A polyurethane elastomer, its preparation method and application

By introducing epoxy monomers into polyurethane elastomers to regulate the strength and concentration of hydrogen bonds, the problem of insufficient adhesion energy at the interface between soft and hard materials is solved, and polyurethane elastomers with high adhesion performance and low thermal resistance are prepared, which are suitable for electronic products and other fields.

CN117567719BActive Publication Date: 2026-11-17SHENZHEN INST OF ADVANCED ELECTRONICS MATERIALS +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311434266.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-30
Publication Date
2026-11-17
Estimated Expiration
2043-10-30

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively improve adhesion energy at the interface between soft and hard materials to reduce interfacial thermal resistance, especially in nanoscale structures where interfacial thermal resistance significantly impacts heat transfer performance.

Method used

By introducing epoxy monomers, such as epoxidized soybean oil, into polyurethane elastomers, the hydrogen bond strength and concentration can be controlled to enhance adhesion to hard interfaces, thus preparing polyurethane elastomers with high adhesion performance and low thermal resistance.

Benefits of technology

A polyurethane elastomer with high adhesion and low thermal resistance has been developed, which is suitable for soft-hard interface materials, and significantly reduces interfacial thermal resistance, especially in electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117567719B_ABST
    Figure CN117567719B_ABST
Patent Text Reader

Abstract

This invention relates to the field of interface materials technology. It provides a method for preparing a polyurethane elastomer by introducing epoxy monomers into the polyurethane elastomer to control the hydrogen bond strength and concentration, thereby obtaining a polyurethane elastomer with high adhesive work and low contact thermal resistance. The introduction of hydrogen bonds not only enhances the cohesive force of the elastomer but also improves its adhesion to hard interfaces. When epoxy monomers are added to the system, the introduction of polymers that cannot generate strong hydrogen bonds reduces the overall hydrogen bond concentration and strength of the material. Epoxy monomers, acting as crosslinking agents, can enhance the cohesive force of the elastomer, thus increasing the adhesive work. Therefore, with the appropriate addition of epoxy monomers, excellent adhesive properties and low thermal resistance can be obtained. Experiments show that when the epoxy monomer is epoxidized soybean oil, by adding epoxidized soybean oil to control the hydrogen bond strength and concentration, a polyurethane elastomer with high adhesive work and low thermal resistance is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of interface materials technology, and in particular to a polyurethane elastomer, its preparation method, and its application. Background Technology

[0002] Thermal resistance at soft-hard material interfaces has always been one of the most significant bottlenecks in improving interfacial thermal transport performance, which is crucial for a wide range of applications, including electronic packaging, batteries, electronic skin, and medicine. Particularly when the feature size of the structure approaches the nanometer scale, interfacial thermal resistance becomes increasingly important, even dominating heat transport, due to the high interfacial density. It is well known that interfacial thermal resistance largely depends on the phonon spectrum matching (acoustic matching) of the materials constituting the interface. However, due to different compositions and bond properties, the phonon spectra of soft and hard materials often exhibit large mismatches. Strategies such as inserting intermediate layers at the interface to enhance phonon matching have attracted considerable attention in order to reduce interfacial thermal resistance. However, these strategies typically involve extremely complex and time-consuming fabrication processes, and it is difficult to obtain structurally similar intermediate layers to match the phonon spectra of common soft materials such as epoxy resins, polyurethanes, and silicones.

[0003] In fact, numerous studies have demonstrated that adhesion energy is another key factor influencing interfacial heat transfer. Typically, soft-hard material interfaces primarily depend on relatively weak physical interactions, such as van der Waals interactions, and thus exhibit large interfacial thermal resistance. Existing research has shown that the van der Waals interaction between a pair of atoms at two interfaces can be quantitatively represented by adhesion energy rather than adhesion strength. Furthermore, Scott T. Huxtable et al. found that as the hydrophilicity of the gold surface increases, the interfacial adhesion energy increases, and the thermal conductivity increases linearly. Forming covalent bonds at the interface can increase the adhesion energy, thereby enhancing interfacial heat transfer. However, this strategy is generally not applicable to soft-hard interfaces because, in practical applications, they are typically bonded through physical means rather than chemical reactions.

