Adhesive tape, items, and methods for removing items.

By introducing a high volume resistivity heating element into the adhesive tape, the adhesive layer is melted or softened by resistance heating, which solves the problems of inconvenient disassembly and thermal degradation in the prior art, and realizes fast and safe disassembly of the adhesive tape.

CN117580920BActive Publication Date: 2026-11-17DIC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202280046180.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-07-09
Filing Date
2022-07-07
Publication Date
2026-11-17
Estimated Expiration
2042-07-07

AI Technical Summary

Technical Problem

Existing methods for removing adhesive tape require external heating devices and are difficult to heat evenly, which can easily lead to thermal degradation, especially in electronic components, affecting reuse efficiency.

Method used

Using a heating element with a volume resistivity of 30 μΩ·cm or higher, the adhesive layer is melted or softened by resistance heating, enabling rapid peeling of the adhesive tape and avoiding thermal damage to the adhered objects.

Benefits of technology

It enables heat-based peeling in a short time, preventing thermal damage to the adhered material, simplifying the disassembly process, and is suitable for complex environments such as electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117580920B_ABST
    Figure CN117580920B_ABST
Patent Text Reader

Abstract

This invention provides an adhesive tape that can be peeled off by heat in a short time, prevents thermal damage to the adhered objects, and is easy to peel off by heat. The adhesive tape has an adhesive layer A comprising a heating element and an adhesive. The volume resistivity of the heating element is 30 μΩ·cm or higher. By resistive heating, the adhesive layer A melts or softens, thereby enabling peeling. Preferably, the adhesive is at least one of pressure-sensitive adhesive and hot-melt adhesive, and the heating element is selected from the group consisting of nickel-chromium alloy, stainless steel, titanium, nickel-silver, and carbon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive tape (the Japanese term for "adhesive" is "nenchaku"), an article, and a method for disassembling an article. Background Art

[0002] Adhesive tapes are used as joining means with excellent workability and high bonding reliability, for applications such as component fixing, temporary component fixing, and labels for displaying product information in various industrial fields including OA equipment, IT products, home appliances, and automobiles. In recent years, from the viewpoint of protecting the global environment, the demand for recycling and reusing used products has increased in various industrial fields such as home appliances and automobiles. When recycling and reusing various products, it is necessary to perform the operation of peeling off the adhesive tapes used for fixing components and labels. However, since adhesive tapes are provided in various places in products, it is desired to reduce operation costs through a simple removal process.

[0003] In order to separate adherends from each other, for example, a hot-melt adhesive composition that rapidly dissolves in a short time by electromagnetic induction heating has been proposed (for example, see Patent Document 1). As a method for separating adherends from each other, a building disassembly method has been proposed, in which a metal base material is heated using an electromagnetic induction heating device, the adhesive between the base material and the interior material is heated and foamed to peel off, and the interior material is peeled from the metal base material (for example, see Patent Document 2). In addition, a double-sided adhesive tape has been proposed which has a thermally conductive layer that can be easily disassembled by contacting a heat generating source and directly heating the thermally conductive layer (for example, see Patent Document 3). Prior Art Documents Patent Documents

[0004] Patent Document 1: Japanese Unexamined Patent Application Publication No. 2002-188068 Patent Document 2: Japanese Unexamined Patent Application Publication No. 2006-200279 Patent Document 3: Japanese Unexamined Patent Application Publication No. 2016-108394 Summary of Invention

[0005] However, in the conventional methods for peeling and disassembling by heating, it is necessary to use an external device as a heating unit such as electromagnetic induction heating or a heat generating source, which poses the problem of enlarged scale of the disassembly operation. In addition, when the heating method is electromagnetic induction heating or infrared heating, since heat is applied from the outside, there is a problem that when heating an adhesive tape wrapped around by a component, the adhesive tape is not sufficiently heated, and it is difficult to adjust the heating to a temperature at which the adhesive tape can be peeled off. In particular, in electronic components that are completely shielded from the outside, it is difficult to heat only the adhesive tape, and when heating takes time, there arises a problem that the adherends are exposed to high temperatures and cause thermal degradation.

[0006] Therefore, in adhesive tapes that fix rigid bodies or other adhered objects to each other, it is desirable to have an adhesive tape that can disassemble and reuse the parts that are adhered objects. In particular, an adhesive tape that can be easily disassembled and peeled off by heating is required.

[0007] The objective of this invention is to solve the aforementioned problems and achieve the following: that is, to provide an adhesive tape, article, and method for removing the article that can be peeled off by heating in a short time, prevents heat damage to the adhered material, and facilitates the heating-peeling operation. Technical solutions for solving technical problems

[0008] This invention was made based on the above-described insights of the inventors, and the means for solving the aforementioned technical problems are as follows. That is, <1> An adhesive tape, characterized in that the adhesive tape has an adhesive layer A comprising a heating element and an adhesive, wherein the volume resistivity of the heating element is 30 μΩ·cm or more, and the adhesive layer A melts or softens by resistance heating, thereby enabling peeling. <2> According to the above <1> The described adhesive tape, wherein the adhesive is at least one of pressure-sensitive adhesive and hot melt adhesive. <3> According to the above <1> ~ <2> The heating element described in any one of the above is selected from the group consisting of nickel-chromium alloy, stainless steel, titanium, nickel-silver and carbon. <4> According to the above <1> ~ <3> The adhesive layer described in any one of the claims, wherein the adhesive layer A is a laminate having a planar heating element and adhesive layers a1 and a2 on each surface of the heating element, wherein at least one of the adhesive layers a1 and a2 is melted or softened by resistance heating, thereby enabling peeling. <5> According to the above <4> The described adhesive tape, in a top view, has a planar heating element having a pair of protrusions extending from the outer peripheries of the adhesive layer a1 and the adhesive layer a2. <6> According to the above <1> ~ <3> The adhesive tape described in any one of the above, wherein the adhesive layer A is composed of a single layer comprising the heating element and the adhesive. <7> According to the above <1> ~ <6> The adhesive tape described in any one of the above describes a temperature range in which the temperature at which the loss tangent tanδ of the adhesive layer formed by the adhesive reaches 0.45 or higher is located between 80°C and 200°C. <8> An article, characterized in that the article comprises at least two adhered objects and a space between the two adhered objects. <1> ~ <7> The adhesive tape described in any one of the above describes the bonding of two of the aforementioned objects. <9> According to the above <8> The described article, in a top view, has a pair of protrusions extending from the outer periphery of the object to be adhered to. <10> According to the above <8> or <9> The method for disassembling the items described herein involves electrically connecting the adhesive layer A to a power source, supplying electricity to the heating element from the power source, and softening or melting the adhesive layer A through resistance heating, thereby separating the two adhered objects. <11> According to the above <10> The method for disassembling the described item, wherein the power source is an external power source. <12> According to the above <10> The described method for disassembling an item is as follows: the item is an electronic device or a component built into an electronic device; the power source is the driving power source of the electronic device; the adhesive layer A is electrically connected to the driving power source and circuit of the electronic device; electricity is supplied from the driving power source to the heating element; and the adhesive layer A is melted or softened by resistance heating, thereby separating the two adhered objects. (Invention Effects)

[0009] According to the present invention, the aforementioned problems can be solved and the above-mentioned objectives can be achieved. An adhesive tape, article, and method for removing the article can be provided that can be peeled off by heating in a short time, can prevent heat damage to the adhered object, and is easy to peel off by heating. Attached Figure Description

[0010] Figure 1A This is a schematic cross-sectional view showing an example of the adhesive tape of the present invention. Figure 1B This is a schematic cross-sectional view showing another example of the adhesive tape of the present invention. Figure 1C This is a schematic top view illustrating another example of the adhesive tape of the present invention. Figure 1D This is a schematic top view showing an example of a pattern of the heating element in the adhesive tape of the present invention. Figure 2 This is a schematic cross-sectional view showing another example of the adhesive tape of the present invention. Figure 3 This is a schematic cross-sectional view showing another example of the adhesive tape of the present invention. Figure 4A This is a schematic top view illustrating an example of the article of the present invention. Figure 4B This is a schematic cross-sectional view showing an example of the article of the present invention. Figure 5This is a schematic cross-sectional view showing another example of the article of the present invention. Figure 6 This is a schematic diagram illustrating a method for disassembling the article of the present invention. Figure 7A This is a schematic top view of the adhesive tape of Example 1. Figure 7B This is a schematic cross-sectional view of the adhesive tape of Example 1. Figure 8A This is a schematic top view illustrating the article and evaluation method of Embodiment 1. Figure 8B This is a schematic front view illustrating the article and evaluation method of Embodiment 1. Figure 8C This is a schematic side view showing the article and evaluation method of Embodiment 1. Detailed Implementation

[0011] In this specification, "adhesive" refers to a type of bonding that occurs through pressure, also known as "pressure-sensitive adhesive." Correspondingly, "adhesive" refers to an adhesive that combines the properties of both liquids and solids, possesses tack, and exerts its bonding effect through pressure; also known as "pressure-sensitive adhesive."

[0012] 1. Adhesive tape The adhesive tape of the present invention has at least an adhesive layer A comprising a heating element and an adhesive, and may also have other layers such as a release layer. The adhesive tape of the present invention is an adhesive tape that can be peeled off by melting or softening the adhesive layer A through resistance heating.

[0013] The adhesive tape of the present invention can be used as an easily detachable adhesive tape, which, after being pasted onto the adhered objects and used to fix the adhered objects together, can be easily detached after a certain period of time. Specifically, by electrically connecting the adhesive layer A to a power source and applying voltage to the heating element to turn on the power, the heating element and its surroundings are heated using a resistance heating method. As a result, the adhesive or any melt-softening layer in the adhesive layer A softens or melts, releasing the adhesive state at a desired location within or within the adhesive layer A itself. The adhesive layer A can then be peeled off, and the adhered objects can be detached. In the adhesive tape of the present invention, since current is directly applied to the heating element during disassembly, the current amount and other parameters are easily adjusted. By using a heating element with a given volume resistivity, heating and peeling can be performed in a short time. Compared to conventional heating methods that utilize electromagnetic induction or infrared heating, the adhesive tape of this invention heats only the interior of the tape. Therefore, even when the tape is wound around a part, heating adjustment is easy, preventing overheating of the adhered object. Furthermore, when the adhesive tape is thermally removed using a driving current from an electronic component, thermal degradation of the circuitry within the part can be prevented. Specifically, by using a heating element with a given volume resistivity, the adhesive tape of this invention prevents excessive temperature rise in the electronic circuitry within the part and the connection points between the circuitry and the adhesive tape when energized by a driving current from an electronic component.

