A method for preparing metallized ceramics for 5G communication

By using the composite plating solution technology of pre-plating copper alloy layer and graphene in the 5G communication system, the composition and sintering process of ceramic powder are optimized, and the problem of low quality factor of existing ceramics is solved, which significantly improves the dielectric performance of ceramics and Adhesion, suitable for high-end filter devices.

CN117567149BActive Publication Date: 2024-11-12CHANG JIANG ELECTRONIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311605708.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-11-12
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

The existing microwave dielectric ceramics have a low quality factor in 5G communication systems, which limits their application in high-end filtering devices. They are mainly due to the large conductivity loss caused by silk screen burning technology, which affects the dielectric performance of the ceramics.

Method used

A metallized ceramic preparation method is adopted, including the addition of graphene in the pre-plating copper alloy layer and composite plating solution, and the composition and structure of the ceramic powder are optimized through ball milling and sintering processes, and the dielectric properties of the ceramic are improved. Specific steps include the preparation of ceramic powder, sintering, pre-plating, preparation of composite plating solution and ceramic metallization, and the use of additives such as B2O3, ZnO and Fe2O3 to reduce the sintering temperature and the generation of the mesophase, and improve density and conductivity.

Benefits of technology

Through the addition of pre-copper alloy layer and graphene, the adhesion and conductivity of the composite coating and ceramics are improved, and the quality factor and dielectric properties of the ceramics are significantly improved. It is suitable for high-end filtering devices in 5G communication systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117567149B_ABST
    Figure CN117567149B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing metallized ceramics for 5G communication, which belongs to the technical field of ceramic preparation; the preparation process thereof comprises the following steps: preparation of ceramic powder; preparation of ceramic; pre-plating of ceramic; preparation of composite plating solution; ceramic metallization. The present invention adds B2O3 to the ceramic powder so that boron exists in liquid phase during sintering. The appearance of liquid phase promotes the formation and growth of grains during sintering, which can reduce the sintering temperature and improve the density of the ceramic. The addition of ZnO and Fe2O3 can effectively inhibit the generation of intermediate phase MgTi2O5, which can effectively reduce the sintering temperature and obtain a dense crystal structure. The addition of ZnO and Fe2O3 improves the quality factor of the ceramic and effectively improves the dielectric properties of the ceramic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic preparation, and in particular to a method for preparing metallized ceramics for 5G communications. Background Art

[0002] Microwave dielectric ceramics refer to ceramics used as dielectric materials in microwave frequency band circuits and perform one or more functions. They are new functional ceramics that have developed rapidly in the past three decades. Microwave dielectric ceramics have the characteristics of high dielectric constant, high stability and low loss, and can meet the requirements of high reliability, low cost, miniaturization and integration of microwave circuits. Therefore, microwave dielectric ceramics are used as key materials for manufacturing dielectric filters in 5G / 6G communication systems. MgTiO3 is low-cost, with a dielectric constant of about 17 and a quality factor of 160,000 GHz, but the resonant frequency temperature coefficient is about -51ppm / ℃. Materials with a large positive temperature coefficient are usually compounded with MgTiO3 to adjust the temperature coefficient. At present, the MgTiO3-CaTiO3 system is widely used in industry. Although the system has relatively excellent comprehensive performance, the quality factor is often low, which limits its application in high-end filtering devices.

[0003] The quality factor of microwave dielectric ceramics is mainly determined by the dielectric loss of the material and the conductivity loss of the metal film. The dielectric loss has been greatly reduced by improving the material properties. The conductivity loss is closely related to the conductivity of the metal film on the ceramic surface. The higher the conductivity of the metal material, the larger the quality factor and the smaller the loss. At present, the ceramic metallization process basically uses the traditional silk-screen silver burning technology. The conductivity loss of the silk-screen silver burning metallized film is large, resulting in a small filter quality factor.

[0004] Therefore, we propose a method for preparing metallized ceramics for 5G communications that can improve the quality factor of ceramic materials. Summary of the invention

[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for preparing metallized ceramics for 5G communications.

