Low shrinkage geopolymer mortar, preparation method and application thereof, low shrinkage geopolymer curing mortar

By adding red brick sand to geopolymer mortar, its water absorption and water release properties are used to slow down the water loss rate during the dry shrinkage process, solve the high dry shrinkage problem of geopolymer mortar, and improve the fluidity and construction performance. , realizing the resource utilization of waste red bricks, reducing cement demand and carbon emissions, and solving the application challenges of geopolymer materials in engineering.

CN117550841BActive Publication Date: 2024-10-11SHENZHEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311525911.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-15
Publication Date
2024-10-11
Estimated Expiration
2043-11-15

AI Technical Summary

Technical Problem

The mortar drying shrinkage of geopolymer cementitious materials is high, which hinders its wide application. Moreover, when fly ash and slag are used alone, there are problems such as short setting time and poor workability.

Method used

The preparation method of low-shrinkage geopolymer mortar is adopted, including raw materials such as fly ash, slag, sand and red brick sand. Through an alkaline activator reaction, porous red brick sand is added to slow down the water loss rate during dry shrinkage. , improve the pore structure, and use the water absorption and water release properties of red brick sand for internal curing.

Benefits of technology

Significantly reduces the dry shrinkage performance of geopolymer mortar, making the dry shrinkage level close to that of traditional OPC mortar. It also improves fluidity and construction performance, realizes the resource utilization of industrial solid waste and construction waste, and reduces the use of cement. demand, alleviating the shortage of cement resources and high carbon emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117550841B_ABST
    Figure CN117550841B_ABST
Patent Text Reader

Abstract

The present invention provides a low shrinkage geopolymer mortar and a preparation method and application thereof, and a low shrinkage geopolymer curing mortar, and relates to the technical field of cementitious materials. The present invention adds red brick sand to replace fine aggregate, and utilizes the internal curing function of red brick sand to absorb and release water, slows down the rate of decrease of the relative humidity inside the geopolymer mortar, improves the pore structure of the mortar, and effectively reduces the shrinkage of the mortar, so that the shrinkage level of the mortar is reduced to the same level as that of traditional silicate mortar, and the compressive strength does not decrease significantly, solving the problem of high shrinkage of geopolymer materials in engineering use. In addition, the addition of red brick sand can also improve the fluidity of the mortar, improve the construction performance of the geopolymer mortar, realize the resource utilization of discarded red bricks, and have both environmental protection and economic benefits, which is of great significance for promoting the application of geopolymer materials in engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cementitious materials, and in particular relates to a low-shrinkage geopolymer mortar and a preparation method and application thereof, and a low-shrinkage geopolymer curing mortar. Background Art

[0002] Geopolymer refers to a three-dimensional network polymer gel of silicon-oxygen tetrahedron and aluminum-oxygen tetrahedron prepared by reacting with alkaline activators using natural minerals or solid waste and artificial silicon-aluminum compounds as raw materials. Compared with traditional ordinary Portland cement (OPC), geopolymer cementitious materials have many excellent properties, such as fast setting and high strength, low hydration heat, good impermeability and frost resistance. It is a low-cost, high-performance environmentally friendly cementitious material. Fly ash and slag are two commonly used geopolymer cementitious materials. When slag is used alone to prepare mortar, there are problems such as too short setting time and poor workability and inconvenient construction. Fly ash is difficult to harden at room temperature and requires high-temperature curing. If the two are combined, their respective defects will be effectively improved, and fly ash / slag composite geopolymer cementitious materials will have more application prospects. However, the drying shrinkage rate of mortar prepared by geopolymer cementitious materials is 1.6 to 3 times that of OPC mortar, which hinders the widespread application of geopolymer cementitious materials.