[0014] In the adhesive tape of the present invention, "melting or softening the adhesive layer A by resistance heating" means that the entire adhesive layer A can be melted or softened by resistance heating, or a portion of the adhesive layer A can be melted or softened by resistance heating. The melting or softening of a portion of the adhesive layer A means, for example, in the case where the adhesive layer A is a laminate as described later, one or more layers constituting the laminate can be melted or softened.

[0015] Furthermore, the phrase "the adhesive tape of the present invention becomes peelable by melting or softening the adhesive layer A through resistance heating" can refer to the following methods: melting or softening the entire adhesive layer A through resistance heating, thereby making the adhesive layer A in the adhesive tape a single unit and peelable from the adhered object; melting or softening one or more layers constituting the adhesive layer A through resistance heating, thereby making the adhesive layer A in the adhesive tape a single unit and peelable from the adhered object; or melting or softening one or more layers constituting the adhesive layer A through resistance heating, causing peeling within the adhesive layer A, thereby making a portion of the adhesive layer A in the adhesive tape peelable from the adhered object.

[0016] The phrase "containing adhesive" in the above-mentioned adhesive layer A means that adhesive layer A can be a single layer containing adhesive throughout, or it can be a laminate containing multiple layers, with adhesive contained in at least one of the multiple layers constituting the laminate. For example, as described later, when adhesive layer A has two adhesive layers a (e.g., adhesive layers a1 and a2), the two adhesive layers a (e.g., adhesive layers a1 and a2) can each contain the same or different adhesives. Furthermore, when adhesive layer A has adhesive layer a, heating element b, and melt softening layer c, adhesive layer a can contain adhesive, and melt softening layer c can also contain adhesive. The same applies when there are two melt softening layers c (e.g., melt softening layers c1 and c2). It should be noted that when adhesive layer A is a laminate, sometimes adhesive layers a1 and a2 constituting adhesive layer A are collectively referred to as adhesive layer a, and sometimes melt-softening layers c1 and c2 are collectively referred to as melt-softening layer c. Adhesive layer a, heating element b, and melt-softening layer c will be described in detail later.

[0017] <Adhesive Layer A> The aforementioned adhesive layer A contains at least a heating element and an adhesive, and may contain other components as needed. The aforementioned adhesive layer A is a layer with adhesive properties on both sides, and may be a single layer or comprise multiple layers.

[0018] The adhesive layer A described above having adhesive properties on both sides means that both sides of the adhesive layer A have pressure-sensitive adhesive properties, both sides of the adhesive layer A have heat-adhesive properties, or one side of the adhesive layer A has pressure-sensitive adhesive properties and the other side has heat-adhesive properties. When both sides of the adhesive layer A have pressure-sensitive adhesive properties, it can easily bond to the adhered object and other layers constituting the adhesive tape of the present invention at room temperature, and can firmly bond before being resistively heated, therefore this is preferred.

[0019] <<Fever Body>> There are no particular limitations on the heating element used, and any known heating element for resistance heating can be appropriately selected according to the purpose. The volume resistivity of the heating element at room temperature (20°C) is 30 μΩ·cm or more, preferably 50 μΩ·cm or more, more preferably 70 μΩ·cm or more, and particularly preferably 100 μΩ·cm or more. Furthermore, there is no particular upper limit to the volume resistivity of the heating element, but if the volume resistivity is too high, a high voltage is required when energized. Therefore, the volume resistivity is preferably 100,000 μΩ·cm or less, more preferably 20,000 μΩ·cm or less, more preferably 10,000 μΩ·cm or less, and particularly preferably 5,000 μΩ·cm or less. Specifically, the volume resistivity of the heating element can be set within the ranges of 30 μΩ·cm to 100,000 μΩ·cm, 50 μΩ·cm to 20,000 μΩ·cm, 70 μΩ·cm to 10,000 μΩ·cm, and 100 μΩ·cm to 5,000 μΩ·cm. Here, "resistive heating" refers to an electric heating method in which an electric current is passed through a resistive conductor (heating element), and the conductor is heated by its Joule heat. If a constant current is passed through the conductor, the amount of Joule heat generated within a certain time is proportional to the square of the current and the resistance of the conductor (Joule's law). The conductor has an inherent resistance value (volume resistivity, etc.). By setting the volume resistivity of the heating element to 30 μΩ·cm or higher, when disassembling an item, or when connecting it to the wiring circuit within an electronic device and energizing the heating element with the drive current of the electronic device, only the adhesive tape can be heated, preventing high-temperature deterioration of the wiring circuit. Furthermore, by using a heating element with a given volume resistivity, the adhesive layer A can be melted or softened in a short time, thus shortening the disassembly time. Moreover, by using a heating element with a given volume resistivity, especially when using drive current within electronic components, overheating of electronic circuits and connections can be prevented in order to energize the heating element, thereby preventing thermal degradation of the electronic components.

[0020] There are no particular limitations on the heating element used, and any known heating element can be appropriately selected according to the purpose, such as metals or non-metals. Examples of metals include nickel-chromium alloys (108 μΩ·cm); stainless steels such as SUS 410 (62.2 μΩ·cm), SUS 304 (72.0 μΩ·cm), and SUS 430 (60.0 μΩ·cm); titanium (55.0 μΩ·cm); and nickel silver (for example, 34.0 μΩ·cm in "Yangbai C7701" manufactured by Takeuchi Metal Foil Powder Industry Co., Ltd.). It should be noted that the values ​​in parentheses represent the approximate volume resistivity of each material at 20°C. Examples of non-metals include carbon nanomaterials such as graphite, graphene, graphene oxide, carbon nanotubes, graphene platelets, and carbon nanofibers (for example, 3352 μΩ·cm). Among these, nickel-chromium alloys and stainless steel are preferred from the perspectives of being difficult to break when made into metal foils, easy to process as tape, and capable of melting or softening the adhesive layer in a short time to significantly reduce adhesive strength. Furthermore, carbon is preferred from the perspectives of exhibiting high volume resistivity, being easy to form into thin films, and not compromising the required properties of the tape, such as conformability. Among these, carbon nanomaterials such as carbon nanotubes are preferred because their rod-like shape readily exhibits conductivity even in small quantities, enabling the adhesive layer A to melt or soften quickly due to resistance heating.

[0021] The volume resistivity of the aforementioned heating element was measured at 20°C using a low resistivity meter (manufactured by Nitto Seiko Analytech Co., Ltd., trade name: "Loresta-AX MCT-T370") and a four-probe probe (manufactured by Nitto Seiko Analytech Co., Ltd., trade name: "ASP probe MCP-TP03P"), according to JIS K 7194. The measurement point was set to 1 point, and a resistivity correction factor of 4.532 was used.

[0022] As for the shape of the heating element, there are no particular limitations as long as the heating elements are in electrical contact with each other in a way that generates resistance heating. The shape can be appropriately selected according to the purpose, for example, planar, mesh, granular, and fibrous shapes. Among these, a planar shape is preferred from the perspective of being able to fully adhere to other layers in contact with the heating element before energizing, and heating the surface when energized, so that the heating element itself is not easily damaged or broken when disassembled after energizing. Examples of planar heating elements include: metal foil containing the aforementioned metal, sheets of the aforementioned non-metal, resin sheets with high-density dispersion of particles or fibers containing the aforementioned metal or non-metal, coatings of the aforementioned metal or non-metal, sheets of the aforementioned metal or non-metal impregnated in nonwoven fabric, and nonwoven fabrics of the aforementioned metal or non-metal. Even among these planar heating elements, from the perspective of being able to heat the entire surface through high volume resistance and not easily broken, metal foil, non-metal sheets, coatings of metal or non-metal, or nonwoven fabrics of metal or non-metal are further preferred, and metal foil is more preferred.

[0023] In the top view of the adhesive tape, the planar heating element can cover the entire surface of the adhesive layer or only a portion of it. Furthermore, the planar heating element can be patterned, or it can be in the form of a strip or line (see also the following description). Figure 1D If the heating element is strip-shaped or wire-shaped, it has high heating efficiency and a small contact area with the adhered object, thus offering advantages in terms of ease of peeling. In this case, the length (bandwidth or linewidth) of the heating element along its short axis is preferably 0.5 mm to 20 mm, more preferably 1 mm to 10 mm, and even more preferably 2 mm to 5 mm.

[0024] If the planar heating element is patterned (has a patterned shape), the distance between the terminals (terminals for connection to the power supply) of the heating element can be increased, thereby increasing the resistance. Therefore, the heating efficiency of the planar heating element is higher, and the adhesive tape of the present invention can be peeled off in a short time. In the case where the planar heating element is patterned, the line width of the pattern is not particularly limited and can be within the same preferred range as the bandwidth or line width described above.

[0025] In planar heating elements, the heating element can be disposed on one or both sides of the substrate. When the heating element is disposed on one or both sides of the substrate, it can be disposed to cover the entire area of ​​one or both sides of the substrate, or it can be disposed in a linear, strip-like, or patterned manner. When the planar heating element is disposed on one or both sides of the substrate, it is disposed in direct contact with one or both sides of the substrate. As for the aforementioned substrate, there are no particular limitations as long as it can support the heating element; from the viewpoints of adhesive tape conformability and thin-film properties, a resin film is preferred. For example, common films such as polyethylene terephthalate (PET) film, polyethylene naphthalate (PEN) and other polyester resin films, imide resin films such as polyimide (PI) film, and polyolefin resin films such as polypropylene (PP) film can be used. Alternatively, a resin film used for the melt softening layer described later can also be used.

[0026] Examples of mesh-like heating elements include integrally formed heating elements such as heating elements with multiple through holes on the surface-shaped heating element, mesh-like or grid-like heating elements, etc.

[0027] Furthermore, regarding the shape of the heating element, even if the heating element is not integrally formed, as long as the heating elements can make electrical contact with each other, it can be, for example, particles or fibers containing the aforementioned metal or non-metal. By dispersing the granular or fibrous heating element in the adhesive, electrical contact between the heating elements can be formed even if the heating element is not integrally formed. When the granular or fibrous heating element is dispersed in the adhesive, there is no particular limitation on the content of the particles or fibers, as long as electrical contact between the heating elements can be formed, and it can be appropriately selected according to the purpose. Relative to the total amount of the adhesive, it is preferably 20% to 95% by mass, more preferably 40% to 90% by mass. When the adhesive layer A is a monolayer formed of adhesive and the monolayer contains the heating element, the content of particles or fibers can be set to the content relative to the total amount of adhesive layer A. In addition, when the adhesive layer A is a laminate, and one of the layers constituting the laminate has an adhesive layer a in which particles or fibers of the heating element are dispersed, the content of particles or fibers can be set to the content relative to the total amount of one adhesive layer a.