[0006] A method for preparing a metallized ceramic for 5G communication comprises the following steps:

[0007] S1: Preparation of ceramic powder

[0008] MgO and TiO2 raw materials are mixed and ball-milled, dried and calcined to synthesize MgTiO3; CaCO3 and TiO2 raw materials are calcined to pre-synthesize CaTiO3; MgTiO3 and CaTiO3 powders are mixed and added into a planetary ball mill; B2O3, ZnO and Fe2O3 are added, and a binder is added; anhydrous ethanol and ZrO2 balls are used as ball milling media for ball milling; after the ball milling is completed, the ball milled slurry is dried and sieved to obtain ceramic powder;

[0009] S2: Preparation of ceramics

[0010] Adding polyvinyl alcohol to the dried ceramic powder for granulation, sieving to obtain granulated powder, pressing the granulated powder into green compacts, placing the green compacts in a muffle furnace for sintering to obtain ceramics;

[0011] S3: Pre-plating of ceramics

[0012] The ceramic is placed in industrial alcohol, cleaned and dried under the assistance of ultrasound, and then plasma glow cleaned to obtain a treated ceramic, and the ceramic is pre-plated with a copper alloy by magnetron sputtering in an argon environment to obtain a pre-plated ceramic;

[0013] S4: Preparation of composite plating solution

[0014] Ethylenediamine and disodium ethylenediaminetetraacetate are dissolved in water and mixed evenly, and then the dissolved silver nitrate solution is added, and the pH is adjusted with sodium hydroxide to obtain component A, graphene is added into TW-20, stirred and mixed with a stirring rod, and then added into component A, fully stirred and ultrasonically dispersed to obtain component B, potassium sodium tartrate is dissolved in water, and the pH is adjusted with sodium hydroxide solution to obtain component C, and component B and component C are mixed evenly to obtain a composite plating solution;

[0015] S5: Ceramic Metallization

[0016] The pre-plated ceramic is placed in a H2SO4 solution for activation to obtain an activated ceramic, and the activated ceramic is placed in a composite plating solution, heated and plated under mechanical stirring, and after the plating is completed, a metallized ceramic plated with a composite coating is obtained.

[0017] Furthermore, the preparation of ceramic powder in step S1 specifically includes the following steps:

[0018] S1.1: 99.9% MgO and 99.9% TiO2 are mixed and ball-milled for 4-5 hours, dried, and then calcined at 1150-1200℃ for 2-3 hours to synthesize pure MgTiO3;

[0019] S1.2: Pre-synthesize CaTiO3 by calcining 99.3% CaCO3 and 99.9% TiO2 at 1090-1100℃ for 5-6h;

[0020] S1.3: Take 90-95 parts of MgTiO3 and 2-5 parts of CaTiO3, mix the MgTiO3 powder and CaTiO3 to obtain a mixed powder, put the mixed powder into a planetary ball mill, add 2-5 parts of B2O3, 1-2 parts of ZnO, 1-2 parts of Fe2O3, and 5-6 parts of a binder, use anhydrous ethanol and ZrO2 balls as ball milling media, the ball milling speed is 400-450r / min, and the mixture is ball milled for 24-25h to obtain a ball milled slurry;

[0021] S1.4: The ball mill slurry is placed in a drying oven for drying. After drying, it is sieved through a 100-110 mesh sieve to obtain ceramic powder.

[0022] Furthermore, the preparation of the ceramic in step S2 specifically includes the following steps:

[0023] S2.1: Add 10-15% polyvinyl alcohol to the dried ceramic powder for granulation, sieve the granules, and bake at 100-105°C for 50-60 minutes to obtain a granulated powder;

[0024] S2.2: Weigh 2-3 portions of the granulated powder and place them into a mold. Apply unidirectional pressure of 2-3 MPa and maintain the pressure for 30-40 seconds to press the powder into a green body.

[0025] S2.3: Place the green body in a muffle furnace, keep it at 600-700°C for 3-4 hours, and then sinter it for 3-4 hours to obtain ceramics.

