Coated steel with excellent machinability and corrosion resistance

By controlling the Al and Mg content and microstructure in the Zn-Al-Mg coating, the problems of deterioration in workability and reduction in corrosion resistance of coated steel sheets during processing were solved, achieving excellent workability and corrosion resistance.

CN117545870BActive Publication Date: 2026-11-10HYUNDAE STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202280043508.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2022-12-15
Publication Date
2026-11-10
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

Existing Zn-Al-Mg coated steel sheets suffer from deterioration in workability and reduced corrosion resistance during processing, mainly due to the high hardness and low crack resistance of the MgZn2 phase leading to crack formation.

Method used

By controlling the content and microstructure of Al and Mg in the hot-dip alloy coating, and limiting the shape and area ratio of the MgZn2 phase, the microstructure of the coating can be optimized to improve processability and corrosion resistance.

Benefits of technology

This technology enables coated steel with excellent workability and corrosion resistance, reduces crack formation in the coating during processing, and improves the overall performance of the steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117545870B_ABST
    Figure CN117545870B_ABST
Patent Text Reader

Abstract

This invention provides a coated steel with excellent processability and corrosion resistance, the coated steel comprising: base iron; and a hot-dip alloy coating formed on the base iron, the hot-dip alloy coating comprising 5% to 30% by weight Al, 2% to 10% by weight Mg, the balance Zn and other unavoidable impurities, wherein, in the cross-section of the hot-dip alloy coating, the area fraction of the MgZn2 phase is 20% to 70%, and the ratio of the area fraction of the Al phase to the area fraction of the MgZn2 phase is 1% to 70%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a type of steel, and more specifically, to a coated steel with excellent workability and corrosion resistance. Background Technology

[0002] Hot-dip galvanized steel sheets exhibit excellent sacrificial corrosion resistance; when exposed to corrosive environments, the low-potential zinc is preferentially leached away to prevent corrosion. Due to this superior corrosion resistance, hot-dip galvanized steel sheets have been used in household appliances, building materials, and automotive applications. However, with increasing expectations and demands for corrosion resistance due to technological advancements and improved quality levels, the need to develop products with even better corrosion resistance than existing hot-dip galvanized steel sheets is also growing. To address these issues, since the early 2000s, Europe and Japan have begun producing high-corrosion-resistant coated steel sheets by adding aluminum (Al) and magnesium (Mg) to the zinc (Zn) plating bath to enhance corrosion resistance. In addition to the sacrificial corrosion resistance of Zn, high-corrosion-resistant coated steel sheets can form dense corrosion products in corrosive environments due to the addition of Mg and Al, which protect the steel from oxidizing atmospheres, thus improving corrosion resistance. However, while Zn-Al-Mg coated steel sheets offer superior corrosion resistance compared to galvanized steel sheets, they suffer from reduced processability. Zn-Al-Mg intermetallic compounds exhibit high hardness and low crack resistance, and cracks can lead to surface deterioration during processing or reduced corrosion resistance of the base steel. A relevant prior art is found in Japanese Patent Application Publication No. 2005-105367. Summary of the Invention

[0003] Technical issues

[0004] The technical problem to be solved by the present invention is to provide a coated steel with excellent processability and corrosion resistance.

[0005] Technical solution

[0006] According to one aspect of the present invention, a coated steel with excellent workability and corrosion resistance for solving the above-mentioned problems comprises: a base steel; and a hot-dip alloy coating formed on the base steel, wherein the hot-dip alloy coating comprises 5% to 30% by weight Al, 2% to 10% by weight Mg, the balance Zn, and unavoidable impurities. The area fraction of the MgZn2 phase in the cross-section of the hot-dip alloy coating is 20% to 70%, and the ratio of the area fraction of the Al phase to the area fraction of the MgZn2 phase in the cross-section of the hot-dip alloy coating is 1% to 70%.