[0028] The average thickness of the planar heating element is not particularly limited and can be appropriately selected according to the purpose. Preferably, it is 1μm to 200μm, more preferably 2μm to 200μm, more preferably 3μm to 150μm, more preferably 5μm to 150μm, more preferably 5μm to 100μm, even more preferably 10μm to 100μm, and preferably 10μm to 50μm. The average thickness of the planar heating element is the average value obtained by measuring the thickness at five or more randomly selected locations. The greater the average thickness of the planar heating element, the greater the current flow and heat generation, but from the viewpoint of the adhesive tape's followability and adhesion operability, the thickness is limited. In contrast, if the average thickness of the planar heating element is within the above range, sufficient current flow and heat generation can be obtained, the heating element can be effectively heated by resistance heating, and excellent adhesive tape followability and adhesion operability can be obtained.

[0029] It should be noted that when the planar heating element is arranged on one or both sides of the substrate, the average thickness of the planar heating element refers to the thickness excluding the resin film. When the heating element is formed on both sides of the resin film, it refers to the thickness of the heating element on each single side.

[0030] As the heating element mentioned above, a suitably manufactured heating element or a commercially available product can be used. As for the aforementioned commercially available products, there are no particular restrictions, and appropriate selections can be made according to the purpose. For example, nickel-chromium alloy foils such as NCH1-H; stainless steel foils such as SUS304-H and SUS430-H; titanium foils such as TR270C-H; and nickel silver such as C7701 (all of which are manufactured by Takeuchi Metal Foil Powder Industry Co., Ltd.) can be used as surface heating elements. In addition, heating elements formed by patterning these materials can also be used.

[0031] <<Adhesives>> There are no particular limitations on the adhesive used, and it can be appropriately selected according to the purpose, but at least one of pressure-sensitive adhesive and hot-melt adhesive is preferred. By setting the adhesive included in adhesive layer A to a pressure-sensitive adhesive containing hot-melt adhesive and thermoplastic resin, since the resin can melt or soften by the heat generated by the electric current, it is advantageous that it can be peeled off even without mixing components that cause the starting point of peeling at the adhesive interface, such as heating foaming agents, or components that reduce adhesive strength. In addition, the adhesive preferably has a softening point, which is advantageous in that it becomes rapidly softer and exhibits high deformability and fluidity when heated to a temperature higher than the softening point.

[0032] The adhesive described above melts or softens the resin when heated, resulting in a lower adhesive strength during heating compared to that at room temperature.

[0033] The storage modulus G of the above-mentioned adhesive (the adhesive layer formed by the above-mentioned adhesive) was determined by dynamic viscoelastic spectra at 1 Hz and 23°C. 23 From the viewpoint of ensuring that the adhered objects are well fixed to each other under normal conditions, a 1.0 × 10⁻⁶ ohmmeter is preferred. 3 Pa ~ 1.0 × 10 9 Pa, wherein, preferably, 1.0 × 10 Pa. 3 Pa ~ 5.0 × 10 7 Pa, more preferably 5.0 × 10 Pa 3 Pa ~ 5.0 × 10 7 Pa, further optimized to 5.0 × 10 3 Pa ~ 5.0 × 10 6 Pa, preferably 5.0 × 10 Pa. 3 Pa ~ 1.0 × 10 6 Pa.

[0034] In the case where the adhesive is a pressure-sensitive adhesive (adhesive), the storage modulus G of the pressure-sensitive adhesive (pressure-sensitive adhesive layer) is measured using dynamic viscoelastic spectra at 1 Hz and 23°C. 23 From the viewpoint of ensuring that the adhered objects are well fixed together under normal conditions (without resistance heating), the aforementioned storage modulus G... 23 Within the range, 1.0 × 10 is preferred. 3 Pa ~ 5.0 × 10 7 Pa, more preferably 5.0 × 10 Pa 3 Pa ~ 5.0 × 10 6 Pa, further optimized to 5.0 × 10 3 Pa ~ 1.0 × 10 6 Pa.

[0035] Furthermore, when the aforementioned adhesive is a hot melt adhesive, the storage modulus G of the aforementioned hot melt adhesive (hot melt adhesive layer) is measured using dynamic viscoelastic spectra at 1 Hz and 23°C. 23 From the viewpoint of ensuring good adhesion between the adhered objects under normal conditions (without resistance heating), a 1.0 × 10⁻⁶ ohmmeter is preferred. 3 Pa ~ 1.0 × 10 9 Pa, more preferably 5.0 × 10 Pa 3 Pa ~ 5.0 × 10 8 Pa, further preferred to be 1.0 × 10 4 Pa ~ 1.0 × 10 8 Pa.

[0036] The storage modulus G of the above-mentioned adhesive (the adhesive layer formed by the above-mentioned adhesive) was determined by dynamic viscoelastic spectrum at 1 Hz and 100 °C.100 From the viewpoint that resistive heating makes it easier to separate the adhered materials from each other, 1.0 × 10 is preferred. 0 Pa ~ 5.0 × 10 6 Pa, preferably 1.0 × 10 3 Pa ~ 1.0 × 10 6 Pa, more preferably 1.0 × 10 Pa 3 Pa ~ 1.0 × 10 6 Pa, further optimized to 5.0 × 10 3 Pa ~ 5.0 × 10 5 Pa.

[0037] In the case where the adhesive is a pressure-sensitive adhesive (adhesive), the storage modulus G of the pressure-sensitive adhesive (pressure-sensitive adhesive layer) is determined by dynamic viscoelasticity spectra at 1 Hz and 100 °C. 100 In the above energy storage modulus G 100 Within the range, 1.0 × 10 is preferred. 2 Pa ~ 5.0 × 10 6 Within the range of Pa, 1.0 × 10 Pa is more preferred. 3 Pa ~ 1.0 × 10 6 Within the Pa range, 5.0 × 10 Pa is further preferred. 3 Pa ~ 5.0 × 10 5 Within the range of Pa. This is because, by increasing the storage modulus G of the aforementioned pressure-sensitive adhesive (the adhesive layer formed by the aforementioned pressure-sensitive adhesive), 100 Within the aforementioned range, even when using low current, pressure-sensitive adhesives can melt or soften in a short time through resistance heating, thereby allowing for peeling.

[0038] When the adhesive is a pressure-sensitive adhesive, the above storage modulus G 23 and energy storage modulus G 100 The following method can be used to determine the energy modulus. Using a viscoelasticity testing machine (ARES-G2, manufactured by TA Instruments Japan), a test piece is sandwiched between parallel discs with a diameter of 8 mm, which serve as the measuring section of the same testing machine. The storage modulus G' is measured at a frequency of 1 Hz, a temperature range of -40°C to 200°C, and a heating rate of 2°C / min. The values ​​at 23°C and 100°C are recorded. The test piece uses the following pressure-sensitive adhesive layer (adhesive layer): the pressure-sensitive adhesive is applied using a coater to a dry thickness of approximately 2 mm and dried, then cured as needed.

[0039] Furthermore, when the adhesive is a hot melt adhesive, the aforementioned storage modulus G 23 and energy storage modulus G 100The test piece is clamped between the tensile testing fixtures of the measuring section of a viscoelasticity testing machine, and the storage modulus G' is measured under conditions of 1 Hz frequency, a temperature range of -40℃ to 200℃, and a heating rate of 2℃ / min. The values ​​are recorded at 23℃ and 100℃. The test piece is formed using a hot melt adhesive layer: the hot melt adhesive is applied using a coater to a thickness of approximately 0.1 mm after drying, and then dried and cured as needed.

[0040] The temperature at which the loss tangent (tanδ) of the adhesive (the adhesive layer formed by the adhesive) reaches 0.45 or more is preferably located in the temperature range of 80°C or more and 200°C or less. The temperature at which the loss tangent (tanδ) reaches 0.8 or more is more preferably located in the temperature range of 80°C or more and 200°C or less. The temperature at which the loss tangent (tanδ) reaches 1.0 or more is even more preferably located in the temperature range of 80°C or more and 200°C or less.

[0041] By ensuring that the temperature at which the tanδ of the adhesive (the adhesive layer formed by the adhesive) reaches a predetermined value is located in the temperature range of 80°C or higher and 200°C, the adhesive, when heated to this temperature by a heat source, is prone to plastic deformation due to melting or softening. Furthermore, the cohesive breakdown within the layer formed by the adhesive facilitates easier peeling and disassembly in a shorter time, which is advantageous. As will be described later, when adhesive layer A has adhesive layer a1 and adhesive layer a2, it is preferable that at least one of adhesive layers a1 and a2 has a loss tangent (tanδ) of 0.45 or higher located in the temperature range of 80°C or higher and 200°C.

[0042] It should be noted that the loss tangent (tanδ) is calculated from the storage modulus (G') and loss modulus (G”) obtained by dynamic viscoelasticity measurement based on temperature dispersion, using the formula tanδ = G” / G'. The dynamic viscoelasticity measurement and the aforementioned storage modulus G… 23 and energy storage modulus G 100 The determination method is the same.

[0043] Storage modulus G of the adhesive (the adhesive layer formed using the above-mentioned adhesive) 23 Energy storage modulus G 100The loss tangent (tanδ) can be adjusted by modifying the types and combinations of monomers in the resin (base polymer) that constitutes the main component of the adhesive, the proportions of each monomer, the amount of tackifying resin added as needed, and the amount of crosslinking agent added as needed (gel fraction). The resin (base polymer) that is the main component of the adhesive can be used alone or in combination of two or more. The resin that is the main component of the adhesive will be explained in the "-Resin-" section below. Furthermore, when the adhesive layer contains a heating element, the storage modulus G of the adhesive layer... 23 Energy storage modulus G 100 And the loss tangent (tanδ) is set to the value of the adhesive (adhesive layer) excluding the heating element.

[0044] The melting point of the aforementioned adhesive is preferably 70°C or higher and 150°C or lower, more preferably 75°C or higher and 130°C or lower, and even more preferably 80°C or higher and 110°C or lower. This is because by setting the melting point of the adhesive within the aforementioned range, high adhesive strength can be achieved before energization, and the adhesive can easily melt or soften even with minimal resistance heating caused by energization. The melting point of the aforementioned adhesive can be adjusted by selecting the type of resin as the main component of the adhesive, the content of tackifying resin in the adhesive, the gel fraction, etc. The melting point of the aforementioned adhesive can be set as the temperature of the endothermic peak accompanying melting, as measured using differential scanning calorimetry (DSC).