[0026] Furthermore, step S3 pre-plates the ceramic, specifically comprising the following steps:

[0027] S3.1: Place the ceramic in industrial alcohol, clean it with the aid of ultrasonic waves for 5-10 minutes, take it out, and vacuum dry it at 80-90°C for 20-30 minutes;

[0028] S3.2: The dried ceramic is subjected to plasma glow cleaning in an argon environment at 30-35 Pa and an incident power of 90-95 W for 1-2 min to obtain a treated ceramic;

[0029] S3.3: Pre-plating the ceramic with copper alloy by magnetron sputtering in an argon environment at 0.5-1 Pa for 5-10 minutes to obtain a pre-plated ceramic.

[0030] Furthermore, the preparation of the composite plating solution in step S4 specifically comprises the following steps:

[0031] S4.1: Weigh 25-30 parts of ethylenediamine and 15-18 parts of disodium ethylenediaminetetraacetate and dissolve them in water, then mix them evenly, add 8-10 parts of the dissolved silver nitrate solution, stir evenly, adjust the pH to 12.3-12.5 with sodium hydroxide, and obtain component A;

[0032] S4.2: Weigh 0.25-0.27 parts of graphene and add it to 0.8-1% TW-20. Stir with a stirring rod and add it to component A. Stir thoroughly and disperse ultrasonically for 1-2 hours to obtain component B.

[0033] S4.3: Weigh 15-18 parts of potassium sodium tartrate and dissolve it in water, and adjust the pH with sodium hydroxide solution to obtain component C;

[0034] S4.4: Take 3-6 parts of component B and 1-2 parts of component C and mix them evenly to obtain a composite plating solution.

[0035] Furthermore, step S4 of ceramic metallization specifically includes the following steps:

[0036] S5.1: placing the pre-plated ceramic in a 5-6% H2SO4 solution for 20-30 seconds to activate it, thereby obtaining an activated ceramic;

[0037] S5.2: Place the activated ceramic in a composite plating solution, heat to 45-50°C, and perform plating for 1-2 hours under mechanical stirring at 800-850r / min. After the plating is completed, a metallized ceramic plated with a composite coating is obtained.

[0038] Furthermore, the binder in step S1.3 is a polyvinyl alcohol solution.

[0039] Furthermore, in step S1.4, the temperature of the drying oven is 70-75°C.

[0040] Furthermore, the sintering temperature in step S2.3 is 1200-1250°C.

[0041] Furthermore, in step S3.3, the composition and content of the copper alloy are 54-55% Cu, 29-30% Ti, 14-15% Zn and 1-2% Ag.

[0042] Compared with the prior art, the present invention has at least the following beneficial effects:

[0043] 1. The present invention pre-plates the ceramic with a copper alloy layer and then metallizes the ceramic, so that the subsequent composite coating can better adhere to the ceramic. Because the shrinkage and expansion rates of the silver-containing coating and the ceramic substrate are quite different, the composite coating is wrinkled and separated from the substrate, while the linear thermal expansion coefficient of the copper alloy is relatively small and the bonding force is better. Therefore, the adhesion between the composite coating and the ceramic can be improved by pre-plating the copper alloy layer and then performing the composite coating.

[0044] 2. The present invention adds graphene to the composite plating solution. Since graphene is a conductive particle, the conductivity of the composite coating can be improved after adding graphene. The higher the conductivity, the greater the quality factor value and the smaller the loss. Therefore, after adding graphene, the conductivity of the composite coating is improved and the quality factor of the ceramic is improved.

[0045] 3. The present invention adds B2O3 to the ceramic powder so that boron exists in the liquid phase during sintering. The appearance of the liquid phase promotes the formation and growth of grains during sintering, which can reduce the sintering temperature and improve the density of the ceramic. The addition of ZnO and Fe2O3 can effectively inhibit the generation of the intermediate phase MgTi2O5, which can effectively reduce the sintering temperature and obtain a dense crystal structure. The addition of ZnO and Fe2O3 improves the quality factor of the ceramic and effectively improves the dielectric properties of the ceramic. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable those skilled in the relevant art to make and use the present disclosure.

