Wear-resistant graphene ultra-high molecular weight polyethylene material for rollers and preparation method
By combining aramid fiber and graphene oxide composite reinforcement with ultra-high molecular weight polyethylene to form a quadruple hydrogen bond structure, the problem of insufficient strength and wear resistance of the roller material is solved, and the high durability of the roller material is achieved. Grinding, high strength and low friction properties expand its application scope.
Patent Information
- Application Number
- CN202311572360.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-23
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-11-23
AI Technical Summary
Existing roller materials have shortcomings such as high mass, high running resistance, and loud running noise. The application of ultra-high molecular weight polyethylene in rollers is limited by strength and wear resistance.
Aramid fiber and graphene oxide composite reinforcements are used to modify the aramid fiber and graphene through ureidopyrimidinone isocyanate intermediate to form a quadruple hydrogen bond structure, which improves the strength and wear resistance of the material, and through thermal Wear-resistant graphene ultra-high molecular weight polyethylene material is prepared by compression molding technology.
It significantly improves the tensile properties, Rockwell hardness and impact strength of the material, reduces the friction coefficient, improves the wear resistance of the roller, and expands its application prospects in rollers.
Smart Images

Figure BDA0004565898170000041 
Figure BDA0004565898170000071 
Figure BDA0004565898170000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ultra-high molecular weight polyethylene, in particular to a wear-resistant graphene ultra-high molecular weight polyethylene material for rollers and a preparation method thereof. Background Art
[0002] Rollers are important components on belt conveyors. Rollers are mainly made of metal, which has disadvantages such as large mass, high running resistance, and high running noise. In recent years, the development of polymer roller materials has been a research hotspot. Among them, ultra-high molecular weight polyethylene has the advantages of light weight and high wear resistance, and is the most promising polymer material for manufacturing rollers. It is of great significance to improve the strength and friction resistance of ultra-high molecular weight polyethylene and expand its application in rollers.
[0003] Aramid fiber has high strength, high temperature resistance, wear resistance and other properties. As a reinforcement, it is widely used in plastics, rubber and other materials. Graphene oxide is a new type of carbon nanomaterial with high specific surface area, high strength and modulus, and excellent conductivity. Patent CN104047160B discloses the preparation of amino-modified graphene oxide and dopamine-modified aramid fiber, which can obtain aramid fiber with graphene oxide uniformly covered on the surface, which can improve the bonding force between aramid and the matrix material, thereby improving the performance of the composite material. Therefore, aramid fiber and graphene oxide can be combined to form a reinforcement to improve the comprehensive performance of ultra-high molecular weight polyethylene and applied to rollers. Summary of the invention
[0004] The technical problem solved by the present invention is to provide a highly wear-resistant and high-strength graphene ultra-high molecular weight polyethylene material for use in rollers.
[0005] The technical solution provided by the present invention is:
[0006] A method for preparing a wear-resistant graphene ultra-high molecular weight polyethylene material for rollers, comprising the following components in parts by weight: 100 parts by weight of ultra-high molecular weight polyethylene, 2-20 parts by weight of aramid fiber modified graphene composite reinforcement, and 0.1-0.6 parts by weight of antioxidant;
[0007] The preparation method is as follows: S1. Add N,N-dimethylformamide and ureido-pyrimidone-modified aramid fiber into a reaction bottle, stir for 4-8 hours, add ureido-pyrimidone-modified graphene, ultrasonically vibrate for 30-60 minutes, then stir for 6-12 hours, filter, wash with water, and dry to obtain an aramid fiber-modified graphene composite reinforcement.
[0008] S2. Add ultra-high molecular weight polyethylene, aramid fiber modified graphene composite reinforcement, and antioxidant into a torque rheometer for mixing, and then put into a mold, and hot-press mold in a flat vulcanizer to obtain a wear-resistant graphene ultra-high molecular weight polyethylene material for rollers.
[0009] Furthermore, the mass of the ureido-pyrimidone-modified graphene in S1 is 5-30% of the ureido-pyrimidone-modified aramid fiber.
[0010] Furthermore, the torque rheometer in S2 controls the rotor speed to be 100-180 r / min, the temperature to be 200-220° C., and the mixing time to be 8-15 min.
[0011] Furthermore, the pressure in the flat vulcanizing press in S3 is 8-15 MPa, the temperature is 190-220° C., and the hot pressing time is 5-15 min.
[0012] Furthermore, the preparation method of ureidopyrimidone modified graphene is as follows: add solvent and graphene oxide to a reaction bottle, ultrasonically vibrate for 10-30 minutes, add ureidopyrimidone isocyanate intermediate, react at 65-90°C for 12-36 hours, filter, wash with ethanol, and dry to obtain ureidopyrimidone modified graphene.