[0045] <<<Pressure-sensitive adhesives>>> The aforementioned pressure-sensitive adhesive refers to an adhesive that bonds by applying pressure for a short time at room temperature. Pressure-sensitive adhesives are also called adhesives. The aforementioned pressure-sensitive adhesive is viscous at room temperature. There are no particular limitations on the aforementioned pressure-sensitive adhesive; any known pressure-sensitive adhesive can be appropriately selected according to the purpose. Examples include: acrylic-based pressure-sensitive adhesives (acrylic adhesives), urethane-based pressure-sensitive adhesives (urethane adhesives), synthetic rubber-based pressure-sensitive adhesives, natural rubber-based pressure-sensitive adhesives, and other rubber-based pressure-sensitive adhesives (rubber adhesives), silicone-based pressure-sensitive adhesives (silicone adhesives), etc.

[0046] The aforementioned pressure-sensitive adhesive may contain a thermoplastic resin or may contain a non-thermoplastic resin instead of a thermoplastic resin. When the pressure-sensitive adhesive contains a thermoplastic resin, resistance heating melts or softens the adhesive, reducing its adhesive strength and allowing adhesive layer A to be peeled off. When the pressure-sensitive adhesive contains a non-thermoplastic resin instead of a thermoplastic resin, by combining it with at least one of the aforementioned hot-melt adhesive and the melt-softened layer, resistance heating can melt either the hot-melt adhesive or the melt-softened layer, causing adhesive layer A to peel off.

[0047] As described above, the acrylic-based pressure-sensitive adhesive includes acrylic resin, and further includes, as needed, other components such as tackifying resin, crosslinking agent, and antioxidant. As described above, the urethane-based pressure-sensitive adhesive includes urethane resin, and further includes, as needed, other components such as tackifying resin, crosslinking agent, and antioxidant. As described above, the rubber-based pressure-sensitive adhesive includes rubber materials such as styrene resin, and further includes, as needed, other components such as tackifying resin, crosslinking agent, and antioxidant. As described above, the silicone-based pressure-sensitive adhesive includes silicone resin, and further includes, as needed, other components such as tackifying resin, crosslinking agent, and antioxidant.

[0048] <<<Hot Melt Adhesives>>> The aforementioned hot melt adhesive refers to a thermoplastic adhesive that is solid at room temperature but melts upon heating, liquefies, and is applied to the substrates, then solidifies upon cooling to form a bond. This hot melt adhesive can be dissolved in a solvent for coating, cured by drying to form a film, and bonded by applying heat when adhering to the substrates. This hot melt adhesive typically has no tackiness at room temperature or has lower tackiness than pressure-sensitive adhesives. This hot melt adhesive contains a thermoplastic resin, and may further include, as needed, tackifying resins, crosslinking agents, antioxidants, and other components.

[0049] Examples of the aforementioned hot melt adhesives include: ethylene-vinyl acetate copolymer (EVA) based hot melt adhesives, polyolefin based hot melt adhesives, polyamide based hot melt adhesives, polyurethane based hot melt adhesives, acrylic based hot melt adhesives, polyester based hot melt adhesives, and rubber-based hot melt adhesives with styrene-based thermoplastic elastomers as their base.

[0050] -Resin- Examples of resins (base polymers) that can be used as the main component of the aforementioned pressure-sensitive adhesives and hot-melt adhesives include: urethane resins such as polyurethane (PU) and thermoplastic polyurethane (TPU); polycarbonate (PC); vinyl chloride resins such as polyvinyl chloride (PVC) and vinyl chloride-vinyl acetate copolymer; acrylic resins such as polyacrylic acid, polymethacrylic acid, polymethyl acrylate, polymethyl methacrylate (PMMA), polyethyl methacrylate, and acrylic polymers formed by polymerizing one or more (meth)acrylic acid monomers; polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate, polypropylene terephthalate, polyethylene naphthalate, and polybutylene naphthalate; and nylon. Polyamide resins such as Long (registered trademark); polystyrene resins such as polystyrene (PS), imide-modified polystyrene, acrylonitrile-butadiene-styrene (ABS) resin, imide-modified ABS resin, styrene-acrylonitrile copolymer (SAN) resin, and acrylonitrile-ethylene-propylene-diene-styrene (AES) resin; olefin resins such as polyethylene (PE) resin, polypropylene (PP) resin, and cycloolefin resins; cellulose resins such as nitrocellulose and cellulose acetate; silicone resins; thermoplastic resins such as fluorinated resins; thermoplastic elastomers such as styrene thermoplastic elastomers, olefin thermoplastic elastomers, vinyl chloride thermoplastic elastomers, acrylic thermoplastic elastomers, urethane thermoplastic elastomers, ester thermoplastic elastomers, and amide thermoplastic elastomers. These can be used individually or in combination with two or more.

[0051] Among these, thermoplastic resins are preferred, and more preferably, acrylic resins, urethane resins, polyester resins, styrene thermoplastic elastomers, olefin thermoplastic elastomers, vinyl chloride thermoplastic elastomers, acrylic thermoplastic elastomers, ester thermoplastic elastomers, urethane thermoplastic elastomers, amide thermoplastic elastomers, etc., with styrene thermoplastic elastomers being particularly preferred.

[0052] Examples of the aforementioned styrene thermoplastic elastomers include: styrene-ethylene-butene copolymers (SEB) and other styrene-based AB-type diblock copolymers; styrene-butadiene-styrene copolymers (SBS), hydrides of SBS (styrene-ethylene-butene-styrene copolymer (SEBS)), styrene-isoprene-styrene copolymers (SIS), hydrides of SIS (styrene-ethylene-propylene-styrene copolymer (SEPS)), styrene-isobutylene-styrene copolymers (SIBS) and other styrene-based ABA-type triblock copolymers; styrene-butadiene-styrene-butadiene copolymers (SBSB) and other styrene-based ABAB-type tetrablock copolymers; styrene-butadiene-styrene-butadiene copolymers (SBSBS) and other styrene-based ABABA-type pentablock copolymers; styrene-based multiblock copolymers having more than one AB repeating unit; hydrides formed by hydrogenating the ethylene double bonds of styrene-based random copolymers such as styrene-butadiene rubber (SBR); etc. They can be used individually or in combination of two or more. Commercially available products can be used as the aforementioned styrene-based thermoplastic elastomers.

[0053] The weight-average molecular weight of the thermoplastic elastomer is preferably in the range of 10,000 to 800,000, more preferably in the range of 30,000 to 500,000, and even more preferably in the range of 50,000 to 300,000. By setting it within the above range, it is easy to adjust the storage modulus and loss tangent of the adhesive (adhesive layer) to the desired range, and it becomes easier to melt or soften the adhesive by resistance heating. The method for determining the weight-average molecular weight can be the same as the method for determining the weight-average molecular weight of acrylic polymers described later.

[0054] The aforementioned thermoplastic elastomer can be one or more triblock copolymers, one or more diblock copolymers, or a mixture of triblock copolymers and diblock copolymers. Preferably, the thermoplastic elastomer contains at least a diblock copolymer because the adhesive exhibits moderate cohesiveness, good adhesion at room temperature before energization, and easy melting or softening by resistance heating after energization. The content of the diblock copolymer in the thermoplastic elastomer is preferably in the range of 10% to 100% by mass, more preferably in the range of 10% to 90% by mass, more preferably in the range of 15% to 80% by mass, and further preferably in the range of 20% to 75% by mass from the perspective of an excellent balance between adhesion at room temperature and melting or softening based on resistance heating.

[0055] Furthermore, the thermoplastic resin used as the main component of the adhesive is preferably a polyester resin. It can be a crystalline polyester resin or a non-crystalline polyester resin.

[0056] Furthermore, acrylic resin is preferred as the main thermoplastic resin used as the adhesive. As the aforementioned acrylic resin, an acrylic polymer obtained by polymerizing a monomer component containing a (meth)acrylate monomer can be used. The acrylic polymer can be a homopolymer of the (meth)acrylate monomer or a copolymer with the (meth)acrylate monomer and other monomers. Copolymers are preferred. It should be noted that (meth)acrylate refers to acrylic acid or methacrylic acid. (Meth)acrylate refers to acrylate or methacrylate.

[0057] Examples of (meth)acrylate monomers constituting acrylic polymers include: methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, n-octyl methacrylate, isooctyl methacrylate, 2-ethylhexyl methacrylate, isononyl methacrylate, isodecanyl methacrylate, lauryl methacrylate, and other (meth)acrylate monomers with 1 to 14 carbon atoms. Preferably, the monomers contain alkyl (meth)acrylate monomers having alkyl chains with 1 to 9 carbon atoms; more preferably, they contain alkyl (meth)acrylate monomers having alkyl chains with 2 to 9 carbon atoms. From the perspective of easily adjusting the storage modulus and loss tangent of the adhesive (adhesive layer) to the desired range, monomers containing alkyl (meth)acrylate monomers having 4 to 9 carbon atoms are further preferred; more preferably, they contain alkyl acrylate monomers having alkyl chains with 4 to 9 carbon atoms. Examples of alkyl acrylate monomers having alkyl chains with 4 to 9 carbon atoms include n-butyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, and isononyl acrylate. The acrylic polymer preferably contains one or more of the groups selected from these monomers in its structural units.

[0058] In the total amount of monomer components constituting the above-mentioned acrylic polymer, the content of the above-mentioned (meth)acrylate monomer is preferably in the range of 70% to 99.9% by mass, more preferably in the range of 80% to 99% by mass, and even more preferably in the range of 90% to 97% by mass, since it is easy to adjust the storage modulus and loss tangent of the adhesive (adhesive layer) to the desired range.

[0059] In the aforementioned acrylic polymers, the (meth)acrylic acid monomer, in addition to the aforementioned (meth)acrylate monomers, preferably includes a (meth)acrylic acid monomer having a polar group in the structural unit. Examples of polar groups include hydroxyl, carboxyl, amide, and other polar groups.

[0060] Examples of hydroxyl-containing (meth)acrylate monomers include, for instance, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, hydroxypropyl (meth)acrylate, caprolactone-modified (meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate. Among these, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate are preferred.

[0061] Examples of (meth)acrylic acid monomers with carboxyl groups include acrylic acid, methacrylic acid, itaconic acid, maleic acid, crotonic acid, dimers of acrylic acid or methacrylic acid, and ethylene oxide-modified succinic acid acrylates. Among these, acrylic acid is preferred.

[0062] Examples of (meth)acrylic acid monomers having an amide group include N-vinyl-2-pyrrolidone, N-vinylcaprolactam, acrylmorpholine, acrylamide, N,N-dimethylacrylamide, and 2-(perhydrogenated phthalimide-N-yl)ethyl acrylate. Among these, N-vinyl-2-pyrrolidone, N-vinylcaprolactam, and acrylmorpholine are preferred.

[0063] Examples of vinyl monomers having the other polar groups mentioned above include vinyl acetate, acrylonitrile, maleic anhydride, and itaconic anhydride.