[0004] In summary, improving adhesion energy to reduce interfacial thermal resistance at the interface between soft and hard materials remains a pressing issue in this field. Summary of the Invention

[0005] This invention provides a polyurethane elastomer, its preparation method, and its application, in order to solve or at least partially solve the defects existing in the prior art.

[0006] In a first aspect, the present invention provides a polyurethane elastomer comprising the following raw materials: hydroxyl-terminated polyolefin, diisocyanate, epoxy monomer, first catalyst, second catalyst, and solvent;

[0007] The molar ratio between the hydroxyl-terminated polyolefin and the epoxy monomer is 1:(0.01 to 0.1).

[0008] Preferably, in the polyurethane elastomer, the epoxy monomer comprises at least one of epoxidized soybean oil, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, glycerol triglycidyl ether, and trimethylolpropane triglycidyl ether.

[0009] Preferably, in the polyurethane elastomer, the hydroxyl-terminated polyolefin includes at least one of hydroxyl-terminated polyethylene, hydroxyl-terminated polypropylene, hydroxyl-terminated polybutadiene, hydroxyl-terminated hydrogenated polybutadiene, hydroxyl-terminated polyisoprene, and hydroxyl-terminated hydrogenated polyisoprene.

[0010] Preferably, in the polyurethane elastomer, the diisocyanate includes at least one selected from isophthalic diisocyanate, toluene-2,4-diisocyanate, terephthalic diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate.

[0011] Preferably, in the polyurethane elastomer, the first catalyst comprises at least one selected from dibutyltin dilaurate, stannous isooctanoate, triethylenediamine, and N,N-dimethylcyclohexylamine;

[0012] And / or, the second catalyst comprises at least one of benzyldimethylamine, imidazole, boron trifluoride complex, and 4-dimethylaminopyridine.

[0013] Preferably, the solvent in the polyurethane elastomer includes at least one selected from dichloromethane, trichloromethane, toluene, and tetrahydrofuran.

[0014] Preferably, in the polyurethane elastomer, the molar ratio of hydroxyl groups in the hydroxyl-terminated polyolefin to isocyanates in the diisocyanate is (1.1-2):1.

[0015] The molar amount of the first catalyst is 0.1% to 5% of the molar amount of isocyanate in the diisocyanate;

[0016] The molar ratio between the hydroxyl-terminated polyolefin and the solvent is 1:(0.1~10);

[0017] The molar amount of the second catalyst is 1 to 10% of the molar amount of the epoxy monomer.

[0018] Secondly, the present invention also provides a method for preparing the polyurethane elastomer, comprising the following steps:

[0019] Hydroxyl-terminated polyolefin, diisocyanate, first catalyst, and solvent are mixed, then epoxy monomer and second catalyst are added, and the mixture is cured to obtain polyurethane elastomer.

[0020] Preferably, the method for preparing the polyurethane elastomer involves mixing hydroxyl-terminated polyolefin, diisocyanate, a first catalyst, and a solvent at 25–80°C, adding an epoxy monomer and a second catalyst, and curing at 150–200°C for 1–6 hours to obtain the polyurethane elastomer.

[0021] Thirdly, the present invention also provides an application of the above-described polyurethane elastomer or the polyurethane elastomer prepared by the above-described preparation method as an interface material in electronic products.