[0047] Figure 1 A flow chart of a method for preparing a metallized ceramic for 5G communication adopted in an embodiment of the present invention;

[0048] Figure 2 This is a comparison table of dielectric properties of Comparative Example 1 of the present invention;

[0049] Figure 3 This is a comparative table diagram of the conductivity of Example 2 of the present invention. DETAILED DESCRIPTION

[0050] The following is a detailed description of a preparation method of a metallized ceramic for 5G communication provided by the present invention in combination with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternative methods for some known technologies; and the accompanying drawings are only for a more specific description of the embodiments, and are not intended to specifically limit the present invention.

[0051] Example 1

[0052] A method for preparing metallized ceramics for 5G communication, such as Figure 1 As shown, the following steps are included:

[0053] S1: Preparation of ceramic powder

[0054] S1.1: 99.9% MgO and 99.9% TiO2 were mixed and ball-milled for 4 hours and then dried and calcined at 1150℃ for 2 hours to synthesize pure MgTiO3;

[0055] S1.2: Pre-synthesize CaTiO3 by calcining at 1090℃ for 5h with 99.3% CaCO3 and 99.9% TiO2 as raw materials;

[0056] S1.3: Take 90 parts of MgTiO3 and 2 parts of CaTiO3, mix the MgTiO3 powder and CaTiO3 to obtain a mixed powder, put the mixed powder into a planetary ball mill, add 2 parts of B2O3, 1 part of ZnO, 1 part of Fe2O3, and 5 parts of a binder, use anhydrous ethanol and ZrO2 balls as ball milling media, the ball milling speed is 400r / min, mix and ball mill for 24h to obtain a ball milling slurry;

[0057] S1.4: The ball mill slurry is placed in a drying oven at 70°C for drying. After drying, it is sieved through a 100-mesh sieve to obtain ceramic powder.

[0058] S2: Preparation of ceramics

[0059] S2.1: Add 10% polyvinyl alcohol to the dried ceramic powder for granulation, sieve the granules, and bake at 100°C for 50 minutes to obtain a granulated powder;

[0060] S2.2: Weigh 2 portions of the granulated powder and place them into a mold. Apply unidirectional pressure of 2 MPa and maintain the pressure for 30 seconds to press the powder into a green body.

[0061] S2.3: Place the green body in a muffle furnace, keep it at 600°C for 3 hours, and then sinter it at 1200°C for 3 hours to obtain ceramics.

[0062] S3: Pre-plating of ceramics

[0063] S3.1: Place the ceramic in industrial alcohol, clean it under ultrasonic assistance for 5 minutes, take it out, and vacuum dry it at 80℃ for 20 minutes;

[0064] S3.2: The dried ceramic is subjected to plasma glow cleaning in an argon environment, 30 Pa, and an incident power of 90 W for 1 min to obtain a treated ceramic;

[0065] S3.3: The ceramic is pre-plated with a copper alloy by magnetron sputtering in an argon environment at 0.5 Pa for 5 minutes. The composition and content of the copper alloy are 54.75% Cu, 29.13% Ti, 14.32% Zn and 1.8% Ag to obtain a pre-plated ceramic.

[0066] S4: Preparation of composite plating solution

[0067] S4.1: Weigh 25 parts of ethylenediamine and 15 parts of disodium ethylenediaminetetraacetate and dissolve them in water, then mix them evenly, add 8 parts of the dissolved silver nitrate solution, stir evenly, adjust the pH to 12.3 with sodium hydroxide, and obtain component A;

[0068] S4.2: Weigh 0.25 parts of graphene and add it to 0.8% TW-20. Stir with a stirring rod and then add it to component A. Stir thoroughly and disperse ultrasonically for 1 hour to obtain component B.

[0069] S4.3: Weigh 15 parts of potassium sodium tartrate and dissolve it in water, and adjust the pH with sodium hydroxide solution to obtain component C;

[0070] S4.4: Take 3 parts of component B and 1 part of component C and mix them evenly to obtain a composite plating solution.