[0064] Among the (meth)acrylic acid monomers having polar groups, it is preferable to include at least one of (meth)acrylic acid monomers having hydroxyl groups and (meth)acrylic acid monomers having carboxyl groups. This is because, when used with the crosslinking agent described later, a crosslinked structure can be formed between the hydroxyl and carboxyl groups and the crosslinking agent, thereby adjusting the storage modulus of the adhesive (adhesive layer).

[0065] In the total amount of monomer components constituting the above-mentioned acrylic polymer, the content of (meth)acrylic acid monomers having polar groups is preferably in the range of 0.1% to 20% by mass, more preferably in the range of 1% to 13% by mass, and more preferably in the range of 1.5% to 8% by mass in order to easily adjust the storage modulus and loss tangent of the adhesive (adhesive layer) to the desired range.

[0066] The weight-average molecular weight of the acrylic polymer is preferably 400,000 to 1,400,000, more preferably 600,000 to 1,200,000, and preferably 650,000 to 1,100,000 in order to easily adjust the storage modulus and loss tangent of the adhesive (adhesive layer) to the desired range.

[0067] Weight-average molecular weight can be determined by gel permeation chromatography (GPC). More specifically, the GPC measuring instrument can be the "SC8020" manufactured by Tosoh Corporation, which determines the weight-average molecular weight by measuring the polystyrene equivalent under the following GPC measuring conditions. (GPC determination conditions) • Sample concentration: 0.5% by mass (tetrahydrofuran solution) • Sample injection volume: 100 μL • Eluent: Tetrahydrofuran (THF) • Flow rate: 1.0 mL / min • Column temperature (measurement temperature): 40℃ ·Pillar: "TSKgel GMHHR-H" manufactured by Tosoh Corporation • Detector: Differential Refraction

[0068] The resin content, as the main component of the adhesive, is preferably 50% by mass or more out of 100% by mass of the total solid content of the adhesive, more preferably 70% by mass or more, further preferably 90% by mass or more, more preferably 98% by mass or more, and even more preferably 99% by mass or more. It should be noted that when the adhesive includes the heating element, it refers to the proportion of the adhesive, excluding the content of the heating element, in the total solid content.

[0069] Furthermore, when the adhesive, in addition to the resin as the main component, also includes the tackifying resin described later, the total proportion of the main component resin and the tackifying resin is preferably 50% by mass or more, more preferably 70% by mass or more, further preferably 90% by mass or more, more preferably 98% by mass or more, and even more preferably 99% by mass or more, out of 100% by mass of the total solid components of the adhesive. It should be noted that when the adhesive includes the heating element described above, this refers to the proportion of the adhesive, excluding the content of the heating element, in the total solid components.

[0070] -Other ingredients- Other components that can be used in the aforementioned pressure-sensitive adhesives and hot-melt adhesives include, for example: tackifying resins, crosslinking agents, antioxidants, thermally expandable fillers, solvents, infrared absorbers, ultraviolet absorbers, fillers; fibers made of glass and plastics; fillers such as balls, beads, and metal powders; pigments, thickeners, etc.

[0071] The adhesive described above and the adhesive layer formed using the adhesive described above can be a thermally foamed type that can foam and / or expand upon heating, and preferably a non-thermally foamed type that does not foam and / or expand upon heating. Even without the presence of thermally expandable fillers, foaming agents, or other components that foam and / or expand within the adhesive layer (expansion-promoting components), the adhesive can be peeled off by the melting or softening of the resin contained in the adhesive. Furthermore, by using a non-thermally foamed adhesive layer, malfunctions of articles and parts caused by gas generated through foaming, and damage to articles and parts caused by pressure applied to the adhered objects by pressure generated through expansion, can be suppressed. Moreover, in the case of a thermally foamed adhesive layer, after long-term use in articles and parts, there may be instances where the foaming agent or other components are modified, deactivated, or released to the outside, resulting in no foaming upon disassembly. However, by using a non-thermally foamed adhesive layer, articles and parts can be reliably disassembled even after long-term use. The adhesive (adhesive layer) does not contain foaming and / or swelling components (swelling performance components) meaning that the content of these components is less than 1 part by mass relative to 100 parts by mass of the base polymer of the adhesive (adhesive layer).

[0072] -Tackifying resin- In the above-mentioned adhesives, a tackifying resin can be used to adjust the strong adhesion of the resulting adhesive layer. There are no particular limitations on the tackifying resin used; it can be appropriately selected according to the purpose. Examples include: rosin-based tackifying resins, polymerized rosin-based tackifying resins, polymerized rosin ester-based tackifying resins, rosin phenol-based tackifying resins, stabilized rosin ester-based tackifying resins, disproportionated rosin ester-based tackifying resins, hydrogenated rosin ester-based tackifying resins, terpene-based tackifying resins, terpene phenolic aldehyde-based tackifying resins, aliphatic (petroleum resin)-based tackifying resins, C5 / C9 petroleum-based tackifying resins, and (meth)acrylate-based tackifying resins.

[0073] In addition to the aforementioned tackifying resin, tackifying resins that are liquid at room temperature can also be used. Examples of such liquid tackifying resins include processing oils, polyester-based tackifying resins, and low molecular weight liquid rubbers such as polybutene.

[0074] The content of the tackifying resin in the adhesive is preferably in the range of 1 to 150 parts by weight relative to 100 parts by weight of the base polymer, with a view to ensuring good adhesion of the adhesive at room temperature and enabling it to perform heat durability. More preferably, it is in the range of 10 to 150 parts by weight, even more preferably in the range of 15 to 100 parts by weight, and even more preferably in the range of 50 to 100 parts by weight.

[0075] -Crosslinking agent- In the above-mentioned adhesives, a crosslinking agent can be used to improve the cohesiveness of the resulting adhesive layer. There are no particular limitations on the crosslinking agent used; it can be appropriately selected according to the purpose. Examples include: isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, polyvalent metal salt-based crosslinking agents, metal chelate-based crosslinking agents, ketone-hydrazide-based crosslinking agents, oxazoline-based crosslinking agents, carbodiimide-based crosslinking agents, silane-based crosslinking agents, and glycidyl (alkoxy)epoxysilane-based crosslinking agents.

[0076] The content of the crosslinking agent contained in the above adhesive can be set to an amount that makes the adhesive reach the range of gel fractions described later, and can be appropriately set.

[0077] -Antioxidants- There are no particular restrictions on the antioxidants mentioned above, and they can be appropriately selected according to the purpose. For example, phenolic antioxidants, amine antioxidants, and carbodiimide antioxidants can be cited.

[0078] -solvent- There are no particular limitations on the solvents used in the adhesive composition. Solvents commonly used in adhesive compositions can be appropriately selected according to the purpose. Examples include organic solvents such as toluene, xylene, ethyl acetate, butyl acetate, acetone, methyl ethyl ketone, and hexane; and water or aqueous solvents with water as the main component. It should be noted that adhesive layer A typically does not contain solvent, but may contain residual solvent.

[0079] -Adhesive- When the adhesive comprises the resin and crosslinking agent as the main components, and the gel fraction of the adhesive is 0% to 80% by mass, the adhesive can be sufficiently melted and / or softened by the resistance heating generated by the short-term energization of the heating element, which is therefore preferable. Within the above range, from the perspective of good initial tack of the adhesive layer and good holding power even at high temperatures, the gel fraction is more preferably 10% to 65% by mass, and even more preferably 15% to 55% by mass. Particularly when the adhesive is a pressure-sensitive adhesive, the above gel fraction range is preferred. On the other hand, within the above range, from the perspective of good removability due to heating, the gel fraction is more preferably 0% to 60% by mass, and even more preferably 0% to 40% by mass. Among these, when the adhesive is a hot-melt adhesive, the above gel fraction range is preferred.

[0080] The gel fraction of an adhesive is the percentage of the dried mass of the remaining insoluble components after the adhesive coating has been immersed in toluene for 24 hours. The gel fraction can be adjusted by adjusting the amount of crosslinking agent, etc.

[0081] [Layer structure of adhesive layer A] The adhesive layer A in the aforementioned adhesive tape is a layer with adhesive properties on both sides, and can be a single layer or contain multiple layers. Preferably, adhesive layer A has pressure-sensitive adhesive and / or heat-sensitive adhesive properties on both sides.

[0082] [First Method] In the case where the adhesive layer A comprises multiple layers, for example as follows: Figure 1A and Figure 1B As shown, the adhesive tape 10 of the present invention has a planar heating element b and adhesive layers a1 and a2 on each surface of the heating element. It can be a laminate containing adhesive layer A, which is a stacked body in the order of adhesive layer a1 / heating element b / adhesive layer a2. That is, the adhesive layer A in the first embodiment is a laminate containing the heating element b, adhesive layer a1 in contact with one side of the heating element b, and adhesive layer a2 in contact with the other side of the heating element b. Adhesive layers a1 and a2 can have the same composition or different compositions. At least one of adhesive layers a1 and a2 can be softened or melted by heating, or both adhesive layers a1 and a2 can be softened or melted by heating. At least one of the adhesive layers a1 and a2 that are in contact with the heating element b is melted or softened by resistance heating, reducing the adhesive force, thereby allowing the adhesive layer A to be peeled off.

[0083] Preferably, adhesive layers a1 and a2 have different compositions. By forming adhesive layers a1 and a2 with different adhesives, the tendency of the storage modulus and loss tangent (tanδ) can be changed. Even if adhesive layers a1 and a2 can be softened or melted by heating, the temperature and peeling position during disassembly can be adjusted according to the differences in the physical properties of adhesive layers a1 and a2, which is advantageous.

[0084] In the adhesive layer A of the first method, the details of the adhesive forming adhesive layer a are the same as those described in the "<<Adhesive>>" section above.

[0085] At least one of the aforementioned adhesive layers a1 and a2 is preferably a pressure-sensitive adhesive layer formed of a pressure-sensitive adhesive, and more preferably, both adhesive layers a1 and a2 are pressure-sensitive adhesive layers. The pressure-sensitive adhesive layer is viscous at room temperature, therefore, adhesive layer a1 and / or adhesive layer a2, as pressure-sensitive adhesive layers, can easily adhere to and bond with other layers constituting the adhesive tape and the adhered object at room temperature.

[0086] Furthermore, at least one of the aforementioned adhesive layers a1 and a2 may be a hot-melt adhesive layer formed of a hot-melt adhesive, and both adhesive layers a1 and a2 may also be hot-melt adhesive layers. Hot-melt adhesives exhibit adhesive properties upon heating; therefore, adhesive layers a1 and / or a2, as hot-melt adhesive layers, can easily bond with other layers constituting the adhesive tape and the adhered object upon heating.

[0087] Alternatively, one of the adhesive layers a1 and a2 may be a pressure-sensitive adhesive layer and the other may be a hot-melt adhesive layer.