[0022] The present invention has the following advantages over the prior art:

[0023] The method for preparing polyurethane elastomers of the present invention controls the hydrogen bond strength and concentration in the elastomer by introducing epoxy monomers (such as epoxidized soybean oil) into the polyurethane elastomer, thereby obtaining a polyurethane elastomer with high adhesive work and low contact thermal resistance. The introduction of hydrogen bonds not only enhances the cohesive force of the elastomer but also improves adhesion to hard interfaces. When epoxy monomers (such as epoxidized soybean oil) are added to the system, the overall hydrogen bond concentration and strength of the material decrease due to the introduction of polymers that cannot generate strong hydrogen bonds. However, epoxy monomers (such as epoxidized soybean oil) act as crosslinking agents, enhancing the cohesive force of the elastomer and thus improving adhesive work. Therefore, with the addition of appropriate epoxy monomers (such as epoxidized soybean oil), excellent adhesive performance and low thermal resistance can be obtained. When the molar ratio between hydroxyl-terminated polyolefins and epoxy monomers is 1:(0.01 to 0.1), the addition of epoxy monomers at this molar ratio can give the polyurethane elastomer high adhesive performance and low thermal resistance. Experiments show that when the epoxy monomer is epoxidized soybean oil, by adding epoxidized soybean oil to control the hydrogen bond strength and concentration, a high adhesion work (13535 J·m) can be prepared. -2 ) and low thermal resistance (0.89×10 -6 m 2 ·K·W -1 ) of polyurethane elastomer. Attached Figure Description

[0024] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0025] Figure 1 This is a schematic diagram illustrating the preparation principle of the polyurethane elastomer of the present invention;

[0026] Figure 2 The hydrogen bond distribution of the polyurethane elastomer prepared according to the present invention is shown. Detailed Implementation

[0027] The technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0028] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.

[0029] The following provides a detailed description of each example. It should be noted that the order of description of the embodiments below is not intended to limit the preferred order of the embodiments. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a rigid limitation on the scope of the invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single digits within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Additionally, whenever a numerical range is indicated herein, it means including any referenced number (fraction or integer) within the indicated range.

[0030] This invention provides a polyurethane elastomer comprising the following raw materials: hydroxyl-terminated polyolefin, diisocyanate, epoxy monomer, first catalyst, second catalyst, and solvent;

[0031] The molar ratio between the hydroxyl-terminated polyolefin and the epoxy monomer is 1:(0.01~0.1).

[0032] It should be noted that the polyurethane elastomer of the present invention controls the hydrogen bond strength and concentration in the elastomer by introducing epoxy monomers (such as epoxidized soybean oil). The introduction of hydrogen bonds not only enhances the cohesive force of the elastomer but also enhances its adhesion to hard interfaces. When epoxy monomers (such as epoxidized soybean oil) are added to the system, the overall hydrogen bond concentration and strength of the material will decrease due to the introduction of polymers that cannot generate strong hydrogen bonds. However, epoxy monomers (such as epoxidized soybean oil) can enhance the cohesive force of the elastomer and thus enhance the adhesive work by acting as crosslinking agents. Therefore, with the addition of appropriate epoxy monomers (such as epoxidized soybean oil), excellent adhesive properties and low thermal resistance can be obtained. Specifically, when the molar ratio between hydroxyl-terminated polyolefin and epoxy monomer is 1:(0.01~0.1), the addition of epoxy monomers at the above molar ratio can give the polyurethane elastomer higher adhesive properties and lower thermal resistance. Specifically, the molar ratio between hydroxyl-terminated polyolefin and epoxy monomer is 1:(0.01~0.1). For example, the molar ratio between hydroxyl-terminated polyolefin and epoxy monomer is 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, 1:0.1, etc.

[0033] In some embodiments, the epoxy monomer includes at least one selected from epoxidized soybean oil, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, glycerol triglycidyl ether, and trimethylolpropane triglycidyl ether. Preferably, the epoxy monomer is epoxidized soybean oil.

[0034] In some embodiments, the hydroxyl-terminated polyolefin includes at least one selected from hydroxyl-terminated polyethylene, hydroxyl-terminated polypropylene, hydroxyl-terminated polybutadiene, hydroxyl-terminated hydrogenated polybutadiene, hydroxyl-terminated polyisoprene, and hydroxyl-terminated hydrogenated polyisoprene. Preferably, the hydroxyl-terminated polyolefin is hydroxyl-terminated polybutadiene.

[0035] In some embodiments, the diisocyanate includes at least one selected from isophthalic diisocyanate, toluene-2,4-diisocyanate, terephthalic diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate. Preferably, the diisocyanate is hexamethylene diisocyanate.