[0071] S5: Ceramic Metallization

[0072] S5.1: placing the pre-plated ceramic in a 5% H2SO4 solution for 20 seconds to activate it, thereby obtaining an activated ceramic;

[0073] S5.2: Place the activated ceramic in a composite plating solution, heat to 45°C, and perform plating for 1 hour under mechanical stirring at 800 r / min. After the plating is completed, a metallized ceramic plated with a composite coating is obtained.

[0074] Example 2

[0075] A method for preparing metallized ceramics for 5G communication, such as Figure 1 As shown, the following steps are included:

[0076] S1: Preparation of ceramic powder

[0077] S1.1: 99.9% MgO and 99.9% TiO2 were mixed and ball-milled for 4 hours and then dried and calcined at 1150℃ for 2 hours to synthesize pure MgTiO3;

[0078] S1.2: Pre-synthesize CaTiO3 by calcining at 1090℃ for 5h with 99.3% CaCO3 and 99.9% TiO2 as raw materials;

[0079] S1.3: Take 95 parts of MgTiO3 and 5 parts of CaTiO3, mix the MgTiO3 powder and CaTiO3 to obtain a mixed powder, put the mixed powder into a planetary ball mill, add 5 parts of B2O3, 2 parts of ZnO, 2 parts of Fe2O3, and 6 parts of a binder, use anhydrous ethanol and ZrO2 balls as ball milling media, the ball milling speed is 400r / min, and the mixture is ball milled for 24h to obtain a ball milling slurry;

[0080] S1.4: The ball mill slurry is placed in a drying oven at 70°C for drying. After drying, it is sieved through a 100-mesh sieve to obtain ceramic powder.

[0081] S2: Preparation of ceramics

[0082] S2.1: Add 15% polyvinyl alcohol to the dried ceramic powder for granulation, sieve the granules, and bake at 100° C. for 50 min to obtain a granulated powder;

[0083] S2.2: Weigh 3 portions of the granulated powder and place them into a mold. Apply unidirectional pressure of 2 MPa and maintain the pressure for 30 seconds to press the powder into a green body.

[0084] S2.3: Place the green body in a muffle furnace, keep it at 600°C for 3 hours, and then sinter it at 1200°C for 3 hours to obtain ceramics.

[0085] S3: Pre-plating of ceramics

[0086] S3.1: Place the ceramic in industrial alcohol, clean it under ultrasonic assistance for 5 minutes, take it out, and vacuum dry it at 80℃ for 20 minutes;

[0087] S3.2: The dried ceramic is subjected to plasma glow cleaning in an argon environment, 30 Pa, and an incident power of 90 W for 1 min to obtain a treated ceramic;

[0088] S3.3: The ceramic is pre-plated with a copper alloy by magnetron sputtering in an argon environment at 0.5 Pa for 5 minutes. The composition and content of the copper alloy are 54.75% Cu, 29.13% Ti, 14.32% Zn and 1.8% Ag to obtain a pre-plated ceramic.

[0089] S4: Preparation of composite plating solution

[0090] S4.1: Weigh 30 parts of ethylenediamine and 18 parts of disodium ethylenediaminetetraacetate and dissolve them in water, then mix them evenly, add 10 parts of the dissolved silver nitrate solution, stir evenly, adjust the pH to 12.5 with sodium hydroxide, and obtain component A;

[0091] S4.2: Weigh 0.27 parts of graphene and add it to 1% TW-20. Stir with a stirring rod and then add it to component A. Stir thoroughly and disperse ultrasonically for 1 hour to obtain component B.

[0092] S4.3: Weigh 18 parts of potassium sodium tartrate and dissolve it in water, and adjust the pH with sodium hydroxide solution to obtain component C;

[0093] S4.4: Take 6 parts of component B and 2 parts of component C and mix them evenly to obtain a composite plating solution.

[0094] S5: Ceramic Metallization

[0095] S5.1: placing the pre-plated ceramic in a 6% H2SO4 solution for 20 seconds to activate it, thereby obtaining an activated ceramic;

[0096] S5.2: Place the activated ceramic in a composite plating solution, heat to 45°C, and perform plating for 1 hour under magnetic mechanical stirring at 800 r / min. After the plating is completed, a metallized ceramic plated with a composite coating is obtained.