[0003] Chinese patent CN112479674A discloses an alkali-activated recycled red brick powder and slag-based recycled concrete, which is prepared from recycled red brick powder, slag, fly ash, natural river sand, natural coarse aggregate, recycled coarse aggregate, sodium hydroxide solid, water glass, sodium carbonate and water. The fineness of the recycled red brick powder reaches RFP-II grade and above, and the water-binder ratio (the mass of water is the sum of the mass of recycled red brick powder, slag and fly ash) is 0.40-0.52, wherein the water includes the water contained in the water glass and the added water. However, the above alkali-activated material has poor shrinkage performance. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a low shrinkage geopolymer mortar and a preparation method and application thereof, and a low shrinkage geopolymer curing mortar. The low shrinkage geopolymer mortar and the low shrinkage geopolymer curing mortar provided by the present invention have excellent shrinkage performance.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a low shrinkage geopolymer mortar, which comprises the following raw materials, measured by weight: 1 part of a cementitious material, 2 to 2.5 parts of a fine aggregate, and 0.4 to 0.5 parts of an alkaline activator;

[0007] The cementitious material comprises fly ash and slag, and the mass fraction of the fly ash in the cementitious material is 20-70%;

[0008] The fine aggregate comprises sand and red brick sand, the mass fraction of the red brick sand in the fine aggregate is 15-25%, the particle size of the red brick sand is ≤8mm, and the particle size of the sand is ≤4.75mm.

[0009] Preferably, the particle size of the red brick sand is 0.2 to 8 mm;

[0010] The red brick sand includes dry red brick sand or water-soaked red brick sand; the water content of the water-soaked red brick sand is 18-22wt%.

[0011] Preferably, the sand is continuously graded sand.

[0012] Preferably, the fly ash is low-calcium fly ash, and the particle size of the fly ash is 0.3 to 300 μm;

[0013] The slag is blast furnace slag, and the particle size of the slag is 0.3-350 μm.

[0014] Preferably, the alkaline activator comprises sodium hydroxide, water glass and water; the modulus of the alkaline activator is 1 to 1.5, and the alkali equivalent is 0.4 to 0.8.

[0015] Preferably, the density of the low shrinkage geopolymer mortar is 1800-2200 kg / m 3 .

[0016] The present invention provides a method for preparing the low shrinkage geopolymer mortar described in the above technical solution, comprising the following steps: mixing fly ash, slag, sand, red brick sand and an alkaline activator to obtain the low shrinkage geopolymer mortar.

[0017] Preferably, after the alkaline activator is prepared, it is allowed to stand for 12 to 48 hours before use.

[0018] The present invention provides a low shrinkage geopolymer curing mortar, which is obtained by curing the low shrinkage geopolymer mortar after casting; the low shrinkage geopolymer mortar is the low shrinkage geopolymer mortar described in the above technical scheme or the low shrinkage geopolymer mortar prepared by the preparation method described in the above technical scheme.

[0019] The present invention provides the use of the low shrinkage geopolymer mortar described in the above technical solution, the low shrinkage geopolymer mortar prepared by the preparation method described in the above technical solution, or the low shrinkage geopolymer curing mortar described in the above technical solution in building materials.

[0020] The polymerization reaction of geopolymer mortar consumes a low amount of free water. During the drying process, a large amount of free water evaporates with the external drying, and the water is removed from the surface of the gel pores and the volume shrinks. The red brick used in the present invention is a porous material with excellent water absorption and water storage properties. It can keep the water slowly dissipated under high relative humidity and release the water in time when the relative humidity decreases. The present invention introduces red brick sand into geopolymer mortar to play the role of internal curing, slow down the rate of decrease of relative humidity inside the geopolymer, improve the pore structure of the geopolymer mortar, and significantly reduce the shrinkage of the geopolymer mortar, which helps to solve the high shrinkage problem of geopolymer materials in engineering use, and has an important boosting significance for the shrinkage of geopolymer mortar in engineering applications. The present invention uses industrial solid waste fly ash and slag to replace cement to prepare green oligomer mortar, which can reduce the demand for cement materials, alleviate the shortage of cement resources, and reduce the high carbon emissions generated in the cement production process. Using discarded red bricks to slow down the shrinkage of geopolymer mortar can simultaneously realize the resource utilization of industrial solid waste and construction waste. The raw materials are widely available and are economical and environmentally friendly, which has significant environmental and economic benefits to society.