[0013] Furthermore, the solvent includes acetone, tetrahydrofuran, toluene, N,N-dimethylformamide, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0014] Furthermore, the amount of the ureido pyrimidone isocyanate intermediate used is 150-400% of the graphene oxide.
[0015] Further, the preparation method of ureido-pyrimidone modified aramid fiber is:
[0016] (1) The aramid fiber is immersed in ethanol, and ultrasonically cleaned for 5-20 minutes. The fiber is taken out, washed with water, and dried. Then, the aramid fiber is placed in a cold plasma surface modification treatment apparatus, and the air is evacuated and oxygen is introduced. The pressure is controlled to be 20-50 Pa, and the treatment time is 60-120 seconds to obtain activated aramid fiber.
[0017] (2) The activated aramid fiber is placed in N,N-dimethylformamide, and ureidopyrimidone isocyanate intermediate and dibutyltin dilaurate are added, and the reaction is carried out at 60-80°C for 3-6 hours. The solvent is filtered, and the mixture is washed with water and ethanol in sequence, and dried to obtain ureidopyrimidone modified aramid fiber.
[0018] Furthermore, the masses of the ureidopyrimidone isocyanate intermediate and dibutyltin dilaurate in (2) are 20-80% and 0.1-0.5% of the modified aramid fiber, respectively.
[0019] The technical effect of the present invention is as follows: the surface of aramid fiber is modified by low-oxygen plasma method to increase the content of oxygen-containing bodies such as hydroxyl groups on the surface of aramid fiber; then the isocyanate group of ureidopyrimidone isocyanate intermediate is used to react with the surface hydroxyl groups of graphene oxide and the surface hydroxyl groups of activated aramid fiber, respectively, to obtain ureidopyrimidone-modified aramid fiber and ureidopyrimidone-modified graphene, both of which contain ureidopyrimidone structure, and a unique quadruple hydrogen bond structure is formed during the composite process to obtain aramid fiber modified graphene reinforcement, and the quadruple hydrogen bond effect gives the aramid fiber modified graphene ultra-high strength, toughness and other mechanical properties.
[0020] The present invention utilizes aramid fiber-modified graphene reinforcement to fill and modify ultra-high molecular weight polyethylene, thereby achieving the reinforcement modification of ultra-high molecular weight polyethylene by graphene oxide and aramid fiber, improving its tensile properties, Rockwell hardness and impact strength, while improving the wear resistance of the material, showing a lower friction coefficient, and having broad application prospects in rollers. DETAILED DESCRIPTION
[0021] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0022] Ultra-high molecular weight polyethylene: brand L3000, Dongguan Kaiwan Engineering Plastics Raw Materials
[0023] Aramid fiber: Aramid fiber 1414, average length 3mm, Shanghai Ruiyan Economic and Trade.
[0024] Graphene oxide: thickness 0.33-1.0nm, sheet diameter 0.5-5um. Shanghai Yuanye Biotechnology.
[0025] Preparation method of ureidopyrimidone isocyanate intermediate: add 15g of 2-amino-4-hydroxy-6-methylpyrimidine and 150g of hexamethylene diisocyanate to a reaction bottle, reflux at 100°C for 18 hours in a nitrogen atmosphere, cool, add pentane to precipitate, filter, wash with acetone, use a Soxhlet extractor, reflux pentane for extraction, and dry to obtain a ureidopyrimidone isocyanate intermediate with the structural formula:
[0026]
[0027] Example 1
[0028] Add 50 mL of toluene solvent and 0.5 g of graphene oxide to the reaction bottle, ultrasonically shake for 20 min, add 0.75 g of ureidopyrimidone isocyanate intermediate, react at 65 ° C for 36 h, filter, wash with ethanol, and dry to obtain ureidopyrimidone modified graphene.
[0029] The aramid fiber was immersed in ethanol and cleaned by ultrasonic vibration for 10 minutes. The fiber was taken out, washed with water and dried. Then the aramid fiber was placed in a cold plasma surface modification treatment instrument, the air was evacuated and oxygen was introduced. The pressure was controlled at 50Pa and the treatment time was 60s to obtain activated aramid fiber.
[0030] 10 g of activated aramid fiber was placed in N, N-dimethylformamide, 2 g of ureidopyrimidone isocyanate intermediate and 0.01 g of dibutyltin dilaurate were added, and the mixture was reacted at 70°C for 4 h. The solvent was filtered, and the mixture was washed with water and ethanol in sequence and dried to obtain ureidopyrimidone modified aramid fiber.
