A hot-rolled strip steel and its preparation method

By optimizing the preparation process of hot-rolled strip steel, including preheating, staged heating, rolling and cooling, the problem of high energy consumption in the preparation of hot-rolled steel plates has been solved, and high-strength and high-toughness hot-rolled strip steel with a microstructure grain size of 12 to 14 and excellent mechanical properties has been achieved.

CN117548486BActive Publication Date: 2026-11-17SHOUGANG GROUP CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311298013.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-09
Publication Date
2026-11-17
Estimated Expiration
2043-10-09

AI Technical Summary

Technical Problem

The current hot-rolled steel plate manufacturing process consumes a lot of energy, especially in the billet heating stage, and conventional billets require long heating times, resulting in low production efficiency.

Method used

By preheating the billet and controlling the heating and soaking time in the furnace, setting the final rolling temperature and cooling rate in stages, the rolling and cooling process is optimized, promoting the full remelting of TiC precipitates and grain refinement, reducing large TiC particles, and improving the solid solubility of Ti in austenite grains.

Benefits of technology

It reduces the energy consumption in the preparation of hot-rolled steel plates, improves the production pace, and achieves high-strength and high-toughness hot-rolled strip steel with a microstructure grain size of 12 to 14, yield strength ≥650MPa, tensile strength ≥700MPa, elongation after fracture ≥20%, and low-temperature impact energy ≥100J at -20℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117548486B_ABST
    Figure CN117548486B_ABST
Patent Text Reader

Abstract

This application relates to the field of rolling processing technology, and more particularly to a hot-rolled strip steel and its preparation method. The method includes: preheating a billet at a set temperature; heating and homogenizing the preheated billet in a furnace for a first set time to achieve a first temperature; rolling the homogenized billet at a staged final rolling temperature to obtain a hot-rolled plate; cooling the hot-rolled plate in stages to achieve a second temperature, then coiling it at the second temperature, and finally cooling it after coiling to obtain hot-rolled strip steel; wherein the rate of post-coiling cooling is controlled. This application reduces the furnace exit temperature of high-Ti hot-rolled strip steel and shortens the total furnace time by using a preheated billet before entering the furnace. While ensuring the high strength and high toughness of the hot-rolled steel plate, it accelerates the hot rolling process, achieving energy saving, carbon reduction, and cost reduction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of rolling processing technology, and in particular to a hot-rolled strip steel and its preparation method. Background Technology

[0002] In recent years, with increasingly stringent environmental protection requirements and the demand for new energy development, lightweight design to promote energy conservation and emission reduction in automobiles has become a major trend. Under the premise of ensuring safety, developing high-strength and high-toughness automotive steel sheets has become an inevitable trend. With the maturation of high-strength and high-toughness hot-rolled steel sheet production technology, market competition has intensified. Currently, hot-rolled high-strength steel for automotive structures often improves strength and reduces costs by adding Ti through precipitation strengthening and grain refinement.

[0003] Currently, reducing energy consumption per ton of product during production has become a research hotspot for energy conservation and carbon reduction. For hot-rolled high-Ti steel plates (Ti content 0.040%-0.15%), the energy consumption of billet heating is a major source of energy consumption. Lowering the tapping temperature and shortening the total furnace time can not only reduce heating energy consumption but also improve production speed and reduce energy consumption per unit product. Therefore, continuous casting and rolling has become a major development direction for hot rolling technology. However, this technology is rarely applied to production lines where casting and hot rolling processes are separated, mainly because conventional billets require a long heating time. Therefore, how to apply lowering the tapping temperature and shortening the total furnace time to conventional billets to achieve process cost reduction and energy conservation and carbon reduction has become a research direction. Summary of the Invention

[0004] This application provides a hot-rolled strip steel and its preparation method to solve the technical problem of high energy consumption in the preparation of existing hot-rolled steel plates.

[0005] In a first aspect, this application provides a method for preparing hot-rolled strip steel, wherein the hot-rolled strip steel has a Ti content of 0.040%-0.15% by weight, and the method includes:

[0006] The billet is preheated under a set temperature condition;

[0007] Under the condition of a first set time, the preheated billet is heated in the furnace and homogenized in the furnace to bring the billet to a first temperature;

[0008] The hot-rolled plate is obtained by rolling the homogenized billet by setting the final rolling temperature in stages.

[0009] The hot-rolled plate is cooled in stages to bring it to a second temperature, and then coiled and cooled after coiling to obtain hot-rolled strip steel; wherein the rate of the post-coiling cooling is controlled.