[0021] The present invention can improve the fluidity of the mortar by adding water-soaked red brick sand. This is because during the stirring process of the water-soaked red brick sand, part of the water stored in the red brick sand will be separated from the red brick sand and enter the mortar under the centrifugal force generated by the rotation of the mixer, so that the actual mixing water amount of the slurry is increased and the fluidity is improved. Therefore, adding red brick sand can significantly improve the fluidity of the geopolymer mortar and improve the construction performance of the geopolymer mortar. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The shrinkage performance test results of the geopolymer mortar prepared in Examples 1 to 4 and Comparative Example 1;

[0023] Figure 2 This is the water absorption result diagram of red brick sand with different particle sizes;

[0024] Figure 3 This is the moisture-sensitive water release rate result diagram of red brick sand with different particle sizes. DETAILED DESCRIPTION

[0025] The present invention provides a low shrinkage geopolymer mortar, which comprises the following raw materials, measured by weight: 1 part of a cementitious material, 2 to 2.5 parts of a fine aggregate, and 0.4 to 0.5 parts of an alkaline activator;

[0026] The cementitious material comprises fly ash and slag, and the mass fraction of the fly ash in the cementitious material is 20-70%;

[0027] The fine aggregate comprises sand and red brick sand, the mass fraction of the red brick sand in the fine aggregate is 15-25%, the particle size of the red brick sand is ≤8mm, and the particle size of the sand is ≤4.75mm.

[0028] In the present invention, unless otherwise specified, the materials and equipment used are commercially available products in the art.

[0029] In terms of mass fraction, the raw materials for preparing the low shrinkage geopolymer mortar provided by the present invention include 1 part of cementitious material. In the present invention, the cementitious material includes fly ash and slag, and the mass fraction of fly ash in the cementitious material is 20-70%, preferably 50-70%, and more preferably 60-70%. In the present invention, the fly ash is preferably low-calcium fly ash, and more preferably first-grade low-calcium fly ash; the particle size of the fly ash is preferably 0.3-300 μm; in the present invention, the slag is preferably blast furnace slag, and more preferably first-grade ground granulated blast furnace slag; the particle size of the slag is preferably 0.3-350 μm.

[0030] In terms of mass fraction, the raw materials for preparing the low shrinkage geopolymer mortar provided by the present invention include 2 to 2.5 parts of fine aggregate, preferably 2 to 2.3 parts, and more preferably 2 to 2.2 parts. In the present invention, the fine aggregate includes sand and red brick sand, and the mass fraction of red brick sand (i.e. dry red brick sand or water-soaked red brick sand) in the fine aggregate is 15 to 25%, and more preferably 21 to 25%. In the present invention, the particle size of the red brick sand is ≤8 mm, preferably 0.2 to 8 mm, and more preferably 0.2 to 5 mm or 5 to 8 mm. In the present invention, the red brick sand includes dry red brick sand or water-soaked red brick sand; the moisture content of the water-soaked red brick sand is preferably 18 to 22 wt%, more preferably 19 to 21 wt%, and further preferably 20 wt%. In the present invention, the dry red brick sand is preferably obtained by crushing red bricks.

[0031] In the present invention, the preparation method of the water-soaked red brick sand preferably includes the following steps: soaking the dry red brick sand in water, taking it out and wiping it to a saturated surface dry state, to obtain the water-soaked red brick sand. In the present invention, the temperature of the water immersion is preferably 20-25°C, and the time of the water immersion is preferably 48-72h, more preferably 60-72h. The purpose of the present invention of soaking the dry red brick sand in water is to saturate the red brick sand with water, so that the water stored in the red brick sand in advance can be released when the mortar is dried later, slowing down the rate of decrease of the relative humidity inside the material, thereby further reducing the shrinkage of the material. In the present invention, the particle size of the sand is ≤4.75mm, and the sand is preferably continuously graded sand; the sand preferably includes river sand and / or sea sand.

