to remove impurities such as iron, aluminum and silicon, and separating the solid and liquid after impurity removal to obtain impurity-removed slag and impurity-removed liquid;
[0012] One-stage hydrolysis precipitation: the impurity-removed liquid is mixed and stirred with a buffer solution composed of Mg(OH)2 and MgSO4 to precipitate nickel ions and cobalt ions, wherein the solid content of magnesium hydroxide in the buffer solution is 1%-40%, and the solid content of Mg(OH)2 and MgSO4 is 1%-40%. 2+ The concentration is 5-45g / L, and the solid-liquid separation obtains the product nickel cobalt hydroxide and a post-precipitation liquid.
[0013] In an optional embodiment, the mass ratio of the calcined battery powder to the uncalcined battery powder is 1:5-20.
[0014] In an optional embodiment, during the pulping process, the solid-liquid ratio is 3-5:1.
[0015] In an optional embodiment, the solvent used in the pulping is water.
[0016] In an optional embodiment, the calcined battery powder is obtained by placing battery black powder of waste ternary batteries in a tubular furnace and calcining it at 500-1500° C. for 1-3 hours.
[0017] In an optional embodiment, the mixing and slurrying further comprises ball milling and activating the slurry.
[0018] In an optional embodiment, the ball milling activation time is 30-90 minutes.
[0019] In an optional embodiment, in the pressure leaching step, the reaction pressure is 0.3-3.0 MPa.
[0020] In an optional embodiment, in the pressure leaching step, the reaction temperature is 150-250°C.
[0021] In an optional embodiment, in the step of pressurized leaching, the leaching time is 0.5-3.0 h.
[0022] In an optional embodiment, in the pressure leaching step, the acid added is sulfuric acid, the amount of sulfuric acid added is 80%-200% of the theoretical consumption of sulfuric acid for leaching all metals in the slurry, and the liquid-to-solid ratio of the sulfuric acid to the slurry is 2-4:1.
[0023] In an optional embodiment, the oxidant includes at least one of hydrogen peroxide, manganese dioxide and chlorine.
[0024] In an optional embodiment, the amount of the oxidant added is 1-2% of the volume of the pressurized leachate.
[0025] In an optional embodiment, in the precipitation and impurity removal step, a first alkaline substance is used to adjust the pH value of the solution, and the first alkaline substance includes at least one of limestone, sodium carbonate and calcium oxide.
[0026] In an optional embodiment, the mixing and stirring time in the hydrolysis and precipitation step is 1-3 hours.
[0027] In an optional embodiment, after the first-stage hydrolysis precipitation, a second-stage hydrolysis precipitation is further included: the first-stage precipitation liquid is mixed with a second alkaline substance to adjust the pH value of the system to 7.0-9.0 to perform a second-stage hydrolysis precipitation to completely precipitate nickel ions, cobalt ions and manganese ions, and solid-liquid separation is performed to obtain an intermediate product of nickel cobalt hydroxide and the second-stage precipitation liquid.
[0028] In an optional embodiment, the second alkaline substance includes at least one of lime milk, sodium carbonate and sodium hydroxide.
[0029] In an optional embodiment, the intermediate product nickel cobalt hydroxide is returned to the precipitation and impurity removal.
[0030] In an optional embodiment, after the second-stage hydrolysis precipitation, lithium extraction is also included: the liquid after the second-stage precipitation is mixed with a third alkaline substance to adjust the pH value of the system to 10-11 for precipitation and lithium extraction, and solid-liquid separation is performed to obtain lithium carbonate and magnesium sulfate waste liquid.
[0031] In an optional embodiment, the third alkaline substance includes at least one of sodium carbonate, potassium carbonate, ammonium carbonate and carbon dioxide.
[0032] In an optional embodiment, the magnesium sulfate waste liquid is returned to the first-stage hydrolysis precipitation to prepare a buffer solution.
[0033] In an optional embodiment, the solid-liquid separation in the pressure leaching, the precipitation and impurity removal, the first-stage hydrolysis precipitation, the second-stage hydrolysis precipitation and the lithium extraction steps are independently selected from filtration, membrane filtration, filter pressing, centrifugation or sedimentation.
[0034] The present disclosure has the following beneficial effects:
[0035] The present invention provides a full-chain integrated method for recovering nickel and cobalt from waste ternary battery powder, which utilizes calcined battery powder and uncalcined battery powder for mixed pressurized synergistic leaching, wherein the calcined battery powder has a certain reducibility, which can omit the use of H2O2 in the acid leaching process, and thus can efficiently extract nickel, cobalt, manganese and lithium valuable metal elements from the waste ternary battery powder without consuming a reducing agent, thereby improving the leaching rate and avoiding the generation of hydrogen; then, a buffer solution composed of Mg(OH)2 and MgSO4 is used to precipitate the valuable metals, and the present invention controls the solid content of magnesium hydroxide and Mg in the buffer solution. 2+ The concentration can be adjusted to achieve the pH of the system to mainly precipitate nickel ions and cobalt ions, while manganese ions are not precipitated or precipitated in small amounts, thereby ensuring the purity of the nickel cobalt hydroxide product. At the same time, since the present invention adopts a buffer solution to regulate the pH of the solution, the system can be maintained in a stable pH range without the phenomenon of local over-alkalinity. At the same time, the growth rate of the nickel cobalt hydroxide particles is slowed down, and the adverse effects of impurities being "entrained, coated, and adsorbed" are reduced, thereby greatly improving the purity of the product and obtaining a product with low water content and large particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0037] Figure 1 A process flow chart of the fully integrated method for recovering nickel and cobalt from waste ternary battery powder provided in the present invention. DETAILED DESCRIPTION
[0038] The embodiments of the present disclosure will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present disclosure and should not be considered to limit the scope of the present disclosure. Where specific conditions are not specified in the examples, they are carried out under conventional conditions or conditions recommended by the manufacturer. Where the manufacturers of the reagents or instruments used are not specified, they are all conventional products that can be purchased commercially.