[0010] Optionally, the step of heating the preheated billet in the furnace and homogenizing it in the furnace for a set time to bring the billet to a first temperature includes:

[0011] Under the condition of a second set time, the preheated billet is heated in the furnace;

[0012] Under a third predetermined time condition, the cast billet, after being heated in the furnace, is subjected to furnace homogenization to bring the cast billet to a first temperature; wherein,

[0013] The second set time is 60 min to 140 min, and the third set time is ≥40 min.

[0014] Optionally, the first set time is ≤180min.

[0015] Optionally, the first temperature is 1180℃~1220℃.

[0016] Optionally, the set temperature is ≥450℃.

[0017] Optionally, the step of rolling the homogenized billet to obtain a hot-rolled plate by setting the final rolling temperature in stages includes:

[0018] Under the condition of a first set final rolling temperature, the homogenized billet is subjected to rough rolling;

[0019] Under a second predetermined final rolling temperature, the rough-rolled billet is then finished-rolled to obtain a hot-rolled plate; wherein,

[0020] The first set final rolling temperature is ≤1040℃, and the second set final rolling temperature is 800℃~850℃.

[0021] Optionally, the hot-rolled plate is subjected to staged cooling, followed by coiling and post-coiling cooling to obtain hot-rolled strip steel; wherein controlling the rate of post-coiling cooling includes:

[0022] Under a first set cooling rate, the hot-rolled plate is subjected to ultra-fast cooling;

[0023] Under the second set cooling rate, the hot-rolled plate after ultra-fast cooling is subjected to laminar flow front-end cooling;

[0024] Under a third set cooling rate, the hot-rolled plate after laminar flow front-stage cooling is subjected to laminar flow back-stage cooling to bring the hot-rolled plate to a second temperature. Then, it is coiled and cooled after coiling under the second temperature to obtain hot-rolled strip steel. The rate of the cooling after coiling is controlled.

[0025] The first set cooling rate is 45℃ / s to 80℃ / s, the second set cooling rate is 3℃ / s to 10℃ / s, and the third set cooling rate is 1℃ / s to 3℃ / s.

[0026] Optionally, the second temperature is 590℃~630℃.

[0027] Optionally, the post-roll cooling rate is ≤25℃ / h.

[0028] Secondly, this application provides a hot-rolled strip steel, which is obtained by the method described in any embodiment of the first aspect; the microstructure of the hot-rolled strip steel includes:

[0029] Fine-grained bulk ferrite + acicular ferrite + nanoscale TiC precipitates;

[0030] The grain size level of the microstructure is grade 12 to 14.

[0031] The technical solutions provided in this application have the following advantages compared with the prior art:

[0032] The hot-rolled strip steel preparation method provided in this application improves the furnace entry temperature through preheating to reduce the total furnace time and heating energy consumption; it promotes the full remelting of TiC and other precipitates by controlling the furnace heating and holding time, reducing and eliminating large TiC particles without strengthening effect, and improving the actual solid solubility of Ti in the original austenite grains; it controls the furnace exit temperature of the continuously cast slab to reduce the growth of the original austenite grain size; it controls the final rolling temperature in stages to obtain uniform and fine microstructure grains; it promotes the precipitation of TiC in the ferrite region through staged cooling, improving the precipitation strengthening effect, while refining the ferrite grains and increasing the contribution of grain refinement to strength and toughness; and it controls the coiling temperature and post-coiling cooling rate to increase the quantity and size of TiC precipitates. In summary, this application solves the technical problem of high energy consumption in the preparation of existing hot-rolled steel plates, and accelerates the hot rolling process while ensuring the high strength and high toughness of the hot-rolled steel plates, achieving energy saving, carbon reduction, and cost reduction. The grain size of the microstructure of this steel is grade 12 to 14. The yield strength of this hot-rolled steel plate is ≥650MPa, the tensile strength is ≥700MPa, the elongation after fracture is ≥20%, and the impact energy at -20℃ is ≥100J. Attached Figure Description

[0033] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.

[0034] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0035] Figure 1 A schematic flowchart illustrating a method for preparing hot-rolled strip steel provided in this application embodiment;

[0036] Figure 2-5 A microstructure diagram of a hot-rolled strip steel provided in an embodiment of this application. Detailed Implementation

[0037] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0038] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.