[0007] According to another aspect of the present invention, a coated steel with excellent workability and corrosion resistance, for solving the above-mentioned problems, comprises: a base steel; and a hot-dip alloy coating formed on the base steel, wherein the hot-dip alloy coating comprises 5% to 30% by weight Al, 2% to 10% by weight Mg, the balance Zn, and unavoidable impurities. In the entire MgZn2 phase on the surface of the hot-dip alloy coating, the area fraction of the MgZn2 phase with an average minor axis length (a) to average major axis length (b) ratio of 0.5 or less is 70% or less.

[0008] In coated steel, in the MgZn2 phase where the ratio of the average minor axis length (a) to the average major axis length (b) is 0.5 or less, the ratio of the average minor axis length (a) to the average major axis length (b) can be 1 / 10 or greater and can be 1 / 2 or less.

[0009] In the coated steel described herein, the average minor axis length (a) can be from 1 μm to 20 μm, and the average major axis length (b) can be from 2 μm to 200 μm.

[0010] In the coated steel described herein, the area fraction of Al-Zn dendrites composed of Al and Zn phases on the surface of the hot-dip alloy coating can be 30% or less.

[0011] In the coated steel described herein, the area fraction of the MgZn2 phase with an average minor axis length (a) to average major axis length (b) greater than 0.5 in the entire MgZn2 phase on the surface of the hot-dip alloy coating can be 30% or greater.

[0012] In the coated steel described herein, the diameter of the imaginary circle having the same area as the cross-sectional area of ​​the MgZn2 phase with an average minor axis length (a) to average major axis length (b) greater than 0.5 can be from 1 μm to 50 μm.

[0013] In the coated steels described herein, the hot-dip alloy coating may also contain 0.05% to 10% by weight of Fe and more than 0% and less than 1% of Si.

[0014] Beneficial effects

[0015] According to embodiments of the present invention, coated steel with excellent processability and corrosion resistance can be achieved.

[0016] It should be noted that the scope of the present invention is not limited by these effects. Attached Figure Description

[0017] Figure 1 This is a photograph of the surface of the hot-dip alloy coating in Example 2 of the first experimental example.

[0018] Figure 2 It is a 1000x magnified FE-SEM image of the cross-section of the hot-dip alloy coating in Example 2 of the first experimental example.

[0019] Figure 3 This is a 500x magnified FE-SEM image of the processed part after evaluating the 1T bending workability of the hot-dip alloy coating according to Example 2 in the first experimental example. Detailed Implementation

[0020] The coated steel with excellent workability and corrosion resistance according to embodiments of the present invention will be described in detail. The terminology used herein is appropriately selected with regard to its function in the invention. Therefore, the definitions of the terms should be based on the entire contents of this specification. Specific details of ultra-high strength, highly corrosion-resistant coated steel sheets with excellent elongation and methods for manufacturing the same will be provided below.

[0021] As mentioned above, compared with galvanized steel sheet, Zn-Al-Mg coated steel sheet has excellent corrosion resistance, but it suffers from poor processability. The Zn-Al-Mg intermetallic compound exhibits high hardness and low crack resistance, and cracks lead to surface deterioration during processing or reduced corrosion resistance of the base steel. Among the intermetallic compounds, MgZn2 has the highest hardness; therefore, techniques to suppress the shape and size of the MgZn2 phase are important.

[0022] The purpose of this invention is to provide a Zn-Al-Mg based high corrosion-resistant coated steel containing 5% to 30% by weight of Al, 2% to 10% by weight of Mg, the balance of Zn and unavoidable impurities, and to control the microstructure of the high-hardness MgZn2 phase to improve processability and corrosion resistance during processing.

[0023] The coated steel with excellent workability and corrosion resistance according to embodiments of the present invention comprises: a base steel; and a hot-dip alloy coating formed on the base steel, wherein the hot-dip alloy coating comprises 5% to 30% by weight Al, 2% to 10% by weight Mg, the balance Zn, and unavoidable impurities. Furthermore, the hot-dip alloy coating may also comprise 0.05% to 10% by weight Fe and greater than 0% and less than 1% by weight Si.