[0039] The endpoints and any values of the ranges disclosed in this disclosure are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0040] See also Figure 1 The present invention provides a method for recovering nickel and cobalt from waste ternary battery powder with a full-chain integration, which comprises the following steps:
[0041] (1) Mixing and pulping.
[0042] The battery black powder mixed with positive and negative electrode materials is obtained by discharging, disassembling, crushing and sorting, and the battery black powder of the waste ternary battery is placed in a tube furnace and roasted at 500-1500°C for 1-3 hours to obtain the roasted battery powder, wherein the roasted battery powder has a certain reducibility. The battery black powder of the unroasted waste ternary battery is used as the unroasted battery powder.
[0043] The reaction equation during the calcination process is as follows:
[0044] LiNi x Co y Mn (1-x-y) O2+C→Li2CO3+MnO+NiO+CoO+Co-Ni-Mn.
[0045] The calcined battery powder and the uncalcined battery powder are mixed in a mass ratio of 1:5-20, and pure water is added for mixing and pulping. During the pulping process, the solid-liquid ratio is 3-5:1 to obtain a slurry. Since the calcined battery powder alone will produce hydrogen when it reacts with acid later, it will explode under pressure and cannot react under pressure. Therefore, in the present disclosure, the amount of calcined battery powder is less than that of the uncalcined battery powder. The calcined battery powder and the uncalcined battery powder are mixed, which not only overcomes the problem that the single calcined battery powder will produce hydrogen when it reacts with acid, but also makes full use of the reducibility of the calcined battery powder, so that the high-valent nickel, cobalt and manganese metals can be converted into ionic states, which is beneficial to improving the subsequent leaching effect.
[0046] In other embodiments of the present disclosure, the mass ratio of the calcined battery powder to the uncalcined battery powder can be, for example, any one of 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:13, 1:15, 1:16, 1:18, 1:20 or a range value between any two of them, and the solid-liquid ratio in the pulping process can be, for example, any one of 3:1, 4:1, 5:1 or a range value between any two of them. After the mixed pulping, the slurry is also subjected to ball milling activation, and the ball milling activation time is 30-90 minutes. Ball milling can activate the battery black powder, so that more positive electrode materials are "exposed", so that it can react better with sulfuric acid in the pressure leaching section, accelerate the reaction rate, and help improve the pressure leaching efficiency.
[0047] (2) Pressure leaching.
[0048] The activated slurry is mixed with acid and leached under pressure, wherein the added acid is sulfuric acid, the amount of sulfuric acid added is 80%-200% of the theoretical consumption of sulfuric acid for leaching all metals in the slurry, the liquid-solid ratio of sulfuric acid to slurry is 2-4:1, the reaction pressure is 0.3-3.0MPa, the reaction temperature is 150-250℃, and the leaching time is 0.5-3.0h. After leaching, the solid and liquid are separated to obtain pressurized leaching liquid and pressurized leaching residue.
[0049] In other embodiments of the present disclosure, the amount of sulfuric acid added is 80%, 90%, 100%, 110%, 120%, 130%, 140%, 150%, 160%, 170%, 180%, 190%, 200% of the theoretical consumption of sulfuric acid for leaching of all metals in the slurry, or a range value between any two of them; the liquid-solid ratio of sulfuric acid to the slurry is 2:1, 3:1, 4:1, or a range value between any two of them; the reaction pressure can be, for example, 0.3 MPa, 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3.0 MPa, or a range value between any two of them; the present disclosure has found that further increasing the reaction pressure has little effect on the leaching rate, while reducing the reaction pressure will lead to a worse leaching rate; therefore, selecting the reaction pressure of 0.3-3.0 MPa provided in the present disclosure can obtain a good leaching rate. The reaction temperature can be, for example, any one of 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, and 250°C, or a range between any two of them, and the leaching time can be any one of 0.5h, 1h, 1.5h, 2h, 2.5h, and 3.0h, or a range between any two of them.
[0050] In the present disclosure, the slurry contains calcined battery powder with reducing properties. Therefore, the use of H2O2 can be avoided in the process of pressurized leaching. The valuable metal elements of nickel, cobalt, manganese and lithium in the waste ternary battery powder can be efficiently extracted without consuming the reducing agent, and the generation of hydrogen can be avoided.
[0051] (3) Precipitation and removal of impurities.
[0052] The pressurized leaching solution is mixed with an oxidant, the amount of the oxidant added is 1-2% of the volume of the pressurized leaching solution, and the first alkaline substance is added to adjust the pH value of the solution to 4.5-6.0 to remove impurities such as iron, aluminum and silicon. After impurities are removed, the solid and liquid are separated to obtain impurity-removed slag and impurity-removed liquid.
[0053] The oxidant includes at least one of hydrogen peroxide, manganese dioxide and chlorine. The oxidant can oxidize the divalent iron ions in the pressurized leaching solution into trivalent iron ions, so that the pressurized leaching solution can be leached under a lower pH condition. The first alkaline substance includes but is not limited to at least one of limestone, sodium carbonate and calcium oxide. The present disclosure takes lime water as the first alkaline substance as an example. Limestone is slightly soluble in water, and carbonate undergoes hydrolysis reaction. At this time, the system contains OH - , at pH 4.5-6.0, OH - It can react with impurities such as iron, aluminum, and silicon in the system to form precipitates, but will not precipitate with the valuable metals to be recovered, thereby effectively removing impurities.