[0031] The preparation method is as follows: S1. Add 200 mL of N,N-dimethylformamide and 10 g of ureido-pyrimidone-modified aramid fiber into a reaction bottle, stir for 4 h, add 0.5 g of ureido-pyrimidone-modified graphene, ultrasonically vibrate for 30 min, then stir for 12 h, filter, wash with water, and dry to obtain an aramid fiber-modified graphene composite reinforcement.
[0032] 100g ultra-high molecular weight polyethylene, 2g aramid fiber modified graphene composite reinforcement, and 0.5g antioxidant 1076 were added to the torque rheometer for mixing, with the rotor speed of 180r / min, the temperature of 200°C, and the mixing time of 15min; then put into the mold, and hot-pressed in a flat vulcanizer at a pressure of 10MPa, a temperature of 190°C, and a hot-pressing time of 15min to obtain a wear-resistant graphene ultra-high molecular weight polyethylene material for rollers.
[0033] Example 2
[0034] Add 100 mL of tetrahydrofuran solvent and 0.5 g of graphene oxide to the reaction bottle, ultrasonically shake for 20 min, add 1.5 g of ureidopyrimidone isocyanate intermediate, react at 90° C. for 12 h, filter, wash with ethanol, and dry to obtain ureidopyrimidone modified graphene.
[0035] The aramid fiber was immersed in ethanol and cleaned by ultrasonic vibration for 5 minutes. The fiber was taken out, washed with water and dried. Then the aramid fiber was placed in a cold plasma surface modification treatment instrument, the air was evacuated and oxygen was introduced. The pressure was controlled at 20 Pa and the treatment time was 120 seconds to obtain activated aramid fiber.
[0036] 10 g of activated aramid fiber was placed in N,N-dimethylformamide, 5 g of ureidopyrimidone isocyanate intermediate and 0.03 g of dibutyltin dilaurate were added, and the mixture was reacted at 80°C for 3 h. The solvent was filtered, and the mixture was washed with water and ethanol in sequence and dried to obtain ureidopyrimidone modified aramid fiber.
[0037] The preparation method is as follows: S1. Add 400 mL of N,N-dimethylformamide and 10 g of ureido-pyrimidone-modified aramid fiber into a reaction bottle, stir for 6 hours, add 1.5 g of ureido-pyrimidone-modified graphene, ultrasonically vibrate for 60 minutes, then stir for 6 hours, filter, wash with water, and dry to obtain an aramid fiber-modified graphene composite reinforcement.
[0038] 100g of ultra-high molecular weight polyethylene, 10g of aramid fiber modified graphene composite reinforcement, and 0.5g of antioxidant 1076 were added to the torque rheometer for mixing, with the rotor speed of 150r / min, the temperature of 210°C, and the mixing time of 10min; then put into the mold, and hot-pressed in a flat vulcanizer at a pressure of 10MPa, a temperature of 210°C, and a hot-pressing time of 10min to obtain a wear-resistant graphene ultra-high molecular weight polyethylene material for rollers.
[0039] Example 3
[0040] Add 80 mL of N,N-dimethylformamide solvent and 0.5 g of graphene oxide to the reaction bottle, ultrasonically vibrate for 10 min, add 2 g of ureidopyrimidone isocyanate intermediate, react at 80 ° C for 24 h, filter, wash with ethanol, and dry to obtain ureidopyrimidone modified graphene.
[0041] The aramid fiber was immersed in ethanol and cleaned by ultrasonic vibration for 20 minutes. The fiber was taken out, washed with water and dried. Then the aramid fiber was placed in a cold plasma surface modification treatment instrument, the air was evacuated and oxygen was introduced. The pressure was controlled at 40Pa and the treatment time was 90s to obtain activated aramid fiber.
[0042] 10 g of activated aramid fiber was placed in N,N-dimethylformamide, 8 g of ureidopyrimidone isocyanate intermediate and 0.05 g of dibutyltin dilaurate were added, and the mixture was reacted at 60°C for 6 h. The solvent was filtered, and the mixture was washed with water and ethanol in sequence and dried to obtain ureidopyrimidone modified aramid fiber.
[0043] The preparation method is as follows: S1. Add 300 mL of N,N-dimethylformamide and 10 g of ureido-pyrimidone-modified aramid fiber into a reaction bottle, stir for 6 h, add 3 g of ureido-pyrimidone-modified graphene, ultrasonically vibrate for 60 min, then stir for 12 h, filter, wash with water, and dry to obtain an aramid fiber-modified graphene composite reinforcement.