[0024] The zinc alloy coating of the present invention can be composed of a primary Al phase (a single-phase Al structure with Zn solid solution), a Zn solid solution phase, and MgZn2 (including Al-containing MgZn2 phase and Mg2Zn). 11 The coating consists of a phase and an Al / Zn / Mg eutectic structure. The MgZn2 phase and the Al-containing MgZn2 phase on the surface of the Zn-Al-Mg based coating can have polygonal, rod-shaped and needle-shaped shapes in terms of microstructure to improve processability and corrosion resistance.

[0025] Zinc alloy coatings can contain 5% to 30% by weight Al, 2% to 10% by weight Mg, the balance Zn, and unavoidable impurities. Mg and Al in the coating are elements that improve corrosion resistance by forming corrosion products more densely. If Mg is less than 1.0% by weight, its contribution to corrosion resistance is negligible, and in related technologies, the amount of Mg used is less than 2.0% by weight because when the Mg content is greater than 2.0% by weight, production becomes difficult due to Mg oxide scum. However, in this invention, the amount of Mg added is 2.0% by weight or more to achieve better corrosion resistance. As mentioned above, when the amount of Mg added is greater than 2.0% by weight, production becomes difficult due to oxide scum. However, when the amount of Al added is 5.0% by weight or more, scum caused by Mg oxidation in the molten metal can be reduced. Furthermore, when Al is added, it can improve corrosion resistance by forming primary Al and a Zn-Al-Mg ternary eutectic phase. On the other hand, if the amount of Mg added is greater than 10.0% by weight, the growth of the aforementioned rod-shaped and needle-shaped MgZn2 or Al-containing MgZn2 phases exceeds 70% of the total MgZn2 area fraction. Therefore, the processability of the coating deteriorates, and cracks are generated in the coating during processing, thereby reducing the corrosion resistance of the steel or the Fe-Al-Zn interfacial alloy layer. Conversely, if the amount of Al added is greater than 30% by weight, the discontinuous Fe-Al-Zn interfacial alloy layer between the steel and the coating overgrows due to the increased melting point of the plating bath, resulting in poor interfacial adhesion during processing.

[0026] An exemplary process for forming a hot-dip alloy coating on base steel in this invention is as follows.

[0027] First, the base steel, annealed at 680℃ to 850℃, is immersed in a plating bath at 440℃ to 530℃, and then, using an air knife, one side of the base steel is made to achieve a coating thickness of 30g / m². 2 Up to 300g / m 2 However, by controlling the entry temperature of the base steel after annealing, there is no difference of ±20℃ or more from the plating bath temperature.

[0028] The shape and proportion of the MgZn2 phase can be precisely controlled through cooling. After immersion in the plating bath, the base steel is cooled at a rate of 3°C / s to 30°C / s, up to a point of 200°C, allowing control over the shape of the phase formed during plating solidification. More preferably, the base steel can be cooled at a rate of 5°C / s to 20°C / s. If the cooling rate is below 5°C / s, the primary MgZn2 phase grows coarsely, deteriorating processability, and the liquid plating may react with oxygen, thus becoming a factor that damages the surface appearance of the plating. On the other hand, when cooling is performed at a rate greater than 30°C / s, the plating cannot form uniformly due to uneven solidification, and productivity is reduced due to steel plate vibration.

[0029] In the coated steel according to one aspect of the present invention, the area fraction of the MgZn2 phase in the cross section (e.g., longitudinal section) of the hot-dip alloy coating is 20% to 70%, and the ratio of the area fraction of the Al-containing phase to the area fraction of the MgZn2 phase in the cross section (e.g., longitudinal section) of the hot-dip alloy coating is 1% to 70%. Here, the Al-containing phase may exist outside or within the MgZn2 phase in the cross section of the hot-dip alloy coating. In addition, in this embodiment, the Al-containing phase refers to i) a single Al phase, and ii) a phase containing 20% ​​or more Al, but containing less than 2% unavoidable impurities and the balance Zn.