[0036] In some embodiments, the first catalyst includes at least one of dibutyltin dilaurate, stannous isooctanoate, triethylenediamine, and N,N-dimethylcyclohexylamine; preferably, the first catalyst is dibutyltin dilaurate.

[0037] In some embodiments, the second catalyst comprises at least one of benzyldimethylamine, imidazole, boron trifluoride complex, and 4-dimethylaminopyridine. Preferably, the second catalyst is 4-dimethylaminopyridine.

[0038] In some embodiments, the solvent includes at least one selected from dichloromethane, trichloromethane, toluene, and tetrahydrofuran. Preferably, the solvent is dichloromethane.

[0039] In some embodiments, the molar ratio of hydroxyl groups in the hydroxyl-terminated polyolefin to isocyanates in the diisocyanate is (1.1–2):1.

[0040] In some embodiments, the molar amount of the first catalyst is 0.1 to 5% of the molar amount of isocyanate in the diisocyanate.

[0041] In some embodiments, the molar ratio between the hydroxyl-terminated polyolefin and the solvent is 1:(0.1 to 10).

[0042] In some embodiments, the molar amount of the second catalyst is 1 to 10% of the molar amount of the epoxy monomer.

[0043] Based on the same inventive concept, the present invention also provides a method for preparing the above-mentioned polyurethane elastomer, comprising the following steps:

[0044] Hydroxyl-terminated polyolefin, diisocyanate, first catalyst, and solvent are mixed, then epoxy monomer and second catalyst are added, and the mixture is cured to obtain polyurethane elastomer.

[0045] In some embodiments, hydroxyl-terminated polyolefin, diisocyanate, first catalyst, and solvent are mixed at 25–80°C, epoxy monomer and second catalyst are added, and the mixture is cured at 150–200°C for 1–6 hours to obtain polyurethane elastomer.

[0046] Specifically, in some embodiments, the method for preparing polyurethane elastomer includes the following steps:

[0047] S1. Add hydroxyl-terminated polyolefin, diisocyanate, first catalyst, and solvent to a flask to obtain a first mixture;

[0048] S2. Stir the first mixture at 25–80°C for 0.5–6 hours;

[0049] S3. Subsequently, epoxy monomer and second catalyst are added to the flask, and after mixing, a second mixture is obtained.

[0050] S4. Pour the second mixture into a polytetrafluoroethylene mold in a vacuum environment and cure it at 150-200°C for 1-6 hours to obtain a polyurethane elastomer material with low thermal resistance and high adhesion.

[0051] Further reference Figure 1 As shown, it illustrates the preparation principle of the polyurethane elastomer of the present invention. Figure 1The structural formula of hydroxyl-terminated polyolefins (specifically hydroxyl-terminated polybutadiene) is shown below:

[0052]

[0053] The structural formula of the diisocyanate (specifically hexamethylene diisocyanate) is shown below:

[0054]

[0055] In this process, hydroxyl-terminated polyolefins and diisocyanates react to form polyurethane, as shown in the following reaction formula:

[0056]

[0057] The structural formula of polyurethane is shown below:

[0058]

[0059] Furthermore, polyurethane reacts with epoxy monomer X as follows to ultimately obtain polyurethane elastomer, as shown in the following reaction formula:

[0060]

[0061] The hydrogen bond distribution of the final prepared polyurethane elastomer is as follows: Figure 2 As shown.