[0044] 100g of ultra-high molecular weight polyethylene, 20g of aramid fiber modified graphene composite reinforcement, and 0.5g of antioxidant 1076 were added to the torque rheometer and mixed at a rotor speed of 100r / min, a temperature of 220°C, and a mixing time of 8min; then put into a mold and hot-pressed in a flat vulcanizer at a pressure of 8MPa, a temperature of 220°C, and a hot-pressing time of 5min to obtain a wear-resistant graphene ultra-high molecular weight polyethylene material for rollers.
[0045] Comparative Example 1
[0046] The difference between this comparative example and Example 1 is that no aramid fiber-modified graphene composite reinforcement is added, and 2 g of ureidopyrimidone-modified graphene is added.
[0047] 100g of ultra-high molecular weight polyethylene, 2g of ureido-pyrimidone-modified graphene, and 0.5g of antioxidant 1076 were added to a torque rheometer and mixed at a rotor speed of 180r / min, a temperature of 200°C, and a mixing time of 15min; then put into a mold and hot-pressed in a flat vulcanizer at a pressure of 10MPa, a temperature of 190°C, and a hot-pressing time of 15min to obtain an ultra-high molecular weight polyethylene material.
[0048] Comparative Example 2
[0049] The difference between this comparative example and Example 1 is that no aramid fiber-modified graphene composite reinforcement is added, and 2 g of ureidopyrimidone-modified aramid fiber is added.
[0050] 100g of ultra-high molecular weight polyethylene, 2g of ureido-pyrimidone-modified aramid fiber, and 0.5g of antioxidant 1076 were added to a torque rheometer and mixed at a rotor speed of 180r / min, a temperature of 200°C, and a mixing time of 15min; then they were put into a mold and hot-pressed in a flat vulcanizer at a pressure of 10MPa, a temperature of 190°C, and a hot-pressing time of 15min to obtain an ultra-high molecular weight polyethylene material.
[0051] Comparative Example 3
[0052] The difference between this comparative example and Example 1 is that: no aramid fiber-modified graphene composite reinforcement is added, and 0.33 g of ureidopyrimidone-modified graphene and 1.67 g of aramid fiber are added.
[0053] 100g ultra-high molecular weight polyethylene, 0.33g ureido pyrimidone modified graphene, 1.67g aramid fiber, and 0.5g antioxidant 1076 were added to the torque rheometer and mixed at a rotor speed of 180r / min, a temperature of 200°C, and a mixing time of 15min; then put into a mold and hot-pressed in a flat vulcanizer at a pressure of 10MPa, a temperature of 190°C, and a hot-pressing time of 15min to obtain an ultra-high molecular weight polyethylene material.
[0054] Comparative Example 4
[0055] The difference between this comparative example and Example 1 is that: no aramid fiber-modified graphene composite reinforcement is added, and 0.33 g of graphene oxide and 1.67 g of ureidopyrimidone-modified aramid fiber are added.
[0056] 100g ultra-high molecular weight polyethylene, 0.33g graphene oxide, 1.67g ureido-pyrimidone-modified aramid fiber, and 0.5g antioxidant 1076 were added to a torque rheometer and mixed at a rotor speed of 180r / min, a temperature of 200°C, and a mixing time of 15min; then put into a mold and hot-pressed in a flat vulcanizer at a pressure of 10MPa, a temperature of 190°C, and a hot-pressing time of 15min to obtain an ultra-high molecular weight polyethylene material.
[0057] The tensile properties of ultra-high molecular weight polyethylene materials are tested according to the method of ASTM-D638M. The Rockwell hardness is tested according to the method of GB / T 9342-1988. The impact strength is tested according to the method of GB / T1043.1-2008.
[0058] The friction coefficient of ultra-high molecular weight polyethylene material against steel is tested according to the method of GB / T 10006-2021.
[0059]
[0060]
[0061] In Examples 1-3, graphene oxide and activated aramid fiber were grafted and modified using ureidopyrimidone isocyanate intermediates, respectively, to obtain ureidopyrimidone-modified graphene and ureidopyrimidone-modified aramid fiber. The ureidopyrimidone structure contained in both forms a unique quadruple hydrogen bond structure. The quadruple hydrogen bond effect gives the aramid fiber-modified graphene ultra-high strength, toughness and other mechanical properties; the ultra-high molecular weight polyethylene was filled and modified using aramid fiber-modified graphene reinforcement, thereby achieving the enhanced modification of ultra-high molecular weight polyethylene by graphene oxide and aramid fiber, improving its tensile properties, Rockwell hardness and impact strength, while improving the wear resistance of the material and showing a lower friction coefficient.