[0054] (4) One-stage hydrolysis and precipitation.
[0055] The impurity-removed liquid is mixed with a buffer solution consisting of Mg(OH)2 and MgSO4 and stirred for 1-3 hours to precipitate nickel ions and cobalt ions, and the solid-liquid separation is performed to obtain the product nickel-cobalt hydroxide and a precipitated liquid.
[0056] The solid content of magnesium hydroxide in the buffer solution is 1%-40%, Mg 2+ The concentration is 5-45 g / L. In other embodiments of the present disclosure, the solid content of magnesium hydroxide in the buffer solution is 1%, 3%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 20%, 25%, 29%, 31%, 35%, 36%, 38%, 40% or any range between two of them, Mg 2+ The concentration can be, for example, 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L, 10 g / L, 12 g / L, 15 g / L, 18 g / L, 20 g / L, 22 g / L, 24 g / L, 25 g / L, 28 g / L, 30 g / L, 32 g / L, 34 g / L, 35 g / L, 38 g / L, 40 g / L, 42 g / L, 45 g / L, or any range between two of them. In the present disclosure, by controlling the solid content of magnesium hydroxide and Mg in the buffer solution, the solid content of magnesium hydroxide and Mg 2+ The concentration can be adjusted to achieve the pH of the system to mainly precipitate nickel ions and cobalt ions, while manganese ions are not precipitated or precipitated in small amounts, thereby ensuring the purity of the nickel cobalt hydroxide product. At the same time, since the present invention adopts a buffer solution to regulate the pH of the solution, the system can be maintained in a stable pH range without the phenomenon of local over-alkalinity. At the same time, the growth rate of the nickel cobalt hydroxide particles is slowed down, the adverse effects of impurities being "entrained, coated, adsorbed" and the like are reduced, the water content of the product is reduced, and the purity and particle size of the product are improved.
[0057] (5) Two-stage hydrolysis and precipitation.
[0058] The first stage precipitation liquid is mixed with a second alkaline substance, the amount of the second alkaline substance added is such that the pH value of the system is adjusted to 7.0-9.0, and a second stage hydrolysis precipitation is performed to completely precipitate nickel ions, cobalt ions and manganese ions, and solid-liquid separation is performed to obtain an intermediate product of nickel cobalt hydroxide and the second stage precipitation liquid.
[0059] In the present disclosure, the second alkaline substance includes but is not limited to at least one of lime milk, sodium carbonate and sodium hydroxide. The pH value of the second-stage hydrolysis precipitation is relatively high. At this time, the nickel ions, cobalt ions and manganese ions that are not completely precipitated in the first-stage hydrolysis can be fully precipitated, ensuring that the valuable metals in the pressurized leaching solution are fully recovered. Since a large amount of manganese ions are precipitated during the second-stage hydrolysis precipitation, the obtained nickel cobalt hydroxide has poor purity and can only be used as an intermediate product. The intermediate product nickel cobalt hydroxide can be returned to the precipitation and impurity removal step. The intermediate product nickel cobalt hydroxide is alkaline and is returned to the precipitation and impurity removal step. On the one hand, the amount of limestone added can be reduced, and on the other hand, the nickel, cobalt and manganese in the intermediate product nickel cobalt hydroxide can be further recovered.
[0060] (6) Lithium extraction.
[0061] The liquid after the second stage precipitation is mixed with the third alkaline substance to precipitate and extract lithium, and the solid-liquid separation is performed to obtain lithium carbonate and magnesium sulfate waste liquid. The amount of the third alkaline substance added is to adjust the pH value of the system to 10-11. The magnesium sulfate waste liquid can be returned to the first hydrolysis precipitation to prepare a buffer solution. In the present disclosure, the third alkaline substance includes but is not limited to at least one of sodium carbonate, potassium carbonate, ammonium carbonate and carbon dioxide. In the present disclosure, carbonate ions are used to precipitate the liquid after the second stage precipitation to generate lithium carbonate.
[0062] All solid-liquid separation methods involved in the present disclosure include but are not limited to filtration, membrane filtration, filter press, centrifugation or sedimentation. During actual recovery, the method can be selected according to the actual situation.
[0063] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0064] Example 1
[0065] This embodiment provides a full-chain integrated method for recovering nickel and cobalt from waste ternary battery powder, which comprises the following steps:
[0066] (1) discharging, disassembling, crushing and sorting the waste ternary batteries to obtain battery black powder, placing it in a tube furnace for reaction for 1 hour at a reaction temperature of 600° C. to obtain a calcined battery powder with reducing properties;
[0067] (2) Mixing the calcined battery powder and the uncalcined waste ternary battery powder in a uniform ratio to obtain a ternary battery powder mixture, and adding pure water to mix and slurry; in the ternary battery powder mixture, the calcined battery powder: uncalcined battery = 1:5, the solid-liquid ratio is 4:1, and the mixture is placed in a ball mill for mechanical activation for 60 minutes to obtain an activated slurry;
[0068] (3) adding the activated slurry and sulfuric acid into a high-pressure reactor for pressure leaching, wherein the amount of sulfuric acid added is 110% of the theoretical consumption of sulfuric acid for leaching all metals in the slurry added into the reactor, the liquid-solid ratio is 3:1, the reaction temperature is 150° C., the reaction pressure is 0.4 MPa, the leaching time is 1 h, and after leaching, the solid and liquid are separated to obtain a pressure leaching solution and a pressure leaching residue;
[0069] (4) adding 30% hydrogen peroxide to the pressurized leaching solution and stirring continuously to convert the divalent iron ions in the solution into trivalent iron ions, wherein the amount of hydrogen peroxide added is 1% of the volume of the pressurized leaching solution, maintaining the solution at a constant temperature of 50° C., adding limestone to adjust the pH to 5.0, removing impurities such as iron, aluminum, and silicon, and performing precipitation separation to obtain a decontaminated slag and a decontaminated liquid.