[0030] For example, the cross-section of the hot-dip alloy coating contains 20% to 70% MgZn2 phase by area. That is, the cross-sectional area (A2) of the MgZn2 phase is 20% to 70% of the total cross-sectional area (A1) of the hot-dip alloy coating, and the value of (A2 / A1)×100 is in the range of 10 to 60. On the other hand, in the cross-section of the hot-dip alloy coating, the sum of the cross-sectional area (B1) of the Al-containing phase existing outside the MgZn2 phase and the cross-sectional area (B2) of the Al-containing phase existing within the MgZn2 phase is 1% to 70% of the total cross-sectional area (B3) of the MgZn2 phase. That is, the value of [(B1+B2) / B3]×100 is in the range of 1 to 70. According to this structure, crack resistance is excellent; specifically, in bending evaluation (3T bending evaluation, 1T bending evaluation), the average crack width can be 30 μm or less.

[0031] On the surface of the hot-dip alloy coating of the coated steel of the present invention, the area fraction of the MgZn2 phase can be from 10% to 70%. If the area fraction is less than 10%, it is impossible for it to form, and if the area fraction exceeds 70%, the crack resistance is reduced. Here, the surface of the hot-dip alloy coating can refer to the upper surface in contact with the outside.

[0032] In a coated steel according to another aspect of the invention, on the surface of the hot-dip alloy coating of the coated steel, the area fraction of the MgZn2 phase with an average minor axis length (a) to average major axis length (b) ratio of 0.5 or less in the entire MgZn2 phase can be 70% or less. For example, in the entire MgZn2 phase on the surface of the hot-dip alloy coating, the ratio of the average minor axis length (a) to the average major axis length (b) of 70% or less of the MgZn2 phase can be from 1:2 to 1:10, i.e., a value of 0.5 or less. In this case, the MgZn2 phase with an average minor axis length (a) to average major axis length (b) ratio of 0.5 or less can have a ratio of 1 / 10 or greater, and can be 1 / 2 or less. If the ratio of the average minor axis length (a) to the average major axis length (b) is less than 0.5, the crack resistance decreases. The average minor axis length (a) can range from 1 μm to 20 μm, and the average major axis length (b) can range from 2 μm to 200 μm. An average minor axis length (a) less than 1 μm and an average major axis length (b) less than 2 μm cannot be formed, and crack resistance decreases if the average minor axis length (a) exceeds 20 μm or the average major axis length (b) exceeds 200 μm.

[0033] Meanwhile, on the surface of the hot-dip alloy coating of the coated steel according to another aspect of the present invention, the area fraction of Al-Zn dendrites composed of Al and Zn phases can be 30% or less. Al-Zn dendrites preferably have a low area fraction because they are detrimental to chemical conversion treatment performance or resistance to liquid metal embrittlement (LME). Therefore, in the coating according to this embodiment, the area fraction of Al-Zn dendrites is set to 30% or less.

[0034] As described above, in the coated steel with excellent processability and corrosion resistance according to embodiments of the present invention, the MgZn2 phase and the Al-containing MgZn2 phase on the Zn-Al-Mg-based coating surface have polygonal shapes, as well as rod-shaped and needle-shaped shapes, and the ratio of the average minor axis length (a) to the average major axis length (b) of the rod-shaped and needle-shaped shapes is: 1:2 ≤ a:b ≤ 1:10. The rod-shaped and needle-shaped MgZn2 phases in the entire MgZn2 are distributed on the surface with an area fraction of 70% or less, more preferably less than 50%, and the remaining MgZn2 is distributed in a polygonal shape.

[0035] On the surface of a hot-dip alloy coating, the area fraction of the MgZn2 phase with an average minor axis length (a) to average major axis length (b) ratio greater than 0.5 is 30% or greater in the entire MgZn2 phase. For example, in the entire MgZn2 phase on the surface of the hot-dip alloy coating, 30% or more of the MgZn2 phase has an average minor axis length (a) to average major axis length (b) ratio greater than 0.5, for example, 1:1.5 or 1:1.2. The diameter (average diameter) of the imaginary circle having the same cross-sectional area as the MgZn2 phase with an average minor axis length (a) to average major axis length (b) ratio greater than 0.5 can be from 1 μm to 50 μm. If the average diameter is less than 1 μm, it is impossible for it to form; if the average diameter is greater than 50 μm, the crack resistance decreases.