[0062] In Comparative Example 1, only urea-pyrimidone-modified graphene was added, and in Comparative Example 2, only urea-pyrimidone-modified aramid fiber was added. The mechanical strength and friction resistance of the ultra-high molecular weight polyethylene were relatively low.
[0063] Urea-pyrimidone-modified graphene and aramid fiber were added in comparative example 3. Graphene oxide and urea-pyrimidone-modified aramid fiber were added in comparative example 4. Neither graphene nor aramid fiber formed a quadruple hydrogen bond structure, and the mechanical strength and friction resistance of ultra-high molecular weight polyethylene were poor.
[0064] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a wear-resistant graphene ultra-high molecular weight polyethylene material for a roller, characterized in that: The invention comprises the following components in parts by weight: 100 parts by weight of ultra-high molecular weight polyethylene, 2-20 parts by weight of aramid fiber modified graphene composite reinforcement, and 0.1-0.6 parts by weight of antioxidant; The preparation method comprises: S1, adding N,N-dimethylformamide and ureido-pyrimidone-modified aramid fiber into a reaction bottle, stirring for 4-8 hours, adding ureido-pyrimidone-modified graphene, ultrasonically shaking for 30-60 minutes, stirring for 6-12 hours, filtering, washing with water, and drying to obtain an aramid fiber-modified graphene composite reinforcement; S2, adding ultra-high molecular weight polyethylene, aramid fiber modified graphene composite reinforcement, and antioxidant into a torque rheometer for mixing, and then putting into a mold, and hot pressing in a flat vulcanizer to obtain a wear-resistant graphene ultra-high molecular weight polyethylene material for rollers; The preparation method of the ureidopyrimidone modified graphene is as follows: adding a solvent and graphene oxide to a reaction bottle, ultrasonically shaking for 10-30 minutes, adding a ureidopyrimidone isocyanate intermediate, reacting at 65-90° C. for 12-36 hours, filtering, washing with ethanol, and drying to obtain the ureidopyrimidone modified graphene; The preparation method of the ureido-pyrimidone-modified aramid fiber is as follows: (1) Soaking the aramid fiber in ethanol, ultrasonically cleaning it for 5-20 minutes, taking out the fiber, washing it with water, and drying it; then placing the aramid fiber in a cold plasma surface modification treatment apparatus, evacuating the air, introducing oxygen, controlling the pressure to 20-50 Pa, and treating it for 60-120 seconds to obtain activated aramid fiber; (2) The activated aramid fiber is placed in N,N-dimethylformamide, and ureidopyrimidone isocyanate intermediate and dibutyltin dilaurate are added. The reaction is carried out at 60-80 °C for 3-6 h. The solvent is filtered, and the mixture is washed with water and ethanol in sequence and dried to obtain ureidopyrimidone modified aramid fiber.
2. The method for preparing the wear-resistant graphene ultra-high molecular weight polyethylene material for rollers according to claim 1, characterized in that: The mass of the ureido-pyrimidone-modified graphene in S1 is 5-30% of the ureido-pyrimidone-modified aramid fiber.
3. The method for preparing the wear-resistant graphene ultra-high molecular weight polyethylene material for rollers according to claim 1, characterized in that: The torque rheometer in S2 controls the rotor speed to be 100-180 r / min, the temperature to be 200-220° C., and the mixing time to be 8-15 min.
4. The method for preparing the wear-resistant graphene ultra-high molecular weight polyethylene material for rollers according to claim 1, characterized in that: The pressure in the flat vulcanizing press in S2 is 8-15 MPa, the temperature is 190-220° C., and the hot pressing time is 5-15 min.
5. The method for preparing the wear-resistant graphene ultra-high molecular weight polyethylene material for rollers according to claim 1, characterized in that: The solvent includes acetone, tetrahydrofuran, toluene, N,N-dimethylformamide, and N,N-dimethylacetamide.
6. The method for preparing the wear-resistant graphene ultra-high molecular weight polyethylene material for rollers according to claim 1, characterized in that: The amount of the ureido pyrimidone isocyanate intermediate used is 150-400% of the graphene oxide.
7. The method for preparing the wear-resistant graphene ultra-high molecular weight polyethylene material for rollers according to claim 1, characterized in that: The masses of the ureido pyrimidone isocyanate intermediate and dibutyltin dilaurate in (2) are 20-80% and 0.1-0.5% of the modified aramid fiber, respectively.