[0070] (5) The impurity-free solution was continuously added to the buffer solution, the temperature was maintained at 40°C, and stirred for 2.0 hours. The buffer solution contained: 10% solid content of magnesium hydroxide, Mg 2+ The concentration is 15g / L, nickel and cobalt are precipitated, and the product nickel and cobalt hydroxide and a post-precipitation liquid are obtained by filtration;
[0071] (6) adding lime milk to the liquid after the first stage precipitation, adjusting the pH of the solution to 8.5, performing second stage hydrolysis precipitation, filtering to obtain the intermediate product nickel cobalt hydroxide and the liquid after the second stage precipitation, and returning the intermediate product nickel cobalt hydroxide to the precipitation and impurity removal step;
[0072] (7) Sodium carbonate is added to the liquid after the second stage precipitation, and the pH value of the solution is adjusted to 10, and lithium is extracted by precipitation. Lithium carbonate and magnesium sulfate waste liquid are obtained by filtration. The magnesium sulfate waste liquid can be returned to the first stage precipitation to prepare a buffer solution.
[0073] Pass ICP element test:
[0074] Battery black powder: Ni content 21.77%, Co content 3.29%, Mn content 4.27%, Fe content 0.21%, Al content 0.21%, Cu content 0.24%;
[0075] Pressure leaching residue: Ni content 1.27%, Co content 0.58%, Mn content 0.88%, Fe content 0.08%, Al content 0.07%, Cu content 0.08%;
[0076] Pressurized leaching solution: Ni concentration 18.31g / L, Co concentration 2.78g / L, Mn concentration 4.52g / L, Fe concentration 0.15g / L, Al concentration 0.07g / L, Cu concentration 0.006g / L;
[0077] Product nickel cobalt hydroxide: Ni content 40.21%, Co content 4.86%, Mn content 6.17%, Fe content 0.01%, Al content 0.01%, Cu content 0.002%, Mg content 1.47%;
[0078] Liquid after the first stage of precipitation: Ni concentration is 0.42g / L, Co concentration is 0.026g / L, Mn concentration is 2.86g / L, Fe concentration is 0.003g / L, Al concentration is 0.002g / L, and Cu concentration is 0.001g / L.
[0079] Example 2
[0080] This embodiment provides a full-chain integrated method for recovering nickel and cobalt from waste ternary battery powder, which comprises the following steps:
[0081] (1) discharging, disassembling, crushing and sorting the waste ternary batteries to obtain battery black powder, placing it in a tube furnace for reaction for 2 hours at a reaction temperature of 700° C. to obtain a calcined battery powder with reducing properties;
[0082] (2) Mixing the calcined battery powder and the uncalcined waste ternary battery powder in a uniform ratio to obtain a ternary battery powder mixture, and adding pure water to mix and slurry; in the ternary battery powder mixture, the calcined battery powder: uncalcined battery = 1:10, the solid-liquid ratio is 4:1, and the mixture is placed in a ball mill for mechanical activation for 60 minutes to obtain an activated slurry;
[0083] (3) adding the activated slurry and sulfuric acid to a high-pressure reactor for pressure leaching, wherein the amount of sulfuric acid added is 150% of the theoretical consumption of sulfuric acid for leaching all metals in the slurry added to the reactor, the liquid-solid ratio is 3:1, the reaction temperature is 210° C., the reaction pressure is 2.3 MPa, the leaching time is 2 h, and after leaching, the solid and liquid are separated to obtain a pressure leaching solution and a pressure leaching residue;
[0084] (4) adding 30% hydrogen peroxide to the pressurized leaching solution and stirring continuously to convert the divalent iron ions in the solution into trivalent iron ions, wherein the amount of hydrogen peroxide added is 1% of the volume of the leaching solution, maintaining the solution at a constant temperature of 50° C., adding limestone to adjust the pH to 5.0, removing impurities such as iron, aluminum, and silicon, and performing precipitation separation to obtain a decontaminated slag and a decontaminated liquid.
[0085] (5) The impurity-free solution was continuously added to the buffer solution, the temperature was maintained at 40°C, and stirred for 1.0 h. The buffer solution contained: 20% solid content of magnesium hydroxide, Mg 2+The concentration is 30g / L, nickel and cobalt are precipitated, and the product nickel and cobalt hydroxide and a post-precipitation liquid are obtained by filtration;
[0086] (6) adding lime milk to the liquid after the first stage precipitation, adjusting the pH of the solution to 8.5, performing second stage hydrolysis precipitation, filtering to obtain the intermediate product nickel cobalt hydroxide and the liquid after the second stage precipitation, and returning the intermediate product nickel cobalt hydroxide to the precipitation and impurity removal step;
[0087] (7) Sodium carbonate is added to the liquid after the second stage precipitation, and the pH value of the solution is adjusted to 10.5. Lithium is extracted by precipitation, and lithium carbonate and magnesium sulfate waste liquid are obtained by filtration. The magnesium sulfate waste liquid can be returned to the first stage precipitation to prepare a buffer solution.