[0097] Example 3

[0098] A method for preparing metallized ceramics for 5G communication, such as Figure 1 As shown, the following steps are included:

[0099] S1: Preparation of ceramic powder

[0100] S1.1: 99.9% MgO and 99.9% TiO2 are mixed and ball-milled for 5 hours, dried, and then calcined at 1200℃ for 3 hours to synthesize pure MgTiO3;

[0101] S1.2: Pre-synthesize CaTiO3 by calcining 99.3% CaCO3 and 99.9% TiO2 at 1100℃ for 6h;

[0102] S1.3: Take 90 parts of MgTiO3 and 2 parts of CaTiO3, mix the MgTiO3 powder and CaTiO3 to obtain a mixed powder, put the mixed powder into a planetary ball mill, add 2 parts of B2O3, 1 part of ZnO, 1 part of Fe2O3, and 5 parts of a binder, use anhydrous ethanol and ZrO2 balls as ball milling media, the ball milling speed is 400r / min, mix and ball mill for 24h to obtain a ball milling slurry;

[0103] S1.4: The ball mill slurry is placed in a drying oven at 70°C for drying. After drying, it is sieved through a 100-mesh sieve to obtain ceramic powder.

[0104] S2: Preparation of ceramics

[0105] S2.1: Add 15% polyvinyl alcohol to the dried ceramic powder for granulation, sieve the granules, and bake at 105°C for 60 minutes to obtain a granulated powder;

[0106] S2.2: Weigh 2 portions of the granulated powder and place them into a mold. Apply unidirectional pressure of 2 MPa and maintain the pressure for 40 seconds to press the powder into a green compact.

[0107] S2.3: Place the green body in a muffle furnace, keep it at 700°C for 4 hours, and then sinter it at 1250°C for 4 hours to obtain ceramics.

[0108] S3: Pre-plating of ceramics

[0109] S3.1: Place the ceramic in industrial alcohol, clean it under ultrasonic assistance for 10 minutes, take it out, and vacuum dry it at 90°C for 30 minutes;

[0110] S3.2: The dried ceramic is subjected to plasma glow cleaning in an argon environment, 35 Pa, and an incident power of 95 W for 2 min to obtain a treated ceramic;

[0111] S3.3: The ceramic is pre-plated with a copper alloy by magnetron sputtering in an argon environment at 1 Pa for 10 minutes, wherein the composition and content of the copper alloy are 54.75% Cu, 29.13% Ti, 14.32% Zn and 1.8% Ag, to obtain a pre-plated ceramic.

[0112] S4: Preparation of composite plating solution

[0113] S4.1: Weigh 25 parts of ethylenediamine and 15 parts of disodium ethylenediaminetetraacetate and dissolve them in water, then mix them evenly, add 8-10 parts of the dissolved silver nitrate solution, stir evenly, adjust the pH to 12.3 with sodium hydroxide, and obtain component A;

[0114] S4.2: Weigh 0.25 parts of graphene and add it to 0.8% TW-20. Stir with a stirring rod and then add it to component A. Stir thoroughly and disperse ultrasonically for 2 hours to obtain component B.

[0115] S4.3: Weigh 15 parts of potassium sodium tartrate and dissolve it in water, and adjust the pH with sodium hydroxide solution to obtain component C;

[0116] S4.4: Take 3 parts of component B and 1 part of component C and mix them evenly to obtain a composite plating solution.

[0117] S5: Ceramic Metallization

[0118] S5.1: placing the pre-plated ceramic in a 5% H2SO4 solution for 30 seconds to activate it, thereby obtaining an activated ceramic;

[0119] S5.2: Place the activated ceramic in a composite plating solution, heat to 50°C, and perform plating for 2 hours under mechanical stirring at 850 r / min. After the plating is completed, a metallized ceramic plated with a composite coating is obtained.

[0120] Comparative Example 1

[0121] Compared with Example 1, the difference of Comparative Example 1 is that, in Comparative Example 1, ZnO and Fe2O3 in step S1.3 are removed, and the other steps remain unchanged to prepare the metallized ceramic, which is recorded as Comparative Example 1.