[0088] In the first embodiment, the adhesive layer A is preferably, in a top view, a planar heating element b has a pair of protrusions e extending from the outer peripheries of adhesive layers a1 and a2 and exposed (see reference). Figure 1C And D). The protrusion e can be two or more independent locations within the heating element; there are no particular restrictions on its position, and it can be appropriately selected according to the purpose. The two protrusions e can be located on the same side of the outer periphery of adhesive layers a1 and a2 (see reference). Figure 1D (1)~(3)) can also be located on different sides (see reference) Figure 1C , Figure 1D (4)~(6)).

[0089] The protrusion e is preferably located on opposite sides of the outer periphery of adhesive layers a1 and a2, respectively (see reference). Figure 1D (4)~(6)) are preferably located on the diagonal lines of the outer periphery of adhesive layers a1 and a2 respectively (refer to Figure 1D (2)~(7)). This allows current to be passed through the entire area of ​​the planar heating element b, further improving heating efficiency. Furthermore, when the protrusion e is located on the same side of the outer periphery of adhesive layers a1 and a2, it is preferable that the heating element b has a "コ" shape, a sawtooth shape, etc., in the top view (see reference). Figure 1D (1)~(4), (8)), as long as the heating element can uniformly heat the surfaces of adhesive layers a1 and a2, then adjacent parts located on the same side can also be heated (see reference). Figure 1D (3), (8)). Thus, current can be passed through the entire area of ​​the planar heating element b, which can further improve the heating efficiency.

[0090] Additionally, the protruding part e can be in three or more locations (see reference). Figure 1D (9) Alternatively, a desired pair (two locations) can be selected to energize the heating element. The pair of protrusions e of the heating element b function as a pair of terminals for electrical connection to the power source in the article disassembly method described later, allowing for easy energization of the heating element b.

[0091] The length of the aforementioned protrusions is preferably 1mm to 50mm, more preferably 2mm to 25mm, from the viewpoint of easy contact with the power source. Each protrusion can be bent in a direction different from the surface direction of the adhesive tape. For example, when the objects to be bonded together are in a state of being attached to each other, the protrusions can be bent and tucked in a direction perpendicular to the surface direction of the adhesive tape. When it is time to remove the objects from the bond (dismantling), the protrusions can be bent again in the surface direction to make contact with the power source.

[0092] When adhesive layer A is a laminate composed of multiple layers, the average thickness of adhesive layers a1 and a2 is not particularly limited and can be appropriately selected according to the purpose. For example, 5 μm to 200 μm is preferred, 10 μm to 150 μm is more preferred, and 20 μm to 100 μm is even more preferred. The average thickness of adhesive layers a1 and a2 in the second embodiment described later can also be set to the same specification. When adhesive layer A is a laminate composed of multiple layers, the total thickness of adhesive layer A is not particularly limited and can be appropriately selected according to the purpose. 15 μm to 500 μm is preferred, 30 μm to 400 μm is more preferred, and 50 μm to 300 μm is even more preferred. The total thickness of adhesive layer A in the second embodiment described later can also be set to the same specification.

[0093] [Second Method] In addition, such as Figure 2 As shown, the adhesive tape 20 of the present invention can be a laminate containing adhesive layer A, which is stacked in the order of adhesive layer a1 / heating element b / melt softening layer c / adhesive layer a2. Alternatively, adhesive layer A can be a laminate stacked in the order of adhesive layer a1 / melt softening layer c / heating element b / adhesive layer a2; or a laminate stacked in the order of adhesive layer a1 / melt softening layer c1 / heating element b / melt softening layer c2 / adhesive layer a2. Furthermore, it can also be a laminate stacked in the order of adhesive layer a / heating element b / melt softening layer c.

[0094] That is, the adhesive layer A of the second embodiment has a heating element, one or more adhesive layers a, and one or more melt-softening layers c. As an example of the adhesive layer A of the second embodiment, a laminate having a heating element b, an adhesive layer a disposed on one side of the heating element b, and a melt-softening layer c disposed on the other side of the heating element b can be given. As another example of the adhesive layer A of the second embodiment, a laminate having a heating element b, an adhesive layer a1 disposed on one side of the heating element b, an adhesive layer a2 disposed on the other side of the heating element b, and a melt-softening layer c disposed between the heating element b and the adhesive layer a1 and between the heating element b and the adhesive layer a2.

[0095] At least the melt-softened layer c in the adhesive layer A is melted or softened by resistance heating, thereby allowing the adhesive layer A to be peeled off. In this case, each layer of adhesive layer a1 and adhesive layer a2 may contain adhesive that is melted or softened by resistance heating, or may not contain adhesive that is melted or softened by resistance heating. Furthermore, adhesive layers a1 and a2 may have the same composition or different compositions. Preferably, in the top view, the planar heating element b has a pair of protrusions extending from the outer periphery of adhesive layers a1 and a2 and the melt-softened layer c. The details of the protrusions are the same as those of the protrusions in the planar heating element b in the adhesive layer A of the first embodiment described above.

[0096] <<Adhesive layer a>> In the second type of adhesive layer A, adhesive layer a is preferably formed of pressure-sensitive adhesive or hot-melt adhesive. Details regarding the adhesive used to form adhesive layer a are the same as those described in the "<<Adhesive>>" section above.

[0097] In the second type of adhesive layer A, the aforementioned melt-softening layer is a layer that is melted or softened by heating. Therefore, the aforementioned adhesive layer a can be melted or softened by resistance heating, or it can remain unmelted or unsoftened, preferably melted or softened.

[0098] In the second type of adhesive layer A, it is preferable that at least one of the adhesive layers a1 and a2 is a pressure-sensitive adhesive layer formed of a pressure-sensitive adhesive, and more preferably that both adhesive layers a1 and a2 are pressure-sensitive adhesive layers. The pressure-sensitive adhesive layer is viscous at room temperature, therefore, adhesive layer a1 and / or adhesive layer a2, as pressure-sensitive adhesive layers, can easily adhere to and bond with other layers constituting the adhesive tape and the adhered object at room temperature.

[0099] Furthermore, at least one of the aforementioned adhesive layers a1 and a2 may be a hot-melt adhesive layer formed of a hot-melt adhesive, and both adhesive layers a1 and a2 may also be hot-melt adhesive layers. Hot-melt adhesives exhibit adhesive properties upon heating; therefore, adhesive layers a1 and / or a2, as hot-melt adhesive layers, can easily bond with other layers constituting the adhesive tape and the adhered object upon heating.

[0100] Alternatively, one of the adhesive layers a1 and a2 may be a pressure-sensitive adhesive layer and the other may be a hot-melt adhesive layer.

[0101] <<Melted Softened Layer>> The aforementioned melt-softening layer is a layer that is melted or softened by heating. As for the aforementioned melt-softening layer, there are no particular limitations as long as it can achieve good adhesion to the aforementioned adhesive layer and the aforementioned heating element, and ensure the desired adhesive strength between the adhered objects in the article described later. The resin layer that melts or softens by heat can be appropriately selected according to the purpose. Examples include: thermoplastic resin film, resin layer in which particles with a softening point lower than the aforementioned matrix resin are dispersed in the matrix resin, and resin layer in which particles with a softening point are dispersed in a matrix resin that does not have a softening point, etc. Examples of thermoplastic resins used in the aforementioned thermoplastic resin films include: polyolefin resins such as low-density polyethylene (LDPE), medium-density polyethylene (MDPE), polypropylene (PP), and linear low-density polyethylene (LLDPE); ethylene copolymer resins such as ethylene-vinyl acetate copolymer (EVA), ethylene-acrylic acid copolymer (EAA), and ethylene-methacrylic acid copolymer (EMAA); polyester resins such as crystalline polyester and amorphous polyester; and urethane resins. In addition, thermoplastic resins and thermoplastic elastomers described in the above adhesives can also be used.

[0102] In cases where it is difficult to adjust the melting or softening temperature of the resin monomers constituting the thermoplastic film, the aforementioned thermoplastic film may contain additives such as plasticizers and tackifying resins.

[0103] The melting point of the aforementioned melt-softening layer is preferably 70°C or higher and 150°C or lower, more preferably 75°C or higher and 130°C or lower, and even more preferably 80°C or higher and 110°C or lower. This is because, by keeping the melting point of the aforementioned melt-softening layer within the above range, it can be easily melted or softened even with a small amount of resistance heating. The melting point of the aforementioned melt-softening layer can be adjusted by selecting the type and composition of the resin (especially a thermoplastic resin) that is the main component of the aforementioned melt-softening layer. The melting point (melting temperature) of the aforementioned melt-softening layer can be set to the temperature of the endothermic peak accompanying melting, as measured using differential scanning calorimetry (DSC).

[0104] Storage modulus G, as a melt softening layer, was determined by dynamic viscoelastic spectroscopy at 1 Hz and 23 °C. 23 From the viewpoint of ensuring good fixation of adjacent layers under normal conditions, 1.0 × 10⁻⁶ is preferred. 3 Pa ~ 1.0 × 10 9 Pa, more preferably 5.0 × 10 Pa 3 Pa ~ 5.0 × 10 8 Pa, preferably 1.0 × 10 Pa. 4 Pa ~ 1.0 × 10 8 Pa. Storage modulus G of the above-mentioned molten softened layer. 23 The energy storage modulus G of the adhesive (adhesive layer) can be utilized 23 The determination method is the same as that used for the previous determination.

[0105] The storage modulus of the aforementioned melt-softened layer is less than 1.0 × 10⁻⁶. 5 The temperature of Pa is preferably in the temperature range of 80℃ to 200℃, and the storage modulus of the above-mentioned melt softening layer is less than 1.0 × 10⁻⁶. 4 The temperature of Pa is more preferably located in the temperature range of 80°C to 200°C, and the storage modulus of the aforementioned melt-softened layer is less than 1.0 × 10⁻⁶. 3 The temperature of Pa is further preferably located in the temperature range of 80°C to 200°C. The storage modulus of the aforementioned melt-softening layer is less than 1.0 x 10⁻⁶. 5 The temperature of Pa is in the temperature range of 80°C to 200°C. It is advantageous that when the molten softened layer reaches this temperature through heating from the heating element, it melts or softens, resulting in delamination within the molten softened layer or at the interface between these layers and adjacent layers. The storage modulus of the aforementioned molten softened layer can be determined using the same method as the method for determining the storage modulus of the aforementioned adhesive (adhesive layer).

[0106] When the above-mentioned melt-softening layer is present, there is no particular limitation on the average thickness of the melt-softening layer, which can be appropriately selected according to the purpose. Preferably, it is 5 μm to 200 μm, more preferably 10 μm to 150 μm, and even more preferably 20 μm to 100 μm.