[0036] Preferred experimental examples are presented below to better understand the invention. However, these examples are only for illustrative purposes and are not intended to limit the invention.

[0037] First Experimental Example

[0038] 1. Sample composition and processing conditions

[0039] A 1.2 mm cold-rolled material was prepared as the base steel sheet, with the following composition: 0.15 wt% carbon (C), 0.01 wt% silicon (Si), 0.6 wt% manganese (Mn), 0.05 wt% phosphorus (P), 0.05 wt% sulfur (S), and the balance iron (Fe). After annealing at 760 °C in a nitrogen-5% to 10% hydrogen atmosphere, the annealed sample was cooled to a temperature not exceeding 20 °C from the plating bath temperature and then immersed in the plating bath for 1 to 5 seconds. After immersion in a plating bath at 485 °C, the coating thickness was adjusted to approximately 20 μm by nitrogen purging and cooled at a cooling rate of 7 °C / s to obtain a Zn-Al-Mg based coated steel sheet. The composition of the plating bath met the following range: 5 wt% to 30 wt% Al, 2 wt% to 10 wt% Mg, and the balance Zn.

[0040] 2. Evaluation of coating composition and microstructure

[0041] Table 1 shows the composition (unit: weight %) of the hot-dip alloy coating in the coated steel according to the first experimental example of the present invention, as well as the microstructure evaluation results.

[0042] [Table 1]

[0043]

[0044] For each coated steel sheet manufactured, the surface was observed 500 times using FE-SEM, and the area of ​​rod-shaped and needle-shaped MgZn2 was measured using an image processing program. The thickness of the interfacial alloy layer was measured by magnifying the cross-section 1000 times.

[0045] Referring to Examples 1 to 3 in Table 1, it can be confirmed that the area ratio of rod-shaped and needle-shaped MgZn2 is less than 50%, and the processability is excellent. In the comparative examples compared to the examples, the inventors confirmed that the area of ​​the rod-shaped and needle-shaped MgZn2 phases increased sharply, and that the processability deteriorated due to the formation of an interfacial alloy layer exceeding 10 μm caused by the increase in plating bath temperature.

[0046] Figure 1 This is a photograph of the surface of the hot-dip alloy coating from Example 2 of the first experimental example. (Refer to...) Figure 1 It can be confirmed that the rod-shaped and needle-shaped MgZn2 phases appearing on the surface of the Zn-Al-Mg based coating satisfy the following condition: the ratio of the average minor axis length (a) to the average major axis length (b) falls within the range of 1:2 ≤ a:b ≤ 1:10. Furthermore, it can be confirmed that the rod-shaped and needle-shaped MgZn2 phases are distributed on the surface of the entire MgZn2 layer with an area fraction of 70% or less.

[0047] Figure 2 This is a 1000x magnified FE-SEM image of the cross-section of the hot-dip alloy coating in Example 2 of the first experimental case. (Refer to...) Figure 2 It can be confirmed that the Fe-Al interface alloy layer in the hot-dip alloy coating according to Example 2 is 10 μm or less.

[0048] 3. Evaluation of bending workability

[0049] Table 2 shows the evaluation results of the bending workability of the coated steel according to the first experimental example of the present invention. After 3T bending and 1T bending, the bent processed parts were observed 200 and 500 times using a field emission scanning electron microscope (FE-SEM), and the width of the bending crack was measured and the average value was used for evaluation. In 3T (crack width) and 1T (crack width), "◎" indicates that the average crack width in the bending evaluation is 15 μm or less, "○" indicates that the average crack width in the bending evaluation is greater than 15 μm and less than or equal to 30 μm, and "△" indicates that the average crack width in the bending evaluation is greater than 30 μm and less than or equal to 40 μm.