[0122] The metallized ceramics prepared in Example 1, Example 2, Example 3 and the metallized ceramics prepared in Comparative Example 1 were taken into cubes of the same size and mass, and their microwave dielectric properties were tested using a microwave network analyzer. The tests were conducted twice in parallel, and the data were recorded. Figure 2 It can be seen that the dielectric properties of the embodiments are better than those of comparative example 1, and the quality factors of the embodiments are higher than those of comparative example 1, indicating that the addition of ZnO and Fe2O3 can improve the quality factor.

[0123] Comparative Example 2

[0124] Compared with Example 1, the difference of Comparative Example 2 is that step S4.2 is removed in Comparative Example 2, component B in step S4.4 is replaced by component A of medium quality in step S4.1, and the other steps remain unchanged to prepare the metallized ceramic, which is recorded as Comparative Example 2.

[0125] The metallized ceramics prepared in Example 1, Example 2, and Example 3 and the metallized ceramics prepared in Comparative Example 2 were taken into cubes of the same size and mass, and the conductivity of the coating was calculated by measuring the thickness and square resistance of the coating. The square resistance of the coating was measured using an RTS-9 four-probe resistance meter, and the thickness of the coating was measured using a metallographic microscope. The calculation formula is as follows: σ=1 / (RL), where σ is the conductivity, R is the square resistance, and L is the thickness of the coating. The data were recorded and tested twice. Figure 3 It can be seen that the electrical conductivity of the embodiments is higher than that of the comparative example 2, indicating that the electrical conductivity of the coating can be improved after adding graphene.

[0126] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing metallized ceramics for 5G communication, characterized in that: The steps include: S1: Preparation of ceramic powder MgO and TiO2 raw materials are mixed and ball-milled, dried and calcined to synthesize MgTiO3; CaCO3 and TiO2 raw materials are calcined to pre-synthesize CaTiO3; MgTiO3 and CaTiO3 powders are mixed and added into a planetary ball mill; B2O3, ZnO and Fe2O3 are added, and a binder is added; anhydrous ethanol and ZrO2 balls are used as ball milling media for ball milling; after the ball milling is completed, the ball milled slurry is dried and sieved to obtain ceramic powder; S2: Preparation of ceramics Adding polyvinyl alcohol to the dried ceramic powder for granulation, sieving to obtain granulated powder, pressing the granulated powder into green compacts, placing the green compacts in a muffle furnace for sintering to obtain ceramics; S3: Pre-plating of ceramics The ceramic is placed in industrial alcohol, cleaned and dried under the assistance of ultrasound, and then plasma glow cleaned to obtain a treated ceramic, and the ceramic is pre-plated with a copper alloy by magnetron sputtering in an argon environment to obtain a pre-plated ceramic; S4: Preparation of composite plating solution Ethylenediamine and disodium ethylenediaminetetraacetate are dissolved in water and mixed evenly, and then the dissolved silver nitrate solution is added, and the pH is adjusted with sodium hydroxide to obtain component A, graphene is added into TW-20, stirred and mixed with a stirring rod, and then added into component A, fully stirred and ultrasonically dispersed to obtain component B, potassium sodium tartrate is dissolved in water, and the pH is adjusted with sodium hydroxide solution to obtain component C, and component B and component C are mixed evenly to obtain a composite plating solution; S5: Ceramic Metallization Placing the pre-plated ceramic in a H2SO4 solution for activation to obtain an activated ceramic, placing the activated ceramic in a composite plating solution, heating and plating under mechanical stirring, and obtaining a metallized ceramic plated with a composite coating after plating; Step S1: Preparation of ceramic powder, specifically comprising the following steps: S1.1: 99.9% MgO and 99.9% TiO2 are mixed and ball-milled for 4-5 hours, dried, and then calcined at 1150-1200℃ for 2-3 hours to synthesize pure MgTiO3; S1.2: Pre-synthesize CaTiO3 by calcining 99.3% CaCO3 and 99.9% TiO2 at 1090-1100℃ for 5-6h; S1.3: Take 90-95 parts of MgTiO3 and 2-5 parts of CaTiO3, mix the MgTiO3 powder and CaTiO3 to obtain a mixed powder, put the mixed powder into a planetary ball mill, add 2-5 parts of B2O3, 1-2 parts of ZnO, 1-2 parts of Fe2O3, and 5-6 parts of a binder, use anhydrous ethanol and ZrO2 balls as ball milling media, the ball milling speed is 400-450r / min, and the mixture is ball milled for 24-25h to obtain a ball milled slurry; S1.4: The ball mill slurry is placed in a drying oven for drying, and after drying, it is sieved through a 100-110 mesh sieve to obtain ceramic powder; Step S3 pre-plates the ceramic, specifically comprising the following steps: S3.1: Place the ceramic in industrial alcohol, clean it with the aid of ultrasonic waves for 5-10 minutes, take it out, and vacuum dry it at 80-90°C for 20-30 minutes; S3.2: The dried ceramic is subjected to plasma glow cleaning in an argon environment at 30-35 Pa and an incident power of 90-95 W for 1-2 min to obtain a treated ceramic; S3.3: pre-plating the ceramic with copper alloy by magnetron sputtering in an argon environment at 0.5-1 Pa for 5-10 minutes to obtain a pre-plated ceramic; Step S4: Preparation of the composite plating solution, specifically comprising the following steps: S4.1: Weigh 25-30 parts of ethylenediamine and 15-18 parts of disodium ethylenediaminetetraacetate and dissolve them in water, then mix them evenly, add 8-10 parts of the dissolved silver nitrate solution, stir evenly, adjust the pH to 12.3-12.5 with sodium hydroxide, and obtain component A; S4.2: Weigh 0.25-0.27 parts of graphene and add it to 0.8-1% of TW-20. Stir with a stirring rod and add it to component A. Stir thoroughly and disperse ultrasonically for 1-2 hours to obtain component B. S4.3: Weigh 15-18 parts of potassium sodium tartrate and dissolve it in water, and adjust the pH with sodium hydroxide solution to obtain component C; S4.4: Take 3-6 parts of component B and 1-2 parts of component C and mix them evenly to obtain a composite plating solution; Among them, the composition and content of the copper alloy in step S3.3 are 54-55% Cu, 29-30% Ti, 14-15% Zn and 1-2% Ag.