[0032] The polymerization reaction of geopolymer mortar consumes a low amount of free water. During the drying process, a large amount of free water evaporates as the external environment dries, and the water is removed from the surface of the gel pores, causing the volume to shrink. The purpose of internal curing is to introduce additional water into the mortar through internal curing materials. As the hydration reaction proceeds, the water inside the pores is consumed, and the internal curing materials will release additional water to the matrix to compensate for the decrease in internal relative humidity, reduce capillary force and thus slow down shrinkage. When preparing geopolymer mortar, the present invention crushes the discarded red bricks into granules (red brick sand) to replace part of the fine aggregate as a curing material, and adds them to the geopolymer mortar. In a dry environment, when the relative humidity inside the matrix decreases due to water loss, the red brick sand can release water to fill the pores to play an internal curing role, slow down the rate of decrease in relative humidity inside the mortar, improve the pore structure of the mortar, reduce the capillary pressure and thus reduce the shrinkage of the mortar. The introduction of red brick sand can effectively reduce the shrinkage of geopolymer mortar, making the shrinkage of geopolymer mortar at the same level as traditional OPC mortar. At the same time, it improves the fluidity of geopolymer mortar and realizes the resource utilization of waste red bricks. It has both environmental protection and economic benefits, and is of great significance to the engineering application of geopolymer materials.

[0033] The raw materials for preparing the low shrinkage geopolymer mortar provided by the present invention include 0.4 to 0.5 parts of alkaline activator, and more preferably 0.44 to 0.5 parts, by weight. In the present invention, the alkaline activator preferably includes sodium hydroxide, water glass and water; the modulus of the alkaline activator is preferably 1 to 1.5, more preferably 1.1 to 1.4, and further preferably 1.2 to 1.3; the alkali equivalent of the alkaline activator is preferably 0.4 to 0.8, more preferably 0.5 to 0.7, and further preferably 0.6.

[0034] In the present invention, the density of the low shrinkage geopolymer mortar is preferably 1800-2200 kg / m 3 , more preferably 1850 to 2100 kg / m 3 , more preferably 1900~2000kg / m 3 .

[0035] The present invention provides a method for preparing the low shrinkage geopolymer mortar described in the above technical solution, comprising the following steps: mixing fly ash, slag, sand, red brick sand and an alkaline activator to obtain the low shrinkage geopolymer mortar.

[0036] In the present invention, after the alkaline activator is prepared, it is preferably left to stand for 24 to 48 hours (more preferably 24 to 30 hours) before use. The alkaline activator is left to stand for 24 to 48 hours before use, so that water, water glass and sodium hydroxide particles can be fully mixed. In the present invention, the preparation method of the alkaline activator preferably includes the following steps: completely dissolving the sodium hydroxide in water, and stirring the water glass and the sodium hydroxide solution evenly.

[0037] In the present invention, the mixing is preferably: first mixing fly ash, slag, sand and red brick sand to obtain a mixture; second mixing the mixture with an alkaline activator; the time of the first mixing is preferably 2 to 5 minutes, more preferably 2 to 3 minutes; the first mixing and the second mixing are preferably stirred and mixed; the present invention has no special restrictions on the speed of the first mixing and the speed and time of the second mixing, as long as the raw materials can be mixed uniformly. In a specific embodiment of the present invention, the mixing is performed according to the specification JC / T 603-2004.

[0038] The present invention provides a low shrinkage geopolymer curing mortar, which is obtained by curing the low shrinkage geopolymer mortar after casting; the low shrinkage geopolymer mortar is the low shrinkage geopolymer mortar described in the above technical solution or the low shrinkage geopolymer mortar prepared by the preparation method described in the above technical solution. The present invention has no special limitation on the mold used for the casting and molding, which can be determined according to actual needs. In a specific embodiment of the present invention, a 40mm×40mm×160mm stainless steel triple mold is used. In the present invention, the casting and molding is preferably to load the low shrinkage geopolymer mortar into the mold in layers, and each layer of low shrinkage geopolymer mortar is preferably firstly compacted with a tamping rod, and then the next layer of low shrinkage geopolymer mortar is loaded; after the last layer of low shrinkage geopolymer mortar is loaded, the excess low shrinkage geopolymer mortar is scraped off and placed on a vibrating table for vibrating, and the surface is scraped flat after the vibration is completed; the vibration time is preferably 1 to 3 minutes, more preferably 1 to 2 minutes. In the present invention, the curing temperature is preferably 18-22°C, more preferably 19-21°C, and further preferably 20°C; the curing time is preferably 1-3 days, more preferably 1.5-3 days, and further preferably 2-3 days; the relative humidity of the curing is preferably ≥95%, and the curing is preferably carried out in a standard curing room. After the curing is completed, the mold is removed to obtain a low-shrinkage geopolymer curing mortar.