[0062] The method for preparing polyurethane elastomers of the present invention controls the hydrogen bond strength and concentration in the elastomer by introducing epoxy monomers (such as epoxidized soybean oil) into the polyurethane elastomer, thereby obtaining a polyurethane elastomer with high adhesive work and low contact thermal resistance. The introduction of hydrogen bonds not only enhances the cohesive force of the elastomer but also improves adhesion to hard interfaces. When epoxy monomers (such as epoxidized soybean oil) are added to the system, the overall hydrogen bond concentration and strength of the material decrease due to the introduction of polymers that cannot generate strong hydrogen bonds. However, epoxy monomers (such as epoxidized soybean oil) act as crosslinking agents, enhancing the cohesive force of the elastomer and thus improving adhesive work. Therefore, with the addition of appropriate epoxy monomers (such as epoxidized soybean oil), excellent adhesive performance and low thermal resistance can be obtained. When the molar ratio between hydroxyl-terminated polyolefins and epoxy monomers is 1:(0.01 to 0.1), the addition of epoxy monomers at this molar ratio can give the polyurethane elastomer high adhesive performance and low thermal resistance. Experiments show that when the epoxy monomer is epoxidized soybean oil, by adding epoxidized soybean oil to control the hydrogen bond strength and concentration, a high adhesion work (13535 J·m) can be prepared. -2 ) and low thermal resistance (0.89×10 -6 m 2 ·K·W -1 ) of polyurethane elastomer.

[0063] Based on the same inventive concept, the present invention also provides the application of the above-mentioned polyurethane elastomer or the polyurethane elastomer prepared by the above-mentioned preparation method as an interface material in electronic products.

[0064] Specifically, the polyurethane elastomer of the present invention can be used as a soft-hard interface material in electronic packaging, batteries, electronic skin, and medical electronic products.

[0065] The following detailed embodiments further illustrate the polyurethane elastomer and its preparation method of this application. This section further explains the invention in conjunction with specific embodiments, but should not be construed as limiting the invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods, and equipment used in this invention are conventional reagents, methods, and equipment in the art.

[0066] The hydroxyl-terminated hydrogenated polybutadiene in Examples 1-4 and Comparative Example 1 was purchased from Nippon Soda Co., Ltd. (NISSO), model GI2000;

[0067] The epoxidized soybean oil used in Examples 1-4 and Comparative Example 1 was purchased from Aladdin (CAS: 8013-07-8).

[0068] Example 1

[0069] This embodiment provides a polyurethane elastomer comprising the following raw materials: hydroxyl-terminated polyolefin, diisocyanate, epoxy monomer, first catalyst, second catalyst, and solvent;

[0070] Among them, the hydroxyl-terminated polyolefin is hydroxyl-terminated hydrogenated polybutadiene;

[0071] The diisocyanate is hexamethylene diisocyanate;

[0072] The epoxy monomer is epoxidized soybean oil;

[0073] The first catalyst is dibutyltin dilaurate;

[0074] The second catalyst is 4-dimethylaminopyridine;

[0075] The solvent is dichloromethane;

[0076] In the hydroxyl-terminated polyolefin, the molar ratio of hydroxyl groups to isocyanates in the diisocyanate is 1.1:1.

[0077] The molar amount of the first catalyst is 0.5% of the molar amount of isocyanate in the diisocyanate;

[0078] The molar ratio between the hydroxyl-terminated polyolefin and the solvent is 1:0.4;

[0079] The molar ratio between the hydroxyl-terminated polyolefin and the epoxy monomer is 1:0.05;

[0080] The molar amount of the second catalyst is 2.5% of the molar amount of the epoxy monomer.

[0081] The above-mentioned method for preparing polyurethane elastomer includes the following steps:

[0082] S1. Hydroxyl-terminated hydrogenated polybutadiene, hexamethylene diisocyanate, dibutyltin dilaurate, and dichloromethane are added to a flask to obtain the first mixture.

[0083] S2. Stir the first mixture at 25°C for 3 hours;

[0084] S3. Subsequently, epoxidized soybean oil and 4-dimethylaminopyridine were added to the flask and mixed to obtain a second mixture.

[0085] S4. The second mixture is poured into a polytetrafluoroethylene mold in a vacuum environment and cured at 170°C for 2 hours to obtain a polyurethane elastomer material with low thermal resistance and high adhesion.