[0050] In addition, after 3T and 1T bending, the bent processed parts were observed 100 times using FE-SEM (Field Emission Scanning Electron Microscopy), and then the crack area fraction was calculated and evaluated using an image processing program. In 3T (crack area fraction) and 1T (crack area fraction), "◎" indicates that the crack area fraction in the bending evaluation is 30% or less, "○" indicates that the crack area fraction in the bending evaluation is greater than 30% and less than or equal to 50%, and "△" indicates that the crack area fraction in the bending evaluation is greater than 50% and less than or equal to 70%.

[0051] [Table 2]

[0052]

[0053] Referring to Examples 1 to 3 in Table 2, it can be confirmed that the formation of rod-shaped and acicular MgZn2 is relatively low, and the crack width is less than 40 μm. In the comparative examples compared to the embodiments, the inventors confirmed that when the area fraction of rod-shaped and acicular MgZn2 is greater than 70%, cracks propagate along grain boundaries within the high-hardness MgZn2 phase, and the average crack width is greater than 40 μm. Furthermore, in the comparative examples compared to the embodiments, the inventors confirmed that when the MgZn2 phase develops in a rod-like shape, not only does the crack width increase, but the number of crack occurrences also increases, resulting in a crack area greater than 70% and leading to deterioration. Figure 3 This is a 500x magnified FE-SEM image of the processed part after evaluating the 1T bending workability of the hot-dip alloy coating according to Example 2 in the first experimental example. (Refer to...) Figure 3 It can be confirmed that, according to Example 2, the formation of rod-shaped and needle-shaped MgZn2 in the hot-dip alloy coating is relatively small, the crack width is less than 40 μm, and the area fraction of rod-shaped and needle-shaped MgZn2 is 70% or less.

[0054] Based on the results of the first experimental example above, it can be confirmed that even when a high-hardness MgZn2 phase that is detrimental to processability is formed, coated steel sheets with excellent processability can be achieved by suppressing the growth of rod-shaped and needle-shaped MgZn2 phases and controlling their area fraction.

[0055] Second Experimental Example

[0056] 1. Sample composition and processing conditions

[0057] A 1.2 mm cold-rolled material was prepared as the base steel sheet, with the following composition: 0.15 wt% carbon (C), 0.01 wt% silicon (Si), 0.6 wt% manganese (Mn), 0.05 wt% phosphorus (P), 0.05 wt% sulfur (S), and the balance iron (Fe). After annealing at 760 °C in a nitrogen-5% to 10% hydrogen atmosphere, the annealed sample was cooled to a temperature not exceeding 20 °C from the plating bath temperature and then immersed in the plating bath for 1 to 5 seconds. After immersion in a plating bath at 485 °C, the coating thickness was adjusted to approximately 20 μm by nitrogen purging and cooled at a cooling rate of 7 °C / s to obtain a Zn-Al-Mg based coated steel sheet. The composition of the plating bath met the following range: 5 wt% to 30 wt% Al, 2 wt% to 10 wt% Mg, and the balance Zn. The hot-dip alloy coating contains ≥5% by weight and ≤30% by weight of Al, ≥2% by weight and ≤10% by weight of Mg, ≥0.05% by weight and ≤10% by weight of Fe, ≥0% by weight and ≤1% by weight of Si, the balance being Zn and other components diffused from the base steel.

[0058] 2. Evaluation of the microstructure and bending workability of the coating cross-section

[0059] Table 3 shows the evaluation results of bending workability in the coated steel according to the second experimental example of the present invention, based on the area fraction (%) of the MgZn2 phase in the cross-section of the hot-dip alloy coating and the ratio (%) of the area fraction of the Al single phase to the area fraction of the MgZn2 phase in the cross-section of the hot-dip alloy coating. In Table 3, after 3T bending, the bent processed part was observed 200 and 500 times using a field emission scanning electron microscope (FE-SEM), and the width of the bending crack was measured and averaged to evaluate the bending workability. "○" indicates that the average crack width in the bending evaluation is greater than 0 and less than or equal to 30 μm, and "X" indicates that the average crack width in the bending evaluation is greater than 30 μm.