[0039] In this application, unless otherwise stated, directional terms such as "upper" and "lower" specifically refer to the drawing directions in the accompanying drawings. Furthermore, in the description of this application, terms such as "comprising" and "including" mean "including but not limited to." In this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this document, "and / or" describes the relationship between related objects, indicating that three relationships can exist; for example, A and / or B can represent: A alone, A and B simultaneously, or B alone. A and B can be singular or plural. In this document, "at least one" means one or more, and "more than one" means two or more. "At least one," "at least one of the following," or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c" or "at least one of a, b, and c" can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be a single or multiple.

[0040] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0041] Firstly, this application provides a method for preparing hot-rolled strip steel; please refer to [link to relevant documentation]. Figure 1 The hot-rolled strip steel has a Ti content of 0.040%-0.15% by weight, and the method includes:

[0042] S1. Preheat the billet at the set temperature.

[0043] S2. Under the condition of a first set time, the preheated billet is heated in the furnace and homogenized in the furnace to bring the billet to a first temperature;

[0044] S3. The homogenized billet is rolled by setting the final rolling temperature in stages to obtain a hot-rolled plate;

[0045] S4. The hot-rolled plate is cooled in stages to give it a second temperature, and then coiled and cooled after coiling at the second temperature to obtain hot-rolled strip steel; wherein the rate of the cooling after coiling is controlled.

[0046] The hot-rolled strip steel preparation method provided in this application improves the furnace entry temperature through preheating to reduce the total furnace time and heating energy consumption; it promotes the full remelting of precipitates such as TiC by controlling the heating and holding times in the furnace, reducing and eliminating large TiC particles without strengthening effect, and improving the actual solid solubility of Ti in the original austenite grains; it controls the exit temperature of the continuously cast slab to reduce the growth of the original austenite grain size; it controls the final rolling temperature in stages to obtain uniform and fine microstructure grains; it promotes the precipitation of TiC in the ferrite region through staged cooling to improve precipitation strengthening effect, while refining the ferrite grains and increasing the contribution of grain refinement to strength and toughness; and it controls the coiling temperature and post-coiling cooling rate to increase the quantity and size of TiC precipitates.

[0047] In some embodiments, the step of heating and homogenizing the preheated billet in a furnace for a set time to bring the billet to a first temperature includes:

[0048] Under the condition of a second set time, the preheated billet is heated in the furnace;

[0049] Under a third predetermined time condition, the cast billet, after being heated in the furnace, is subjected to furnace homogenization to bring the cast billet to a first temperature; wherein,

[0050] The second set time is 60min to 140min, and the third set time is ≥40min.

[0051] "Second set time" refers to the furnace heating time, "Third set time" refers to the furnace soaking time, and "First temperature" refers to the furnace exit temperature. Controlling the furnace heating time to 60-140 minutes and the furnace soaking time to ≥40 minutes has the following positive effects: promoting the full remelting of precipitates such as TiC, reducing and eliminating large TiC particles without strengthening effect, and improving the actual solid solubility of Ti in the original austenite grains. If the furnace heating time is too long, it will increase the total heating time and heating energy consumption to some extent; if the furnace heating time is too short, it will lead to poor temperature uniformity of the cast billet and reduce the uniformity of the original austenite grains to some extent. Specifically, the furnace heating time can be 60 min, 80 min, 100 min, 120 min, 140 min, etc. If the furnace soaking time is too short, it will reduce the remelting of precipitates such as TiC to some extent. Specifically, the furnace soaking time can be 40 min, 50 min, 60 min, etc.

[0052] In some implementations, the first set time is ≤180 min.

[0053] "First set time" refers to the total furnace time. Controlling the total furnace time to ≤180 min has the positive effects of reducing heating energy consumption while ensuring the remelting amount of precipitated phases such as TiC. If this time is too long, it will increase energy consumption to some extent, and the original austenite grains will coarsen. Specifically, the total furnace time can be 180 min, 170 min, 175 min, etc.

[0054] In some embodiments, the first temperature is 1180°C to 1220°C.

[0055] "First temperature" refers to the tapping temperature. Controlling the tapping temperature to 1180℃~1220℃ has the following positive effects: Within the range of 950℃~1300℃, the initial austenite grain size in the cast slab increases exponentially with increasing heating temperature and parabolically with holding time. Therefore, reducing the tapping temperature of continuously cast slabs to 1180℃~1220℃ reduces the growth of the initial austenite grain size. If this temperature is too high, it will increase energy consumption to some extent, coarsen the initial austenite grains, and ultimately result in insufficient low-temperature toughness of the hot-rolled strip. If this temperature is too low, it will result in insufficient remelting of precipitates such as TiC, insufficient number of nano-sized TiC precipitates formed by slow cooling, and insufficient strengthening effect. Specifically, this tapping temperature can be 1180℃, 1190℃, 1200℃, 1210℃, 1220℃, etc.