[0086] Example 2

[0087] This embodiment provides a polyurethane elastomer comprising the following raw materials: hydroxyl-terminated polyolefin, diisocyanate, epoxy monomer, first catalyst, second catalyst, and solvent;

[0088] Among them, the hydroxyl-terminated polyolefin is hydroxyl-terminated hydrogenated polybutadiene;

[0089] The diisocyanate is hexamethylene diisocyanate;

[0090] The epoxy monomer is epoxidized soybean oil;

[0091] The first catalyst is dibutyltin dilaurate;

[0092] The second catalyst is 4-dimethylaminopyridine;

[0093] The solvent is dichloromethane;

[0094] In the hydroxyl-terminated polyolefin, the molar ratio of hydroxyl groups to isocyanates in the diisocyanate is 1.1:1.

[0095] The molar amount of the first catalyst is 0.5% of the molar amount of isocyanate in the diisocyanate;

[0096] The molar ratio between the hydroxyl-terminated polyolefin and the solvent is 1:0.4;

[0097] The molar ratio between the hydroxyl-terminated polyolefin and the epoxy monomer is 1:0.15;

[0098] The molar amount of the second catalyst is 2.5% of the molar amount of the epoxy monomer.

[0099] The above-mentioned method for preparing polyurethane elastomer includes the following steps:

[0100] S1. Hydroxyl-terminated hydrogenated polybutadiene, hexamethylene diisocyanate, dibutyltin dilaurate, and dichloromethane are added to a flask to obtain the first mixture.

[0101] S2. Stir the first mixture at 25°C for 3 hours;

[0102] S3. Subsequently, epoxidized soybean oil and 4-dimethylaminopyridine were added to the flask and mixed to obtain a second mixture.

[0103] S4. The second mixture is poured into a polytetrafluoroethylene mold in a vacuum environment and cured at 170°C for 2 hours to obtain a polyurethane elastomer material with low thermal resistance and high adhesion.

[0104] Example 3

[0105] This embodiment provides a polyurethane elastomer comprising the following raw materials: hydroxyl-terminated polyolefin, diisocyanate, epoxy monomer, first catalyst, second catalyst, and solvent;

[0106] Among them, the hydroxyl-terminated polyolefin is hydroxyl-terminated hydrogenated polybutadiene;

[0107] The diisocyanate is hexamethylene diisocyanate;

[0108] The epoxy monomer is epoxidized soybean oil;

[0109] The first catalyst is dibutyltin dilaurate;

[0110] The second catalyst is 4-dimethylaminopyridine;

[0111] The solvent is dichloromethane;

[0112] In the hydroxyl-terminated polyolefin, the molar ratio of hydroxyl groups to isocyanates in the diisocyanate is 1.1:1.

[0113] The molar amount of the first catalyst is 0.5% of the molar amount of isocyanate in the diisocyanate;

[0114] The molar ratio between the hydroxyl-terminated polyolefin and the solvent is 1:0.4;

[0115] The molar ratio between the hydroxyl-terminated polyolefin and the epoxy monomer is 1:0.25;

[0116] The molar amount of the second catalyst is 2.5% of the molar amount of the epoxy monomer.

[0117] The above-mentioned method for preparing polyurethane elastomer includes the following steps:

[0118] S1. Hydroxyl-terminated hydrogenated polybutadiene, hexamethylene diisocyanate, dibutyltin dilaurate, and dichloromethane are added to a flask to obtain the first mixture.

[0119] S2. Stir the first mixture at 25°C for 3 hours;

[0120] S3. Subsequently, epoxidized soybean oil and 4-dimethylaminopyridine were added to the flask and mixed to obtain a second mixture.

[0121] S4. The second mixture is poured into a polytetrafluoroethylene mold in a vacuum environment and cured at 170°C for 2 hours to obtain a polyurethane elastomer material with low thermal resistance and high adhesion.