[0088] Pass ICP element test:
[0089] Battery black powder: Ni content 21.77%, Co content 3.29%, Mn content 4.27%, Fe content 0.21%, Al content 0.21%, Cu content 0.24%;
[0090] Pressure leaching residue: Ni content 0.11%, Co content 0.01%, Mn content 0.04%, Fe content 0.18%, Al content 0.01%, Cu content 0.0001%;
[0091] Pressurized leaching solution: Ni concentration 22.38g / L, Co concentration 3.41g / L, Mn concentration 5.14g / L, Fe concentration 0.18g / L, Al concentration 0.09g / L, Cu concentration 0.01g / L;
[0092] Product nickel cobalt hydroxide: Ni content 46.52%, Co content 6.75%, Mn content 7.52%, Fe content 0.01%, Al content 0.009%, Cu content 0.003%, Mg content 1.50%;
[0093] Liquid after the first stage of precipitation: Ni concentration is 0.07g / L, Co concentration is 0.0001g / L, Mn concentration is 2.54g / L, Fe concentration is 0.002g / L, Al concentration is 0.001g / L, and Cu concentration is 0.001g / L.
[0094] Example 3
[0095] This embodiment provides a full-chain integrated method for recovering nickel and cobalt from waste ternary battery powder, which comprises the following steps:
[0096] (1) discharging, disassembling, crushing and sorting the waste ternary batteries to obtain battery black powder, placing it in a tube furnace for reaction for 1 hour at a reaction temperature of 1500° C. to obtain a calcined battery powder with reducing properties;
[0097] (2) Mixing the calcined battery powder and the uncalcined waste ternary battery powder in a uniform ratio to obtain a ternary battery powder mixture, and adding pure water to mix and slurry; in the ternary battery powder mixture, the calcined battery powder: uncalcined battery = 1:20, the solid-liquid ratio is 5:1, and the mixture is placed in a ball mill for mechanical activation for 90 minutes to obtain an activated slurry;
[0098] (3) adding the activated slurry and sulfuric acid into a high-pressure reactor for pressurized leaching, wherein the amount of sulfuric acid added is 200% of the theoretical consumption of sulfuric acid for leaching all metals in the slurry added into the reactor, the liquid-solid ratio is 2:1, the reaction temperature is 250° C., the reaction pressure is 3 MPa, the leaching time is 0.5 h, and after leaching, the solid and liquid are separated to obtain a pressurized leaching solution and a pressurized leaching residue;
[0099] (4) adding 30% hydrogen peroxide to the pressurized leaching solution and stirring continuously to convert the divalent iron ions in the solution into trivalent iron ions, wherein the amount of hydrogen peroxide added is 1% of the volume of the pressurized leaching solution, maintaining the solution at a constant temperature of 50° C., adding limestone to adjust the pH to 4.5, removing impurities such as iron, aluminum, and silicon, and performing precipitation separation to obtain a decontaminated slag and a decontaminated liquid.
[0100] (5) The impurity-free solution was continuously added to the buffer solution, the temperature was maintained at 40°C, and stirred for 1.0 h. The buffer solution contained: 40% solid content of magnesium hydroxide, Mg 2+ The concentration is 45g / L, nickel and cobalt are precipitated, and the product nickel and cobalt hydroxide and a post-precipitation liquid are obtained by filtration;
[0101] (6) adding lime milk to the liquid after the first stage precipitation, adjusting the pH of the solution to 8.5, performing second stage hydrolysis precipitation, filtering to obtain the intermediate product nickel cobalt hydroxide and the liquid after the second stage precipitation, and returning the intermediate product nickel cobalt hydroxide to the precipitation and impurity removal step;
[0102] (7) Sodium carbonate is added to the liquid after the second stage precipitation, and the pH value of the solution is adjusted to 10.5. Lithium is extracted by precipitation, and lithium carbonate and magnesium sulfate waste liquid are obtained by filtration. The magnesium sulfate waste liquid can be returned to the first stage precipitation to prepare a buffer solution.
[0103] Pass ICP element test:
[0104] Battery black powder: Ni content 21.77%, Co content 3.29%, Mn content 4.27%, Fe content 0.21%, Al content 0.21%, Cu content 0.24%;
[0105] Pressure leaching slag: Ni content 0.05%, Co content 0.001%, Mn content 0.02%, Fe content 0.07%, Al content 0.03%, Cu content 0.0001%;
[0106] Pressurized leaching solution: Ni concentration 23.38g / L, Co concentration 3.51g / L, Mn concentration 5.34g / L, Fe concentration 0.23g / L, Al concentration 0.12g / L, Cu concentration 0.05g / L;
[0107] Product nickel cobalt hydroxide: Ni content 43.52%, Co content 6.25%, Mn content 7.82%, Fe content 0.001%, Al content 0.005%, Cu content 0.002%, Mg content 1.53%;
[0108] Liquid after the first stage of precipitation: Ni concentration 0.003g / L, Co concentration 0.0001g / L, Mn concentration 1.44g / L, Fe concentration 0.002g / L, Al concentration 0.0001g / L, Cu concentration 0.0001g / L.