[0039] The present invention provides the use of the low shrinkage geopolymer mortar described in the above technical solution, the low shrinkage geopolymer mortar prepared by the preparation method described in the above technical solution, or the low shrinkage geopolymer curing mortar described in the above technical solution in building materials.

[0040] In order to further illustrate the present invention, the low shrinkage geopolymer mortar, its preparation method and application, and low shrinkage geopolymer curing mortar are described in detail below in conjunction with the drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0041] The raw material parameters used in the following examples and comparative examples are as follows:

[0042] The slag is first-grade finely granulated blast furnace slag of grade S95 or above, with a particle size of 0.3 to 300 μm;

[0043] The fly ash is Class F first-grade low-calcium fly ash with a particle size of 0.3 to 350 μm;

[0044] The sand is continuously graded sea sand, meeting the secondary grade specified in GB / T 14684-2001 (by mass percentage, 600 μm 70-41%, 1.18 mm 50-10%, 2.36 mm 25-0%, 4.75 mm 10-1%).

[0045] The preparation method of water-soaked red brick sand is as follows: the dry red brick sand is immersed in water, and soaked at 20-25° C. for 72 hours. After being taken out, the sand is rubbed to a saturated surface dry state to obtain the water-soaked red brick sand.

[0046] Alkaline activator: sodium hydroxide 5.1wt%, water glass 39.5wt% (wherein, in the water glass, sodium oxide 14.95wt%, silicon dioxide 29.01wt%, modulus 2, density 50Be), water (excluding water in the water glass) 55.4wt%; completely dissolve the sodium hydroxide in water, pour the water glass into the obtained sodium hydroxide solution and stir evenly to obtain the alkaline activator, and let it stand for 24h before use.

[0047] Example 1

[0048] Preparation raw materials: 1 part of cementitious material (30% slag, 70% fly ash), 2 parts of fine aggregate (85% continuous graded sea sand, 15% dry red brick sand), 0.5 parts of alkaline activator. The particle size of red brick sand is 0.2-5mm.

[0049] The slag, fly ash, continuously graded sea sand and red brick sand were placed in a mixer and stirred for 2 minutes, and then an alkaline activator was added and stirred for 2 minutes to obtain a low shrinkage geopolymer mortar.

[0050] The low shrinkage geopolymer mortar is loaded into a triple mold in layers. After the first layer of mortar is loaded into the mold, it is compacted with a small tamping rod, especially at the four corners and positions with measuring nails; then the second layer of mortar is loaded, the excess mortar is scraped off and the mortar is placed on a vibrating table and vibrated for 1 minute. After the vibration is completed, the surface is scraped flat and placed in a standard curing room with a temperature of 20±2°C and a relative humidity of ≥95% for curing for 3 days. The mold is removed to obtain a low shrinkage geopolymer curing mortar specimen.

[0051] Example 2

[0052] Low shrinkage geopolymer mortar and low shrinkage geopolymer curing mortar specimens were prepared according to the method of Example 1, the only difference from Example 1 being that the mass fraction of dry red brick sand in the fine aggregate was 25%, and the particle size of the red brick sand was 0.2-5 mm.

[0053] Example 3

[0054] According to the method of Example 1, low shrinkage geopolymer mortar and low shrinkage geopolymer curing mortar specimens were prepared. The only difference from Example 1 was that the red brick sand in the fine aggregate was water-soaked red brick sand, and the particle size of the red brick sand was 5-8 mm.