[0107] [Third Method] When the adhesive layer A is a single layer, it can be a single layer comprising adhesive layer a3, or adhesive layer a3 containing a heating element b (see [reference]). Figure 3 The adhesive layer a3 preferably comprises at least one of the pressure-sensitive adhesive containing the thermoplastic resin and the hot melt adhesive as the adhesive. The adhesive layer a3 is melted or softened by resistance heating, thereby reducing the adhesive force and allowing the adhesive layer A to be peeled off.

[0108] In the third-party adhesive layer A, the adhesive forming adhesive layer a3 can be a pressure-sensitive adhesive. That is, adhesive layer A can be a pressure-sensitive adhesive layer a3 containing a heating element. This is because both sides of adhesive layer A are tacky at room temperature, allowing it to adhere to the substrate and other layers constituting the adhesive tape of the present invention.

[0109] Furthermore, in the third-party adhesive layer A, the adhesive forming adhesive layer a3 can be a hot melt adhesive. That is, adhesive layer A can also be a hot melt adhesive layer a3 containing a heating element. Hot melt adhesives exhibit adhesive properties when heated, therefore, adhesive layer A, as a hot melt adhesive layer, can be easily bonded to other layers constituting the adhesive tape and the adhered object by heating.

[0110] In the third-party adhesive layer A, the details regarding the adhesive forming adhesive layer a3 are the same as those described in the "<<Adhesive>>" section above. The details regarding the heating element b included in adhesive layer a3 are the same as those described in the "<<Heating Element>>" section above.

[0111] The total thickness of the adhesive layer A, when the adhesive layer A is a single layer, is not particularly limited and can be appropriately selected according to the purpose. Preferably, it is 15μm to 500μm, more preferably 30μm to 400μm, and even more preferably 50μm to 300μm.

[0112] [Other methods] Other forms of adhesive layer A in a laminate include, but are not limited to, the following laminate structures. The " / " in the laminate structure indicates the laminate interface; for example, "Layer A / Layer B" indicates that Layer A and Layer B are in direct contact. • A stacked structure arranged in the order of melt-softened layer c / adhesive layer a1 / heating element b / adhesive layer a2. • A stacked structure arranged in the order of adhesive layer a1 / heating element b / adhesive layer a2 / melt softening layer c. • A stacked structure in the order of melt-softened layer c1 / adhesive layer a1 / heating element b / adhesive layer a2 / melt-softened layer c2 • A laminated structure in which adhesive layer a1 containing heating element b is stacked in the order of adhesive layer a2 not containing heating element b. • A laminated structure in which adhesive layer a1 containing heating element b is stacked in the order of adhesive layer a2 containing heating element b.

[0113] <Peeling Layer> In addition to the adhesive layer A, the adhesive tape may also have other layers such as the release layer D. There are no particular limitations on the release layer used, and it can be appropriately selected according to the purpose. Examples include: cellophane, kraft paper, clay-coated paper, paper laminated with polyethylene films, paper coated with resins such as polyvinyl alcohol and acrylate copolymers, and release layers coated with fluoropolymers, silicone resins, etc., as release agents, onto synthetic resin films such as polyester and polypropylene. The release layer can be present on one side of the adhesive tape or on both sides.

[0114] <Other Layers> The adhesive tape of the present invention is not limited in structure as long as it includes at least an adhesive layer A and an outermost layer (excluding the release layer D) located in a relative position in the thickness direction has an adhesive surface that can adhere to the adhered object. In addition to the adhesive layer A and the release layer D as an arbitrary layer, it may also have other layers such as an insulating layer, a heat-insulating layer (e.g., a foamed resin layer, a hollow layer, or a hollow particle layer) or a functional layer E with insulating, heat-insulating, or heat-resistant properties, an adhesive layer (pressure-sensitive adhesive layer) F constituting the adhesive surface of the adhesive tape.

[0115] [Structure of adhesive tape] The adhesive tape of the present invention can be configured to have at least an adhesive layer A, for example, as illustrated in the following examples, but is not limited thereto. In the following layered structures, " / " indicates a layer interface, for example, "layer A / layer B" indicates that layer A and layer B are in direct contact. • Structure of release layer D / adhesive layer A • Structure of release layer D / adhesive layer A / release layer D • Structure of release layer D / adhesive layer F / functional layer E / adhesive layer A • Structure of adhesive layer F / functional layer E / adhesive layer A / release layer D • Structure of release layer D / adhesive layer F / functional layer E / adhesive layer A / release layer D • Structure of adhesive layer F / functional layer E / adhesive layer A / functional layer E / adhesive layer F / release layer D • Structure of release layer D / adhesive layer F / functional layer E / adhesive layer A / functional layer E / adhesive layer F / release layer D

[0116] In the adhesive tape of the present invention, both sides of the adhesive layer A can be the bonding surfaces with the adhered object, and the adhesive layer F disposed on one or both sides of the adhesive layer A can be the bonding surface with the adhered object.

[0117] When adhesive layer A is a laminate and the adhesive tape has a release layer D that contacts one or both sides of adhesive layer A, the outermost layer of adhesive layer A in contact with release layer D can be a pressure-sensitive adhesive layer or a hot-melt adhesive layer. From the perspective of being able to adhere to the substrate at room temperature, a pressure-sensitive adhesive layer is preferred. Furthermore, when adhesive layer A is a single layer and the adhesive tape has a release layer D that contacts one or both sides of adhesive layer A, adhesive layer A is preferably a pressure-sensitive adhesive layer.

[0118] When adhesive layer A is a laminate and the adhesive tape has a release layer D on one or both sides of adhesive layer A via other layers, the outermost layer of adhesive layer A can be a pressure-sensitive adhesive layer or a hot-melt adhesive layer, as long as it can be bonded to the other layers at room temperature or by heat. Preferably, the outermost layer of adhesive layer A is a pressure-sensitive adhesive layer. The same applies when adhesive layer A is a single layer and the adhesive tape has a release layer D on one or both sides of adhesive layer A via other layers.

[0119] The adhesive layer F described above can be formed using known adhesives, such as the pressure-sensitive adhesive described in adhesive layer A.

[0120] [Uses of adhesive tape] The adhesive tape of the present invention functions as adhesive surfaces (bonding surfaces) on both sides except for the release liner, thus allowing the adhesion of objects to both sides of the adhesive tape, making it suitable for bonding objects together. The adhesive tape of the present invention can be peeled off by resistance heating, therefore it can be used as a resistance heating (electric heating) peeling tape.

[0121] The adhesive tape of the present invention is not particularly limited and is suitable for bonding and separating objects that are rigid. When separating parts during reuse or recycling, the adhesive tape of the present invention can be easily removed by resistance heating. Therefore, it can be used in applications requiring the removal of adhesive tape. For example, it is suitable for fixing parts of various products in industrial applications such as electronics, automobiles, building materials, office automation, and home appliances. It also offers good work efficiency when separating large numbers of parts or peeling off large numbers of labels during reuse or recycling.

[0122] [Preparation method of adhesive tape] As a method for preparing the adhesive tape, when the adhesive tape has a planar heating element or an integrally formed mesh heating element, for example, a method can be used to coat a release sheet with a composition containing the adhesive, and after a drying process, sequentially attach it to each side of the heating element. When the adhesive tape has a granular or fibrous heating element, for example, a method can be used to coat a release sheet with a composition containing a granular or fibrous heating element and an adhesive, and after a drying process, attach other release sheets.

[0123] 2. Items The article of the present invention comprises at least two adherends and an adhesive strip of the present invention located between the two adherends, the two adherends being bonded together via the adhesive strip. As a method of bonding the adherends, examples include attaching the adherends to the adhesive surfaces of the adhesive strip respectively, thereby bringing the two adherends together. There are no particular limitations on the article; it can be appropriately selected depending on the purpose, and is preferably an electronic device, a component built into an electronic device, etc. Preferably, in a top view, the adhesive strip has a pair of protrusions extending from the outer periphery of the adherends.

[0124] Adhesive tape Details regarding the adhesive tape in the articles of the present invention are as described in the item “1. Adhesive Tape” above.

[0125] <Object to be adhered> The aforementioned adhered material can be rigid or flexible, such as a membrane. There are no particular limitations on the materials to be bonded, and they can be appropriately selected according to the purpose. Examples include metal plates, metal frames, metal covers, glass plates, plastic plates, etc.; and parts having any of these on the bonding surface. The two materials to be bonded by the adhesive tape can be the same or different from each other.

[0126] For example, such as Figure 4A schematic top view and Figure 4B As shown in the schematic cross-sectional view, the article 100 of the present invention is an article comprising an adhesive tape 10, wherein two adherends 50 are bonded together by the adhesive tape 10. The adhesive tape 10 comprises two adherends 50 and a laminate, namely adhesive layer A, in which the two adherends 50 are stacked between them in the order of adhesive layer a1 / planar heating element b / adhesive layer a2. In the top view ( Figure 4AIn this process, the two ends of the adhesive tape 10 extend from the outer periphery of the object to be adhered to in the long axis direction. Furthermore, the two ends of the planar heating element b extend from the outer periphery of the adhesive layer a1 and the adhesive layer a2 in the long axis direction. In the article disassembly method described later, the two ends of the extended adhesive tape 10 can be used as a pair of terminals for electrical connection with a power source, making it easy to energize the heating element b of the adhesive tape 10.

[0127] In addition, such as Figure 5 As shown in the schematic cross-sectional view, the article 300 of the present invention may also be an article comprising an adhesive tape 30 and two adherends 50 bonded together by the adhesive tape 30, wherein the adhesive tape 30 comprises two adherends 50 and an adhesive layer a3 containing a heating element b and an adhesive between the two adherends 50.

[0128] In the top view of the aforementioned item, the adhesive tape can be applied to the entire area of ​​the adhesive tape side (i.e., the surface to be bonded), or it can be applied to a portion of the adhesive tape surface. For example, Figure 4A As shown, the adhesive tape 10 is preferably attached to a portion of the adhesive surface of the adherend 50. By making the contact area between the adherend and the adhesive tape small, a peeling start point becomes easier to generate between the adherend and the adhesive tape when the adhesive tape is peeled off from the adherend by resistance heating, which is advantageous in terms of ease of peeling.

[0129] like Figure 4A As shown, in the top view of the article of the present invention, when the adhesive tape 10 is attached to a portion of the adhesive surface of the adhesive object 50, the top view shape of the adhesive tape 10 in the article can be strip-shaped, line-shaped, or patterned.

[0130] Furthermore, in the top view of the article of the present invention, when the adhesive tape is adhered to the entire area of ​​the adhesive tape side of the object to be adhered, that is, the adhesive tape surface, the top view shape of the planar heating element in the adhesive tape can be the same as the top view shape of the adhesive tape, or it can be strip-shaped, line-shaped, or patterned.