[0109] Comparative Example 1
[0110] This comparative example discloses a method for recovering nickel and cobalt from ternary battery powder, which adopts a method of H2SO4 atmospheric pressure leaching-NaOH / Na2CO3 precipitation of nickel, cobalt and manganese, and specifically comprises the following steps:
[0111] (1) discharging, disassembling, crushing and sorting waste ternary batteries to obtain battery black powder mixed with positive and negative electrode materials and pure water to prepare a slurry with a solid-liquid ratio of 4:1, putting it into a ball mill, and mechanically activating it for 60 minutes to obtain an activated slurry;
[0112] (2) adding the activated slurry and sulfuric acid into a beaker for leaching, wherein the amount of sulfuric acid added is 150% of the theoretical consumption of sulfuric acid for leaching all metals in the slurry added into the reactor, the liquid-solid ratio is 3:1, the reaction temperature is 80°C, the reaction pressure is 0.1 MPa, the leaching time is 2 h, and after leaching, the solid and liquid are separated to obtain atmospheric pressure leaching solution and atmospheric pressure leaching residue;
[0113] (3) adding 30% hydrogen peroxide to the pressurized leaching solution and stirring continuously to convert the divalent iron ions in the solution into trivalent iron ions, wherein the amount of hydrogen peroxide added is 1% of the volume of the pressurized leaching solution, maintaining the solution at a constant temperature of 50° C., adding limestone to adjust the pH to 5.0, removing impurities such as iron, aluminum, and silicon, and performing precipitation separation to obtain a decontaminated slag and a decontaminated liquid.
[0114] (4) continuously adding NaOH or Na2CO3 solution to the impurity-removed liquid, maintaining the temperature at 40° C., stirring for 2.0 h, adjusting the pH to 8.0, precipitating nickel and cobalt, and filtering to obtain the product nickel-cobalt hydroxide and a first precipitated liquid;
[0115] (5) adding lime milk to the liquid after the first stage precipitation, adjusting the pH of the solution to 8.5, performing second stage hydrolysis precipitation, and filtering to obtain the intermediate product nickel cobalt hydroxide and the liquid after the second stage precipitation;
[0116] (6) Sodium carbonate is added to the liquid after the second-stage precipitation, and the pH value of the solution is adjusted to 10.5, and lithium is extracted by precipitation, and lithium carbonate and magnesium sulfate waste liquid are obtained by filtration.
[0117] Pass ICP element test:
[0118] Battery black powder: Ni content 21.77%, Co content 3.29%, Mn content 4.27%, Fe content 0.21%, Al content 0.21%, Cu content 0.24%;
[0119] Atmospheric pressure leaching residue: Ni content 17.32%, Co content 2.52%, Mn content 3.34%, Fe content 0.13%, Al content 0.11%, Cu content 0.11%;
[0120] Atmospheric pressure leaching solution: Ni concentration 4.28g / L, Co concentration 0.47g / L, Mn concentration 1.10g / L, Fe concentration 0.124g / L, Al concentration 0.05g / L, Cu concentration 0.01g / L;
[0121] Product nickel cobalt hydroxide: Ni content 36.54%, Co content 3.45%, Mn content 5.36%, Fe content 0.06%, Al content 0.01%, Cu content 0.02%, Mg content 1.1%;
[0122] Liquid after the first stage of precipitation: Ni concentration is 0.07g / L, Co concentration is 0.0001g / L, Mn concentration is 0.84g / L, Fe concentration is 0.002g / L, Al concentration is 0.001g / L, and Cu concentration is 0.001g / L.
[0123] This comparative example is a method of H2SO4 atmospheric pressure leaching-NaOH / Na2CO3 precipitation of nickel, cobalt and manganese, which does not include the synergistic pressure leaching of calcined-uncalcined battery powder and buffer solution as a precipitant in the present disclosure. The leaching efficiency is low and the leaching rate is low. The prepared nickel cobalt hydroxide product has a low Ni+Co+Mn metal content. Due to the strong alkalinity, the product grains grow too fast, resulting in too fine grains, and there are more coated water molecules and impurities. The leaching efficiency and leaching rate of this process are low. The produced nickel cobalt hydroxide has a finer particle size than that of the embodiment, a higher water content and a lower nickel and cobalt content.
[0124] Comparative Example 2
[0125] This comparative example is basically the same as Example 1, except that this comparative example only uses unfired battery powder for activation, wherein step (1): discharging, disassembling, crushing and sorting waste ternary batteries to obtain battery black powder; step (2): adding pure water to the unfired waste ternary battery powder for mixing and slurrying; the solid-liquid ratio is 4:1, and the mixture is placed in a ball mill for mechanical activation for 60 minutes to obtain an activated slurry.
[0126] Pass ICP element test:
[0127] Pressure leaching residue: Ni content 15.27%, Co content 2.48%, Mn content 2.57%, Fe content 0.08%, Al content 0.07%, Cu content 0.08%;
[0128] Pressurized leaching solution: Ni concentration 4.88g / L, Co concentration 0.53g / L, Mn concentration 1.26g / L, Fe concentration 0.15g / L, Al concentration 0.07g / L, Cu concentration 0.006g / L;
[0129] It can be seen from the data of Example 1 and Comparative Example 2 that without adding the reducing roasted battery powder, the leaching effect is extremely poor, wherein the high-valent nickel, cobalt and manganese metals cannot be converted into ions and cannot be recycled.
[0130] Comparative Example 3
[0131] This comparative example is basically the same as Example 1, except that activation is not performed in this comparative example, wherein, step (2): the calcined battery powder and the uncalcined waste ternary battery powder are mixed evenly in proportion to obtain a ternary battery powder mixture, and pure water is added for mixing and slurrying; in the ternary battery powder mixture, the calcined battery powder: uncalcined battery = 1:5, and the solid-liquid ratio is 4:1.
[0132] Pass ICP element test:
[0133] Pressure leaching residue: Ni content 2.27%, Co content 0.65%, Mn content 1.02%, Fe content 0.11%, Al content 0.11%, Cu content 0.12%;
[0134] Pressurized leaching solution: Ni concentration 16.51 g / L, Co concentration 2.48 g / L, Mn concentration 4.02 g / L, Fe concentration 0.11 g / L, Al concentration 0.05 g / L, Cu concentration 0.005 g / L.