[0056] In some implementations, the set temperature is ≥450°C.

[0057] "Set temperature" refers to the preheating temperature. Controlling the preheating temperature to ≥450℃ has the positive effects of reducing total furnace time and lowering heating energy consumption. If this temperature is too low, it will increase the furnace's heating energy consumption to some extent. Specifically, this preheating temperature can be 450℃, 500℃, 550℃, etc.

[0058] In some embodiments, the step of rolling the homogenized billet to obtain a hot-rolled plate by setting the final rolling temperature in stages includes:

[0059] Under the condition of a first set final rolling temperature, the homogenized billet is subjected to rough rolling;

[0060] Under the condition of the second set final rolling temperature, the rough-rolled billet is finished rolled to obtain a hot-rolled plate; wherein, the first set final rolling temperature is ≤1040℃, and the second set final rolling temperature is 800℃~850℃.

[0061] The aforementioned roughing rolling is a 6-pass continuous rolling process, performed above the austenite recrystallization temperature, with a roughing reduction rate greater than 75%. "First set final rolling temperature" represents the final rolling temperature of the roughing roll, and "Second set final rolling temperature" represents the final rolling temperature of the finishing roll. Controlling the final rolling temperature of the roughing roll to ≤1040℃ has the following positive effects: The roughing rolling process is controlled above the austenite recrystallization temperature, ensuring that the austenite undergoes repeated deformation and recrystallization to obtain uniform and fine austenite grains, while avoiding excessively high final rolling temperatures that could cause recrystallized grain growth. If the temperature is too high, the original austenite grains may easily revert to growth, resulting in coarsening; if the temperature is too low, the rolling force may increase to some extent, exceeding the mill's capacity. Specifically, the final rolling temperature of this roughing roll can be 1040℃, 1030℃, 1035℃, 1020℃, etc.

[0062] The aforementioned finishing rolling is a 6-pass continuous rolling process, rolled within the non-recrystallization temperature range of austenite, with a finishing reduction rate greater than 75%. After finishing rolling, the finished steel plate thickness is 6–12 mm. The positive effects of controlling the final rolling temperature to 800℃–850℃ are as follows: The finishing rolling temperature setting is coordinated with the reduction rate. On the one hand, the high reduction rate in the first three passes promotes the deformation of recrystallized austenite grains, forming large deformation bands within the grains. On the other hand, the higher rolling temperature inhibits the precipitation of TiC particles within the deformed austenite grains. The reduced reduction rate in the remaining rolling passes also helps reduce TiC particle precipitation. Simultaneously, the lower rolling temperature inhibits the recovery of deformed austenite grains, ultimately ensuring the required amount of TiC precipitation and ferrite grain refinement in the ferrite region. If the temperature is too high, it will, to some extent, promote the recovery of deformed austenite grains and the precipitation of TiC particles; if the temperature is too low, it will, to some extent, cause a phase transformation in the deformed austenite, producing coarse proeutectoid ferrite. Specifically, the finishing rolling temperature can be 800℃, 810℃, 820℃, 830℃, 840℃, 850℃, etc.

[0063] In some embodiments, the hot-rolled plate is subjected to staged cooling, followed by coiling and post-coiling cooling to obtain hot-rolled strip steel; wherein controlling the rate of post-coiling cooling includes:

[0064] Under a first set cooling rate, the hot-rolled plate is subjected to ultra-fast cooling;

[0065] Under the second set cooling rate, the hot-rolled plate after ultra-fast cooling is subjected to laminar flow front-end cooling;

[0066] Under a third set cooling rate, the hot-rolled plate after laminar flow front-stage cooling is subjected to laminar flow back-stage cooling to bring the hot-rolled plate to a second temperature. Then, it is coiled and cooled after coiling under the second temperature to obtain hot-rolled strip steel. The rate of the cooling after coiling is controlled.

[0067] The first set cooling rate is 45℃ / s to 80℃ / s, the second set cooling rate is 3℃ / s to 10℃ / s, and the third set cooling rate is 1℃ / s to 3℃ / s.