[0055] Example 4

[0056] According to the method of Example 1, low shrinkage geopolymer mortar and low shrinkage geopolymer curing mortar specimens were prepared. The only difference from Example 1 was that the red brick sand in the fine aggregate was soaked red brick sand, the alkaline activator was 0.44 parts, and the particle size of the red brick sand was 0.2-5 mm.

[0057] Comparative Example 1

[0058] Low shrinkage geopolymer mortar and low shrinkage geopolymer curing mortar specimens were prepared according to the method of Example 1, the only difference from Example 1 being that the fine aggregate did not contain red brick sand.

[0059] Comparative Example 2

[0060] The mortar was prepared according to Chinese patent CN112479674A.

[0061] Preparation raw materials: 1 part of cementitious material (30% slag, 55% fly ash, 25% red brick powder), 2 parts of fine aggregate (sand), 0.5 parts of alkaline activator, wherein the particle size of the red brick powder is 0.3-400 μm.

[0062] Test Example 1

[0063] The low shrinkage geopolymer curing mortar specimens were placed in a shrinkage box at a temperature of 20±2°C and a relative humidity of 60±2% for curing, and the shrinkage values ​​of the specimens were measured in accordance with the building specification JC / T 603-2004. Shrinkage compensation rate = (shrinkage value of the test group - shrinkage value of comparative example 1) / shrinkage value of the test group × 100%, wherein the test group is the embodiment or comparative example 2. The strength test method was carried out in accordance with the specification "GB / T-17671-1999 Cement mortar strength test method", and the fluidity test method was carried out in accordance with "GB / T 8077-2012 Concrete admixture homogeneity test method". The operation test results are shown in Table 1 and Figure 1 shown.

[0064] Table 1 Performance test results of low shrinkage geopolymer curing mortar specimens

[0065]

[0066] From Table 1 and Figure 1It can be seen that the present invention uses red brick sand as part of the fine aggregate, the shrinkage compensation rate of the geopolymer mortar is high, and the shrinkage performance of the geopolymer mortar can be significantly reduced. Using soaked red brick sand as part of the fine aggregate can further improve the fluidity of the geopolymer mortar.

[0067] Test Example 2

[0068] Performance test of red brick sand with different particle sizes

[0069] The water absorption rate and moisture-sensitive water release rate were tested with reference to the ASTM C1671 specification. The specific test steps are as follows: When testing the water absorption rate, first put the red brick sand into a 105℃ drying oven for 24 hours, then put the red brick sand into a beaker to submerge the surface with water, take out the red brick sand at different time periods, and weigh it after wiping it to a saturated surface dry state. The water absorption rate was calculated based on the change in mass. When testing the moisture-sensitive water release rate, put the red brick sand into a beaker and soak it in water for 72 hours. After it fully absorbs water, take out the red brick sand and wipe it to a saturated surface dry state. Put it into a constant temperature and humidity chamber at a temperature of 20℃ and relative humidity of 95%, 75%, and 60%, respectively, measure its mass at intervals, and calculate the water release performance of the red brick sand at different relative humidity. Three parallel samples were set for each group of tests, and the results were taken as the average of the three samples.

[0070] Figure 2 The water absorption results of red brick sand with different particle sizes are shown in Figure 2, where the particle sizes of red brick sand are 0.2-5 mm and 5-8 mm respectively. Figure 2 It can be seen that red brick sand has the ability to absorb water quickly. The water absorption rate of red brick sand increases rapidly from 10min to 24h, and the growth rate tends to be slow from 24h to 72h. At 72h, the water absorption rates of red brick sand with large and small particle sizes are 22.62% and 19.8% respectively, indicating that the maximum water absorption rate of red brick sand is about 20%, and there will be a small increase with the increase of particle size. Therefore, in this test, the red brick sand was pre-soaked in water for 72h to make the red brick sand reach a saturated state.