[0135] It can be seen from the data of Example 1 and Comparative Example 3 that if the battery powder is not activated, the leaching effect is slightly worse than that after activation, and the reaction time is longer.
[0136] Comparative Example 4
[0137] This comparative example is basically the same as Example 1, except that atmospheric pressure leaching is used in this comparative example. Wherein, step (3): adding the activated slurry and sulfuric acid to a reactor for atmospheric pressure leaching, the amount of sulfuric acid added is 110% of the theoretical sulfuric acid consumption for leaching all metals in the slurry added to the reactor, the liquid-solid ratio is 3:1, the reaction temperature is 80°C, the reaction pressure is 0.1MPa, the leaching time is 1h, and after leaching, the solid-liquid separation is performed to obtain a leachate and a leaching residue.
[0138] Pass ICP element test:
[0139] Atmospheric pressure leaching residue: Ni content 3.17%, Co content 0.88%, Mn content 1.12%, Fe content 0.15%, Al content 0.12%, Cu content 0.14%;
[0140] Atmospheric pressure leaching solution: Ni concentration is 14.35 g / L, Co concentration is 1.96 g / L, Mn concentration is 3.82 g / L, Fe concentration is 0.10 g / L, Al concentration is 0.04 g / L, and Cu concentration is 0.004 g / L.
[0141] It can be seen from the data of Example 1 and Comparative Example 4 that when leaching battery powder at normal pressure, the leaching rate decreases within the same leaching time, resulting in a longer reaction time and a decreased leaching effect.
[0142] Comparative Example 5
[0143] This comparative example is basically the same as Example 1, except that the solid content of magnesium hydroxide in the buffer solution in this comparative example is 60%, Mg 2+ The concentration is 60g / L.
[0144] Pass ICP element test:
[0145] Product nickel cobalt hydroxide: Ni content 30.54%, Co content 1.86%, Mn content 3.36%, Fe content 0.06%, Al content 0.02%, Cu content 0.02%, Mg content 10.21%;
[0146] It can be seen from the data of Example 1 and Comparative Example 5 that when the solid content of magnesium hydroxide in the buffer solution exceeds a certain range, the nickel and cobalt contents in the product nickel cobalt hydroxide decrease and the impurities increase.
[0147] Comparative Example 6
[0148] This comparative example is basically the same as Example 1, except that the buffer solution in this comparative example is NH4Cl and NH3·H2O, wherein the amount of NH4Cl is 50g, the amount of NH3·H2O is 3.5mL, and 500mL of buffer solution is prepared.
[0149] Pass ICP element test:
[0150] Product nickel cobalt hydroxide: Ni content 38.21%, Co content 4.36%, Mn content 5.67%, Fe content 0.02%, Al content 0.02%, Cu content 0.003%, Mg content 1.3%;
[0151] Liquid after the first stage of precipitation: Ni concentration 0.46g / L, Co concentration 0.056g / L, Mn concentration 2.97g / L, Fe concentration 0.004g / L, Al concentration 0.002g / L, Cu concentration 0.001g / L, Cl concentration 30g / L.
[0152] It can be seen from the data of Example 1 and Comparative Example 6 that the precipitation effect in Comparative Example 6 is slightly worse than that in Example 1, wherein the proportion of valuable metals in the product nickel cobalt hydroxide is slightly lower, and the liquid after one stage of precipitation contains a large amount of impurity chloride ions, requiring excess wastewater treatment, which greatly increases the cost.
[0153] In summary, the present invention provides a full-chain integrated method for recovering nickel and cobalt from waste ternary battery powder, which utilizes calcined battery powder and uncalcined battery powder for mixed pressurized synergistic leaching, wherein the calcined battery powder has a certain reducibility, which can omit the use of H2O2 in the acid leaching process, and thus can efficiently extract the nickel, cobalt, manganese and lithium valuable metal elements in the waste ternary battery powder without consuming the reducing agent, thereby improving the leaching rate and avoiding the generation of hydrogen; then, the valuable metals are precipitated using a buffer solution composed of Mg(OH)2 and MgSO4, and the solid content of magnesium hydroxide and MgSO4 in the buffer solution are controlled in the present invention. 2+ The concentration can be adjusted to achieve the pH of the system to mainly precipitate nickel ions and cobalt ions, while manganese ions are not precipitated or precipitated in small amounts, thereby ensuring the purity of the nickel cobalt hydroxide product. At the same time, since the present invention adopts a buffer solution to regulate the pH of the solution, the system can be maintained in a stable pH range without the phenomenon of local over-alkalinity. At the same time, the growth rate of the nickel cobalt hydroxide particles is slowed down, and the adverse effects of impurities being "entrained, coated, and adsorbed" are reduced, thereby greatly improving the purity of the product and obtaining a product with low water content and large particles.
[0154] The optional implementation modes of the present disclosure are described in detail above, but the present disclosure is not limited thereto. Within the technical concept of the present disclosure, the technical solution of the present disclosure can be subjected to a variety of simple modifications, including combining various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present disclosure and belong to the protection scope of the present disclosure.