[0068] The role of ultra-fast cooling: It rapidly cools the austenitic structure to the ferrite structure, reduces the residence time in the two-phase region, promotes the precipitation of TiC in the ferrite region, enhances precipitation strengthening, and refines the ferrite grains, thereby improving the effect of grain refinement on strength and toughness. However, the temperature after rapid cooling cannot be too low, otherwise it is easy to form bainite structure which is detrimental to toughness. The role of laminar flow front-stage cooling: It increases the grain size of surface ferrite, reduces the grain size difference between the core and the surface, and avoids delamination cracking. The role of laminar flow back-stage cooling: It increases the high-temperature residence time and promotes the precipitation of nano-sized TiC particles.

[0069] "First set cooling rate" indicates the ultra-fast cooling rate, "Second set cooling rate" indicates the cooling rate of the laminar flow front section, and "Third set cooling rate" indicates the cooling rate of the laminar flow rear section.

[0070] The positive effects of controlling the ultrafast cooling rate to 45℃ / s to 80℃ / s include: grain refinement and reduction of micron-sized TiC particles precipitated in the austenite and austenite-ferrite two-phase regions. If the cooling rate is too high, it can increase the grain size difference between the surface and the core, leading to delamination; if the cooling rate is too low, it can increase the precipitation of micron-sized TiC particles in the austenite and austenite-ferrite two-phase regions, reducing the amount of nano-sized precipitation and resulting in insufficient strength and toughness. Cooling to 640℃ to 680℃, specifically at cooling rates of 45℃ / s, 50℃ / s, 55℃ / s, 60℃ / s, 65℃ / s, 70℃ / s, 75℃ / s, and 80℃ / s, is also possible.

[0071] The positive effects of controlling the cooling rate of the laminar flow front section to be 3℃ / s to 10℃ / s are as follows: If the cooling rate is too high, it will inhibit the growth of surface ferrite grains to a certain extent, increase the grain size difference between the surface and the core, and easily lead to delamination; if the cooling rate is too low, it will cause the surface grains to grow rapidly, reduce the grain refinement effect, and result in insufficient strength. Cooling to 620℃ to 650℃, specifically, the cooling rate can be 3℃ / s, 5℃ / s, 7℃ / s, 9℃ / s, 10℃ / s, etc.

[0072] The positive effects of controlling the cooling rate of the laminar flow tail section to 1℃ / s to 3℃ / s include: increasing the high-temperature residence time and promoting the precipitation of nano-sized TiC particles. If the cooling rate is too high, it will reduce the number of nano-sized TiC particles precipitated at high temperatures, resulting in insufficient strength; if the cooling rate is too low, corresponding heat preservation equipment will be required, increasing investment and energy consumption. Cooling to the winding temperature, specifically, this cooling rate can be 1℃ / s, 2℃ / s, 3℃ / s, etc.

[0073] In some embodiments, the second temperature is 590°C to 630°C.

[0074] The "second temperature" refers to the temperature after cooling in the laminar flow stage, which is also the winding temperature. The positive effects of controlling the winding temperature at 590℃~630℃ include: controlling the degree of grain refinement and the quantity and size of TiC precipitates. If this temperature is too high, it can lead to grain growth, resulting in excessively large TiC precipitates, weakening the strengthening effect, and negatively impacting toughness. If the temperature is too low, TiC will not precipitate easily, resulting in too few precipitates and too small precipitates, thus the strengthening effect will not be significant. Specifically, this winding temperature can be 590℃, 600℃, 610℃, 620℃, 630℃, etc.

[0075] In some embodiments, the post-roll cooling rate is ≤25°C / h.

[0076] The post-coiling cooling method is slow cooling, and controlling the post-coiling cooling rate to ≤25℃ / h has the positive effect of increasing the quantity and size of TiC precipitates. A cooling rate that is too high is detrimental to TiC precipitation. This cooling rate can be 25℃ / h, 24℃ / h, 23℃ / h, etc. The starting temperature for this slow cooling is 400℃~600℃.

[0077] Secondly, this application provides a hot-rolled strip steel, which is obtained by the method described in any embodiment of the first aspect; the microstructure of the hot-rolled strip steel includes:

[0078] Fine-grained bulk ferrite + acicular ferrite + nanoscale TiC precipitates;

[0079] The grain size level of the microstructure is grade 12 to 14.

[0080] The role of fine-grained blocky ferrite: fine grain strengthening + delaying the propagation of microcracks, thus achieving simultaneous improvement in strength and toughness.