[0060] [Table 3]

[0061]

[0062]

[0063] Referring to Table 3, it can be confirmed that, in the cases of samples 1, 2, 3 and 4, the area fraction of the MgZn2 phase in the cross section of the hot-dip alloy coating is in the range of 20% to 70%, and the ratio of the area fraction of the Al phase to the area fraction of the MgZn2 phase is in the range of 1% to 70%. Furthermore, after 3T bending, the average crack width of the bent processed part is 30 μm or less.

[0064] In contrast, it can be confirmed that, in the case of sample 5, the area fraction of MgZn2 phase in the cross section of the hot-dip alloy coating does not meet the range of 20% to 70%, and in the cases of samples 6, 7 and 8, the ratio of the area fraction of Al phase to the area fraction of MgZn2 phase in the cross section of the hot-dip alloy coating does not meet the range of 1% to 70%. In this case, the average crack width of the processed part after T-bending is greater than 30 μm.

[0065] [Table 4]

[0066]

[0067]

[0068] Table 4 shows the evaluation results of bending workability in the coated steel according to the second experimental example of the present invention, based on the area fraction (%) of the MgZn2 phase on the surface of the hot-dip alloy coating and the ratio of the average minor axis length (a) to the average major axis length (b). In Case 1, the MgZn2 involved is MgZn2 in the entire MgZn2 on the coating surface where the ratio of the average minor axis length (a) to the average major axis length (b) is greater than 0.5. In Case 2, the MgZn2 involved is MgZn2 in the entire MgZn2 on the coating surface where the ratio of the average minor axis length (a) to the average major axis length (b) is 0.5 or less. In Table 4, the bending workability of the coated steel sheet is evaluated as follows: the area fraction of MgZn2 in the coating cross section is 20% to 70%, and compared with the cross-sectional area of ​​the MgZn2 phase, the aluminum-containing phase present in or outside the MgZn2 phase is present in a proportion of 1% to 70%. After 3T bending, the bent, machined parts were observed 200 and 500 times using field emission scanning electron microscopy (FE-SEM). The width of the bending crack was then measured and averaged to evaluate the bending workability. "◎" indicates that the average crack width in the 3T bending evaluation is greater than 0 and less than or equal to 15 μm, and "○" indicates that the average crack width in the 3T bending evaluation is greater than 15 μm and less than or equal to 30 μm.

[0069] Referring to Table 4, it can be confirmed that samples A1, A2, B1, B2, C1, and C2 meet all of the following conditions: the area fraction of MgZn2 phase in the entire MgZn2 phase on the hot-dip alloy coating surface where the ratio of average minor axis length (a) to average major axis length (b) is greater than 0.5 is 30% or greater; the area fraction of MgZn2 phase in the entire MgZn2 phase on the hot-dip alloy coating surface where the ratio of average minor axis length (a) to average major axis length (b) is 0.5 or less is 70% or less; the ratio of average minor axis length (a) to average major axis length (b) in the entire MgZn2 phase on the hot-dip alloy coating surface is greater than or equal to 1 / 10 and less than or equal to 1 / 2; the average minor axis length (a) is 1 μm to 20 μm; and the average major axis length (b) is 2 μm to 200 μm, and in this case, the average crack width in the 3T bending evaluation is 15 μm or less.

[0070] In contrast, it can be confirmed that samples D1, D2, D3, D4, and D5 do not meet the following ranges: the area fraction of MgZn2 phase in the entire MgZn2 phase on the hot-dip alloy coating surface where the ratio of average minor axis length (a) to average major axis length (b) is greater than 0.5 is 30% or more; and the area fraction of MgZn2 phase in the entire MgZn2 phase on the hot-dip alloy coating surface where the ratio of average minor axis length (a) to average major axis length (b) is 0.5 or less is 70% or less, and in this case, the average crack width in the 3T bending evaluation is greater than 15 μm.