[0122] Example 4

[0123] This embodiment provides a polyurethane elastomer comprising the following raw materials: hydroxyl-terminated polyolefin, diisocyanate, epoxy monomer, first catalyst, second catalyst, and solvent;

[0124] Among them, the hydroxyl-terminated polyolefin is hydroxyl-terminated hydrogenated polybutadiene;

[0125] The diisocyanate is hexamethylene diisocyanate;

[0126] The epoxy monomer is epoxidized soybean oil;

[0127] The first catalyst is dibutyltin dilaurate;

[0128] The second catalyst is 4-dimethylaminopyridine;

[0129] The solvent is dichloromethane;

[0130] In the hydroxyl-terminated polyolefin, the molar ratio of hydroxyl groups to isocyanates in the diisocyanate is 1.1:1.

[0131] The molar amount of the first catalyst is 0.5% of the molar amount of isocyanate in the diisocyanate;

[0132] The molar ratio between the hydroxyl-terminated polyolefin and the solvent is 1:0.4;

[0133] The molar ratio between the hydroxyl-terminated polyolefin and the epoxy monomer is 1:0.35;

[0134] The molar amount of the second catalyst is 2.5% of the molar amount of the epoxy monomer.

[0135] The above-mentioned method for preparing polyurethane elastomer includes the following steps:

[0136] S1. Hydroxyl-terminated hydrogenated polybutadiene, hexamethylene diisocyanate, dibutyltin dilaurate, and 10 mL of dichloromethane were added to a flask to obtain the first mixture.

[0137] S2. Stir the first mixture at 25°C for 3 hours;

[0138] S3. Subsequently, 0.7g of epoxidized soybean oil and 4-dimethylaminopyridine were added to the flask and mixed to obtain a second mixture.

[0139] S4. The second mixture is poured into a polytetrafluoroethylene mold in a vacuum environment and cured at 170°C for 2 hours to obtain a polyurethane elastomer material with low thermal resistance and high adhesion.

[0140] Comparative Example 1

[0141] This comparative example provides a polyurethane elastomer comprising the following raw materials: hydroxyl-terminated polyolefin, diisocyanate, a first catalyst, and a solvent;

[0142] Among them, the hydroxyl-terminated polyolefin is hydroxyl-terminated hydrogenated polybutadiene;

[0143] The diisocyanate is hexamethylene diisocyanate;

[0144] The first catalyst is dibutyltin dilaurate;

[0145] The solvent is dichloromethane;

[0146] In the hydroxyl-terminated polyolefin, the molar ratio of hydroxyl groups to isocyanates in the diisocyanate is 1.1:1.

[0147] The molar amount of the first catalyst is 0.5% of the molar amount of isocyanate in the diisocyanate;

[0148] The molar ratio between the hydroxyl-terminated polyolefin and the solvent is 1:0.4.

[0149] The above-mentioned method for preparing polyurethane elastomer includes the following steps:

[0150] S1. Hydroxyl-terminated hydrogenated polybutadiene, hexamethylene diisocyanate, dibutyltin dilaurate, and dichloromethane are added to a flask to obtain a mixture;

[0151] S2. Stir the mixture at 25°C for 3 hours;

[0152] S3. Pour the mixture from S2 into a polytetrafluoroethylene mold under vacuum and cure at 170°C for 2 hours to obtain a polyurethane elastomer material with low thermal resistance and high adhesion.

[0153] Performance testing

[0154] Test methods

[0155] (1) Thermal resistance test:

[0156] The transient method for determining vertical thermal conductivity uses a photothermal thermal resistance testing system. The specific steps are as follows: The principle involves irradiating the sample surface with a modulated laser beam, directly heating the sample and causing periodic changes in the sample surface temperature. The vertical thermal conduction / diffusion of the entire sample has a significant impact on this surface temperature change, which is obtained by measuring surface thermal radiation.

[0157] (2) Adhesion test:

[0158] The adhesive properties of the samples were measured using a Shimadzu universal testing machine (SUNS UTM4000). Overlap shear bonding tests were performed on Si surfaces with an overlap area of ​​25.4 mm × 10 mm. Specifically, molten sample was directly applied to the Si surface; then, another Si sheet was placed on top, held together for 1 minute, and hot-pressed at 170°C for 2 hours. The load force and displacement during the tensile process were recorded. The point of highest load force was the adhesive force, and the integral of the load force over the displacement was the adhesive work.