[0155] Industrial Applicability
[0156] The present invention provides a full-chain integrated method for recovering nickel and cobalt from waste ternary battery powder, which utilizes calcined battery powder and uncalcined battery powder for mixed pressurized synergistic leaching, wherein the calcined battery powder has a certain reducibility, which can omit the use of H2O2 in the acid leaching process, and thus can efficiently extract nickel, cobalt, manganese and lithium valuable metal elements from the waste ternary battery powder without consuming a reducing agent, thereby improving the leaching rate and avoiding the generation of hydrogen; then, a buffer solution composed of Mg(OH)2 and MgSO4 is used to precipitate the valuable metals, and the present invention controls the solid content of magnesium hydroxide and Mg in the buffer solution. 2+ The concentration can be adjusted to achieve the pH of the system to mainly precipitate nickel ions and cobalt ions, while manganese ions are not precipitated or precipitated in small amounts, thereby ensuring the purity of the nickel cobalt hydroxide product. At the same time, since the present invention adopts a buffer solution to regulate the pH of the solution, the system can be maintained in a stable pH range without the phenomenon of local over-alkalinity. At the same time, the growth rate of the nickel cobalt hydroxide particles is slowed down, and the adverse effects of impurities being "entrained, coated, and adsorbed" are reduced, thereby greatly improving the purity of the product and obtaining a product with low water content and large particles.
Claims
1. A method for recovering nickel and cobalt from waste ternary lithium battery powder with a full chain integration, characterized in that: It includes: Mixed Pulping: Mixing the calcined battery powder and the uncalcined battery powder to obtain slurry; The mass ratio of the calcined battery powder to the uncalcined battery powder is 1:5-20; the calcined battery powder is obtained by placing the battery black powder of the waste ternary lithium battery in a tube furnace and calcining it at 500-1500°C for 1-3h; the battery black powder of the uncalcined waste ternary lithium battery is used as the uncalcined battery powder; after the mixed pulping, the slurry is also subjected to ball milling activation, and the ball milling activation time is 30-90min; pressure leaching: the slurry is mixed with acid and pressure leached, the reaction pressure is 0.3-3.0MPa, and solid-liquid separation is performed after leaching to obtain a pressurized leaching liquid and a pressurized leaching residue; Precipitation and impurity removal: after mixing the pressurized leaching solution with an oxidant, adjusting the solution pH to 4.5-6.0 to remove impurities such as iron, aluminum and silicon, and separating the solid and liquid after impurity removal to obtain impurity-removed slag and impurity-removed liquid; One-stage hydrolysis precipitation: the impurity-removed liquid is mixed and stirred with a buffer solution composed of Mg(OH)2 and MgSO4 to precipitate nickel ions and cobalt ions, wherein the solid content of magnesium hydroxide in the buffer solution is 1%-40%, and the solid content of Mg(OH)2 and MgSO4 is 1%-40%. 2+ The concentration is 5-45g / L, and the solid-liquid separation obtains the product nickel cobalt hydroxide and a post-precipitation liquid.
2. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 1, characterized in that: The solid-liquid ratio during the pulping process is 3-5:
1.
3. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 1, characterized in that: The solvent used in the pulping is water.
4. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 1, characterized in that: In the step of pressure leaching, the reaction temperature is 150-250°C.
5. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 1, characterized in that: In the step of pressurized leaching, the leaching time is 0.5-3.0h.
6. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 1, characterized in that: In the step of pressurized leaching, the acid added is sulfuric acid, the amount of sulfuric acid added is 80%-200% of the theoretical consumption of sulfuric acid for leaching all metals in the slurry, and the liquid-to-solid ratio of the sulfuric acid to the slurry is 2-4:
1.
7. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 1, characterized in that: The oxidant includes at least one of hydrogen peroxide, manganese dioxide and chlorine.
8. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 1, characterized in that: The amount of the oxidant added is 1-2% of the volume of the pressure leaching solution.
9. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 1, characterized in that: In the step of precipitation and impurity removal, a first alkaline substance is used to adjust the pH value of the solution, and the first alkaline substance includes at least one of limestone, sodium carbonate and calcium oxide.
10. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 1, characterized in that: The mixing and stirring time in the hydrolysis and precipitation step is 1-3 hours.
11. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 1, characterized in that: After the first stage hydrolysis precipitation, the method further comprises a second stage hydrolysis precipitation: the first stage precipitation liquid is mixed with a second alkaline substance to adjust the pH value of the system to 7.0-9.0 to perform a second stage hydrolysis precipitation to completely precipitate nickel ions, cobalt ions and manganese ions, and solid-liquid separation is performed to obtain an intermediate product of nickel cobalt hydroxide and the second stage precipitation liquid.
12. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 11, characterized in that: The second alkaline substance includes at least one of lime milk, sodium carbonate and sodium hydroxide.
13. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 11, characterized in that: The intermediate product nickel-cobalt hydroxide is returned to the precipitation and impurity removal.
14. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 11, characterized in that: After the second-stage hydrolysis precipitation, the method further includes lithium extraction: mixing the second-stage precipitation liquid with a third alkaline substance to adjust the pH value of the system to 10-11 to perform precipitation and lithium extraction, and solid-liquid separation to obtain lithium carbonate and magnesium sulfate waste liquid.
15. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 14, characterized in that: The third alkaline substance includes at least one of sodium carbonate, potassium carbonate, ammonium carbonate and carbon dioxide.
16. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 14, characterized in that: The magnesium sulfate waste liquid can be returned to the first-stage hydrolysis precipitation to prepare a buffer solution.
17. The method for recovering nickel and cobalt from waste ternary lithium battery powder according to claim 14, characterized in that: The solid-liquid separation in the steps of pressure leaching, precipitation and impurity removal, the first-stage hydrolysis precipitation, the second-stage hydrolysis precipitation and lithium extraction are independently selected from filtration, membrane filtration, filter pressing, centrifugation or sedimentation.
Citation Information
Patent Citations
Method for synergistically preparing ternary precursor and lithium carbonate by utilizing waste lithium ion battery black powder and nickel-cobalt sulfide ore and application
CN112250120A
Recycling method of waste ternary battery material lithium nickel cobalt manganese
CN113415813A