[0071] Furthermore, it can be confirmed that samples A3, B3, C3, and D5 do not meet the following range: the ratio of the average short axis length (a) to the average long axis length (b) in the entire MgZn2 phase on the surface of the hot-dip alloy coating is greater than or equal to 1 / 10 and less than or equal to 1 / 2, and in this case, the average crack width in the 3T bending evaluation is greater than 15 μm.

[0072] Furthermore, it can be confirmed that samples A4, B4, and C4 do not meet the range of average minor axis length (a) of 1 μm to 20 μm, although they meet the following range: the area fraction of MgZn2 phase in the entire MgZn2 phase on the hot-dip alloy coating surface is 70% or less, where the ratio of average minor axis length (a) to average major axis length (b) in the entire MgZn2 phase on the hot-dip alloy coating surface is greater than or equal to 1 / 10 and less than or equal to 1 / 2, and in this case, the average crack width in the 3T bending evaluation is greater than 15 μm.

[0073] Furthermore, it can be confirmed that samples A5, B5, and C5 do not meet the range of average major axis length (b) of 2 μm to 200 μm, although they meet the following range: the area fraction of MgZn2 phase in the entire MgZn2 phase on the hot-dip alloy coating surface is 70% or less, with the ratio of average minor axis length (a) to average major axis length (b) being 0.5 or less; and the ratio of average minor axis length (a) to average major axis length (b) in the entire MgZn2 phase on the hot-dip alloy coating surface being greater than or equal to 1 / 10 and less than or equal to 1 / 2. In this case, the average crack width in the 3T bending evaluation is greater than 15 μm.

[0074] Although embodiments of the invention have been described, various changes or modifications can be made by those skilled in the art. Such changes and modifications fall within the scope of the invention as long as they do not depart from its scope. Therefore, the scope of the invention should be determined by the claims.

Claims

1. A coated steel with excellent workability and corrosion resistance, comprising: Base steel; and A hot-dip alloy coating formed on the base steel, The hot-dip alloy coating comprises 5% to 30% Al, 2% to 10% Mg, with the balance being Zn and unavoidable impurities. Among them, in the entire MgZn2 phase on the surface of the hot-dip alloy coating, the area fraction of the MgZn2 phase with an average short axis length (a) to an average long axis length (b) greater than or equal to 1 / 10 and less than or equal to 1 / 2 is 30% or greater and 70% or less.

2. The coated steel according to claim 1, wherein, The average minor axis length (a) is 1 μm to 20 μm, and the average major axis length (b) is 2 μm to 200 μm.

3. The coated steel according to claim 1, wherein, On the surface of the hot-dip alloy coating, the area fraction of Al-Zn dendrites composed of Al and Zn phases is greater than 0% and 30% or less.

4. The coated steel according to claim 1, wherein, In the entire MgZn2 phase on the surface of the hot-dip alloy coating, the area fraction of the MgZn2 phase with an average minor axis length (a) to average major axis length (b) ratio greater than 0.5 and less than 1.0 is 30% or greater and 70% or less.

5. The coated steel according to claim 4, wherein, The diameter of an imaginary circle with the same area as the cross-sectional area of ​​a MgZn2 phase whose ratio of average minor axis length (a) to average major axis length (b) is greater than 0.5 and less than 1.0 is 1 μm to 50 μm.

6. The coated steel according to claim 1, wherein, The hot-dip alloy coating also contains 0.05% to 10% Fe and more than 0% and less than 1% Si.

Citation Information

Patent Citations

  • High yield ratio and high strength cold-rolled steel plate and high yield ratio and high strength galvanized steel plate excellent in weldability and ductility, and high yield ratio and high strength alloyed galvanized steel plate and its manufacturing method

    JP2005105367A

  • Zinc alloy-plated steel material having excellent corrosion resistance and surface quality, and method for producing same

    CN113195779A

  • Plated steel material

    CN113677820A

  • KR20210035722A