[0159] The thermal resistance and adhesive work of the polyurethane elastomers prepared in Examples 1-4 and Comparative Example 1 were tested according to the above method. The test results are shown in Table 1.

[0160] Table 1 - Properties of the polyurethane elastomers prepared in Examples 1-4 and Comparative Example 1

[0161] <![CDATA[Thermal resistance (×10 -6 m 2 ·K·W -1 )]]> <![CDATA[Work of adhesion (J·m -2 )]]> Comparative Example 1 1.34 8287 Example 1 0.89 13535 Example 2 0.39 6809 Example 3 1.08 5808 Example 4 1.43 3168

[0162] As can be seen from Table 1, when the molar ratio of hydroxyl-terminated polyolefin to epoxy monomer in Example 1 was 1:0.05, the thermal resistance of the prepared polyurethane elastomer was 0.89 × 10⁻⁶. -6 m 2 ·K·W -1 The bonding work is 13535 J·m -2 A polyurethane elastomer with high adhesive work and low thermal resistance was prepared.

[0163] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A polyurethane elastomer, characterized in that, Including the following raw materials: hydroxyl-terminated polyolefins, Diisocyanate, epoxy monomer, first catalyst, second catalyst, and solvent; Wherein, the molar ratio between the hydroxyl-terminated polyolefin and the epoxy monomer is 1:(0.01~0.1); The epoxy monomer includes at least one of epoxidized soybean oil, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, glycerol triglycidyl ether, and trimethylolpropane triglycidyl ether. The first catalyst comprises at least one of dibutyltin dilaurate, stannous isooctanoate, triethylenediamine, and N,N-dimethylcyclohexylamine; the second catalyst comprises at least one of benzyldimethylamine, imidazole, boron trifluoride complex, and 4-dimethylaminopyridine. The molar ratio of hydroxyl groups in the hydroxyl-terminated polyolefin to isocyanates in the diisocyanate is (1.1~2):1; the molar amount of the first catalyst is 0.1~5% of the molar amount of isocyanates in the diisocyanate; the molar ratio between the hydroxyl-terminated polyolefin and the solvent is 1:(0.1~10); the molar amount of the second catalyst is 1~10% of the molar amount of the epoxy monomer.

2. The polyurethane elastomer according to claim 1, wherein, The hydroxyl-terminated polyolefin includes at least one of hydroxyl-terminated polyethylene, hydroxyl-terminated polypropylene, hydroxyl-terminated polybutadiene, hydroxyl-terminated hydrogenated polybutadiene, hydroxyl-terminated polyisoprene, and hydroxyl-terminated hydrogenated polyisoprene.

3. The polyurethane elastomer of claim 1, wherein, The diisocyanate includes at least one of isophthalic diisocyanate, toluene-2,4-diisocyanate, terephthalic diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate.

4. The polyurethane elastomer of claim 1, wherein, The solvent includes at least one of dichloromethane, trichloromethane, toluene, and tetrahydrofuran.

5. A process for the preparation of a polyurethane elastomer as claimed in any one of claims 1 to 4, characterised in that, Includes the following steps: Hydroxyl-terminated polyolefin, diisocyanate, first catalyst, and solvent are mixed, then epoxy monomer and second catalyst are added, and the mixture is cured to obtain polyurethane elastomer.

6. The method of producing a polyurethane elastomer according to claim 5, wherein Hydroxyl-terminated polyolefin, diisocyanate, first catalyst, and solvent are mixed at 25-80°C, epoxy monomer and second catalyst are added, and cured at 150-200°C for 1-6 hours to obtain polyurethane elastomer.

7. The application of the polyurethane elastomer as described in any one of claims 1 to 4 or the polyurethane elastomer prepared by the preparation method described in any one of claims 5 to 6 as an interface material in electronic products.

Citation Information

Patent Citations

  • Blood environment self-healing polyurethane elastomer as well as preparation method and application thereof

    CN114957592A

  • Preparation method of high-performance integrated polyurethane elastomer auxetic material

    CN115651157A