[0081] The role of acicular ferrite is to refine grains and increase the number of grain boundaries, thereby improving strength and toughness.

[0082] The role of nanoscale TiC precipitates: to hinder dislocation movement and increase strength.

[0083] The positive effect of the steel's microstructure having a grain size level of 12 to 14 is that it achieves a uniform grain distribution along the thickness direction while ensuring that the required strength and toughness are met. The microstructure diagram can be found here. Figures 2-5 .

[0084] In the embodiments of this application, the above-mentioned hot-rolled strip steel has a yield strength ≥650MPa, tensile strength ≥700MPa, elongation after fracture ≥20%, and low-temperature impact energy ≥100J at -20℃.

[0085] The steel plate obtained by the above-described hot-rolled strip preparation method has the aforementioned excellent mechanical properties.

[0086] The hot-rolled strip steel is realized based on the above-described method for preparing hot-rolled strip steel. The specific steps of the method for preparing hot-rolled strip steel can be referred to the above embodiments. Since the hot-rolled strip steel adopts some or all of the technical solutions of the above embodiments, it has at least all the beneficial effects brought about by the technical solutions of the above embodiments, which will not be elaborated here.

[0087] The present application is further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the application. Experimental methods in the following embodiments that do not specify specific conditions are generally determined according to national standards. If there is no corresponding national standard, then general international standards, conventional conditions, or conditions recommended by the manufacturer are followed.

[0088] Table 1. Manufacturing process parameters for hot-rolled strip steel

[0089]

[0090] Table 2. Ti content and grain size grades of microstructure in hot-rolled strip steel.

[0091]

[0092] Table 3 Mechanical properties of hot-rolled strip steel

[0093]

[0094] The aforementioned 180° bending test: A 35mm wide sample was tested in a bending test with a mandrel diameter equal to the sample thickness. Based on the preparation process parameters of hot-rolled strip steel in Table 1, Tables 2 and 3 are obtained. The preparation method of hot-rolled strip steel according to the embodiments of this application improves the grain size of the microstructure and ensures the mechanical properties of the hot-rolled strip steel. In contrast, the comparative example did not use the method of the embodiments of this application, and the parameters were not within the set range. The grain size level of this microstructure was lower than that of the examples, resulting in poorer mechanical properties, especially toughness.

[0095] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A method of producing a hot-rolled steel strip, characterized in that, The hot-rolled strip steel has a Ti content of 0.040%-0.15% by weight, and the method includes: Preheat the billet at a set temperature ≥450℃; Under the condition that the first set time is ≤170min, the preheated billet is heated in the furnace for 60min~140min and homogenized in the furnace for ≥40min to bring the billet to a first temperature; The hot-rolled plate is obtained by rolling the homogenized billet by setting the final rolling temperature in stages, including: rough rolling the homogenized billet under the condition of a first set final rolling temperature ≤1040℃, with a rough rolling reduction rate greater than 75%; and finish rolling the rough rolled billet under the condition of a second set final rolling temperature of 800℃~850℃, with a finish rolling reduction rate greater than 75%, to obtain the hot-rolled plate. The hot-rolled plate is cooled in stages to bring it to a second temperature of 590℃~630℃. It is then coiled and cooled after coiling at the second temperature to obtain hot-rolled strip steel. The rate of post-coiling cooling is controlled to be ≤25℃ / h. The staged cooling includes: ultra-rapid cooling of the hot-rolled plate at a cooling rate of 45℃ / s~80℃ / s to 640℃~680℃; laminar flow pre-cooling of the ultra-rapidly cooled hot-rolled plate at a cooling rate of 3℃ / s~10℃ / s to 620℃~650℃; and laminar flow post-cooling of the hot-rolled plate after laminar flow pre-cooling at a cooling rate of 1℃ / s~3℃ / s.

2. The method of claim 1, wherein, The first temperature is 1180℃~1220℃.

3. A hot-rolled steel strip, characterized in that, The hot-rolled strip steel is as described in any one of claims 1-2. The method yielded the hot-rolled strip steel; the microstructure of the hot-rolled strip steel includes: Fine-grained bulk ferrite + acicular ferrite + nanoscale TiC precipitates; The grain size level of the microstructure is grade 12 to 14.

Citation Information

Patent Citations

  • Manufacturing method of X70 pipeline steel hot rolled steel roll

    CN102653836A

  • Hot-rolled coiled plate and manufacturing method thereof

    CN105256240A