[0071] Figure 3 The moisture-sensitive water release rate of red brick sand with different particle sizes under different relative humidity changes with time, where the particle sizes of red brick sand are 0.2-5 mm and 5-8 mm, and the relative humidity is 60%, 80% and 95% respectively. Figure 3It can be seen that the lower the relative humidity at the same time, the higher the water release rate of red brick sand, indicating that red brick sand is highly sensitive to changes in relative humidity. At the same relative humidity, the water release rate of large-particle red brick sand is higher than that of small-particle red brick sand. At a relative humidity of 90%, the water release rate of red brick sand is slow, much lower than that of 60% and 80% relative humidity. The pores of the soaked red brick sand are saturated, and the water release rate is slow at high relative humidity, which is conducive to the red brick sand not transferring water to the matrix before the specimen solidifies. After solidification, the relative humidity inside the specimen decreases, the water in the pores is evaporated, and the red brick sand begins to release the pre-stored water to fill the pores and play an internal curing role.

[0072] In summary, the present invention adds waste red brick sand instead of fine aggregate when preparing geopolymer mortar, utilizes the internal curing function of red brick sand to absorb and release water, slows down the rate of decrease of relative humidity inside geopolymer mortar, improves the pore structure of geopolymer mortar, effectively reduces the shrinkage of geopolymer mortar, reduces the shrinkage level of geopolymer mortar to the same level as traditional OPC mortar, and does not significantly reduce the compressive strength. In addition, the addition of red brick sand can also improve the fluidity of geopolymer mortar, improve the construction performance of geopolymer mortar, realize the resource utilization of waste red bricks, have both environmental protection and economic benefits, and have important significance for promoting the application of geopolymer materials in engineering.

[0073] Although the above-mentioned embodiments have made a detailed description of the present invention, they are only some embodiments of the present invention, rather than all embodiments. People can also obtain other embodiments based on the embodiments of the present invention without creative work, and these embodiments all fall within the scope of protection of the present invention.

Claims

1. A low shrinkage geopolymer mortar, characterized in that: The raw materials for preparation are: 1 part of cementitious material, 2-2.5 parts of fine aggregate, and 0.4-0.5 parts of alkaline activator by weight. The alkaline activator comprises sodium hydroxide, water glass and water; The cementitious material comprises fly ash and slag, and the mass fraction of fly ash in the cementitious material is 20-70%; The fine aggregate includes sand and red brick sand, the mass fraction of red brick sand in the fine aggregate is 15-25%, the particle size of the red brick sand is ≤8mm, and the particle size of the sand is ≤4.75mm; The particle size of the red brick sand is 0.2-8 mm; the red brick sand includes dry red brick sand or water-soaked red brick sand; The density of the low shrinkage geopolymer mortar is 1800-2200 kg / m 3 .

2. The low shrinkage geopolymer mortar according to claim 1, characterized in that: The water content of the soaked red brick sand is 18-22wt%.

3. The low shrinkage geopolymer mortar according to claim 1, characterized in that: The sand is continuously graded sand.

4. The low shrinkage geopolymer mortar according to claim 1, characterized in that: The fly ash is low-calcium fly ash, and the particle size of the fly ash is 0.3-300 μm; The slag is blast furnace slag, and the particle size of the slag is 0.3-350 μm.

5. The low shrinkage geopolymer mortar according to claim 1, characterized in that: The alkaline activator has a modulus of 1 to 1.5 and an alkali equivalent of 0.4 to 0.

8.

6. The method for preparing the low shrinkage geopolymer mortar according to any one of claims 1 to 5, characterized in that: The following steps are involved: Fly ash, slag, sand, red brick sand and alkaline activator are mixed to obtain low shrinkage geopolymer mortar.

7. The preparation method according to claim 6, characterized in that: After the alkaline activator is prepared, let it stand for 12 to 48 hours before use.

8. A low shrinkage geopolymer curing mortar, characterized in that: The low shrinkage geopolymer mortar is obtained by curing after casting and forming; the low shrinkage geopolymer mortar is the low shrinkage geopolymer mortar described in any one of claims 1 to 5 or the low shrinkage geopolymer mortar prepared by the preparation method described in any one of claims 6 to 7.

9. Use of the low shrinkage geopolymer mortar according to any one of claims 1 to 5, the low shrinkage geopolymer mortar prepared by the preparation method according to any one of claims 6 to 7, or the low shrinkage geopolymer curing mortar according to claim 8 in building materials.