2. The method for preparing a metallized ceramic for 5G communication according to claim 1, characterized in that: Step S2: Preparation of ceramics, specifically comprising the following steps: S2.1: Add 10-15% polyvinyl alcohol to the dried ceramic powder for granulation, sieve the granules, and bake at 100-105°C for 50-60 minutes to obtain granulated powder; S2.2: Weigh 2-3 portions of the granulated powder and place them into a mold. Apply unidirectional pressure of 2-3 MPa and maintain the pressure for 30-40 seconds to press the powder into a green body. S2.3: Place the green body in a muffle furnace, keep it at 600-700°C for 3-4 hours, and then sinter it for 3-4 hours to obtain ceramics.

3. The method for preparing a metallized ceramic for 5G communication according to claim 2, characterized in that: Step S5: ceramic metallization, specifically comprising the following steps: S5.1: placing the pre-plated ceramic in a 5-6% H2SO4 solution for 20-30 seconds to activate it, thereby obtaining an activated ceramic; S5.2: Place the activated ceramic in a composite plating solution, heat to 45-50°C, and perform plating for 1-2 hours under mechanical stirring at 800-850r / min. After the plating is completed, a metallized ceramic plated with a composite coating is obtained.

4. The method for preparing a metallized ceramic for 5G communication according to claim 2, characterized in that: The binder in step S1.3 is a polyvinyl alcohol solution.

5. The method for preparing a metallized ceramic for 5G communication according to claim 2, characterized in that: The temperature of the drying oven in step S1.4 is 70-75°C.

6. The method for preparing a metallized ceramic for 5G communication according to claim 3, characterized in that: The sintering temperature in step S2.3 is 1200-1250°C.