[0131] 3. Methods for disassembling items The method for disassembling the article of the present invention is a method for disassembling the article of the present invention, or a method for disassembling an article formed by two adhered objects bonded together by the adhesive tape of the present invention, which includes a separation step and may further include other steps as needed.

[0132] The details regarding the article and the adhesive tape used in the disassembly method of the present invention are the same as those described in "2. Article" and "1. Adhesive Tape" above.

[0133] <Separation Process> The separation process described above involves electrically connecting the adhesive layer A to a power source, supplying electricity to the heating element, and softening or melting the adhesive layer A through resistance heating, thereby separating the two adhered objects.

[0134] There are no particular limitations on the power source mentioned above, and it can be appropriately selected according to the purpose. It can be an external power source or a driving power source for electronic devices or the aforementioned articles that are built into electronic devices, but it is preferred to be a driving power source for electronic devices or components built into electronic devices. In addition, when the above-mentioned items are electronic devices or parts built into electronic devices, and the above-mentioned power supply is the driving power supply of the above-mentioned electronic devices, the above-mentioned separation process is preferably the following process: electrically connecting the above-mentioned adhesive layer A to the driving power supply and circuit of the above-mentioned electronic devices, energizing the above-mentioned heating element from the driving power supply, and melting or softening the above-mentioned adhesive layer A by resistance heating, thereby separating the two above-mentioned adhered items.

[0135] As a method for the aforementioned electrical connection, known means such as alligator clips can be used to electrically connect the adhesive layer A (preferably the heating element, or the two ends of the protruding heating element) to the power source. The circuit and the means of the electrical connection are preferably formed of a conductive material exhibiting a volume resistivity different from that of the heating element in the adhesive tape, and more preferably of a conductive material with a volume resistivity lower than that of the heating element. By forming the adhesive layer A with a conductive material having a volume resistivity lower than that of the heating element, it is advantageous to prevent overheating of the circuit and the means of the electrical connection when the heating element is electrically connected to the circuit and energized from the driving power source, and to efficiently apply voltage to the adhesive layer A so that it can be peeled off in a short time.

[0136] As for the aforementioned method of applying electricity, it can be appropriately selected according to the size of the adhesive tape, the type of heating element used, etc. For example, a method in which a voltage of 0.1V to 200V is applied until the adhesive layer A melts or softens (e.g., 0.5 seconds to 30 minutes). For example, such as Figure 6 As schematically shown, a simple power source can be used to electrically connect adhesive layer A to the power source, apply voltage to the heating element to energize it, and thereby heat the heating element and its surroundings through resistance heating. As a result, the adhesive or any melt-softening layer in adhesive layer A softens or melts, releasing the adhesive state at a desired location within adhesive layer A itself or within adhesive layer A. Adhesive layer A can be peeled off, and the bonded objects can be removed.

[0137] The voltage applied to the heating element by energizing it is not particularly limited, but is preferably 0.1V or higher and 200V or lower, more preferably 0.5V or higher and 150V or lower, and even more preferably 1.0V or higher and 100V or lower. Even with a low applied voltage, the adhesive layer A of the adhesive tape of the present invention softens or melts within a short time. Therefore, by setting the voltage applied in the separation process within the above-mentioned range, the article can be disassembled in a short time without applying excessive voltage, thus preventing damage to the article. In particular, by applying a voltage that can be handled by small electronic devices and household appliances, the disassembly of these articles can be easily performed.

[0138] The current flowing through the heating element is not particularly limited, but is preferably 0.01A or more and 20A or less, preferably 0.03A or more and 15A or less, preferably 0.05A or more and 10A or less, and more preferably 0.1A or more and 5A or less. Because the adhesive tape of the present invention softens or melts the adhesive layer A in a short time, by setting the current applied in the separation process within the above-mentioned range, the current flowing through common electronic devices and household appliances can be used to disassemble the items in a short time, preventing damage to the items. In particular, by applying a current that can be handled by small electronic devices and household appliances, the disassembly of these items can be easily performed.

[0139] The application time of the current is not particularly limited, but is preferably 0.5 seconds or more and 30 minutes or less, more preferably 0.5 seconds or more and 120 seconds or less, and even more preferably 0.5 seconds or more and 30 seconds or less. By setting the application time to the above range and applying an appropriate voltage, disassembly can be performed in a short time without damaging the item. Example

[0140] The present invention will now be described in more detail with reference to embodiments; however, the present invention is not limited to the embodiments described below. Furthermore, unless otherwise specified, "parts" refers to "parts by mass" and "%" refers to "% by mass".

[0141] In addition, the adhesive tape structure shown in the embodiments and reference examples is a structure that removes the release liner, and the total thickness of the adhesive tape does not include the thickness of the release liner.

[0142] <Methods for Determining Physical Properties> (energy storage modulus G) 23 and energy storage modulus G 100 ) The storage modulus G of the adhesive layer a formed by the adhesive compositions (P-1) and (P-2) 23 and energy storage modulus G 100The following method was used for determination. A viscoelasticity testing machine (ARES-G2, manufactured by TA Instruments Japan) was used. Test specimens were sandwiched between parallel discs with a diameter of 8 mm, which served as the measuring section of the same testing machine. The storage modulus G' was measured at a frequency of 1 Hz, a temperature range of -40°C to 200°C, and a heating rate of 2°C / min. The values ​​at 23°C and 100°C were recorded. For the test specimens, an adhesive layer (adhesive layer) was used as follows: the adhesive composition was applied using a coater to a dry thickness of approximately 2 mm and dried. It was then cured at 40°C for 48 hours.

[0143] (Measured value of volume resistivity of the heating element) The measured volume resistivity of the heating element used in the examples and reference examples was determined using a low resistivity meter (manufactured by Nitto Seiko Analytech Co., Ltd., trade name: Loresta-AX MCT-T370) and a four-probe probe (manufactured by Nitto Seiko Analytech Co., Ltd., trade name: "ASP probe MCP-TP03P"), according to JIS K 7194 at room temperature (20°C). The measurement point was set to 1 point, and a resistivity correction factor of 4.532 was used.

[0144] <Preparation of Adhesive Composition (P-1)> 100 parts by weight of styrene-isoprene block copolymer composition a (a mixture of styrene-isoprene diblock copolymer and styrene-isoprene triblock copolymer, wherein the structural units derived from styrene represented by the following chemical formula (1) are 24% by mass and the proportion of styrene-isoprene diblock copolymer to the total amount of composition a is 67% by mass), 40 parts by mass of Quintone G115 (a C5 / C9 series petroleum resin manufactured by ZEON Corporation of Japan, with a softening point of 115°C), and Pensel 30 parts by weight of D-160 (polymerized rosin ester resin manufactured by Arakawa Chemical Industry Co., Ltd., softening point 15℃~150℃), 5 parts by weight of Nipponshima polybutene HV-50 (polybutene manufactured by JX Nipponshima Energy Co., Ltd., flow point -12.5℃) and 1 part by weight of anti-aging agent (tetra-[methylene-3-(3'5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane) are mixed and dissolved in 100 parts by weight of toluene as solvent to obtain adhesive composition (P-1).

[0145] [Chemical Formula 1]

[0146] <Preparation of Adhesive Composition (P-2)> 79.9 parts by mass of n-butyl acrylate, 6 parts by mass of 2-ethylhexyl acrylate, 10 parts by mass of cyclohexyl acrylate, 4 parts by mass of acrylic acid, 0.1 parts by mass of 4-hydroxybutyl acrylate, and 200 parts by mass of ethyl acetate were added to a reaction vessel equipped with a stirrer, reflux condenser, nitrogen inlet tube, and thermometer. The mixture was stirred and bubbled under nitrogen at room temperature for 1 hour to obtain a mixture. Next, 2 parts by mass of a 2,2′-azobis(2-methylbutyronitrile) solution (1.0% by mass of solids) pre-dissolved in ethyl acetate was added to the mixture. The mixture was stirred and maintained at 72°C for 4 hours, followed by a maintenance at 75°C for 5 hours. The resulting mixture was then diluted with ethyl acetate and filtered through a 200-mesh metal mesh to obtain an acrylic copolymer (A-1) solution (26% solids concentration) with a weight average molecular weight of 1,060,000 and an average carbon number of 4.4 saturated hydrocarbon groups in the alkyl acrylate monomers. In 100 parts by mass of the above acrylic copolymer (A-1) solution, 1.0 parts by mass of the adduct of toluene diisocyanate and trimethylolpropane ("Burnock D-40" manufactured by DIC Corporation, isocyanate crosslinking agent, 40% solids, hereinafter referred to as "D-40") was added to obtain the adhesive composition (P-2).

[0147] (Example 1) Making Adhesive Tape The adhesive composition (P-1) was applied to the release-treated surface of the release liner (a 75 μm thick polyethylene terephthalate film with single-sided release treatment) to a dried thickness of 50 μm, and dried at 90°C for 3 minutes to form adhesive layer a1. Next, the adhesive composition (P-2) was applied to the release-treated surface of the release liner (a 75 μm thick polyethylene terephthalate film with single-sided release treatment) to a dried thickness of 50 μm, and dried at 90°C for 3 minutes to form adhesive layer a2. A 10 μm thick nickel-chromium alloy foil (manufactured by Takeuchi Metal Foil Powder Industry Co., Ltd., "Nichrome Alloy NCH1-H") was used as the heating element.

[0148] Using a hand pressure roller, the adhesive layer a1 cut to an arbitrary width with a length of 50 mm is bonded to a nichrome alloy foil with a length of 100 mm, and positioning is performed such that each of the two ends of the nichrome alloy foil in the longitudinal direction extends by 25 mm. Similarly, the adhesive layer a2 cut to an arbitrary width with a length of 50 mm is bonded to the opposite side of the nichrome alloy foil that is bonded to the adhesive layer a1. Lamination is performed from the upper surface of the release liner using a roller with a linear pressure of 5 kg / cm, so as to produce a laminate with a total thickness of 110 μm in a shape where both ends of the nichrome alloy foil extend 25 mm in the longitudinal direction of the nichrome alloy foil from the outer peripheries of the adhesive layer a1 and the adhesive layer a2, followed by aging for 48 hours in an environment at 40°C. This is cut to a width of 2 mm to obtain the adhesive tape (T-1) of Example 1, in which the adhesive layer a1 and the adhesive layer a2 have dimensions of 2 mm wide × 50 mm long, the nichrome alloy foil has dimensions of 2 mm × 100 mm long, and the nichrome alloy foil has a pair of extending portions extending from the outer peripheries of the adhesive layer a1 and the adhesive layer a2. It should be noted that regarding the volume resistivity of the nichrome alloy foil, the catalog value is 108 μΩ·cm, and the actually measured value is 105 μΩ·cm.

[0149] The viscoelastic parameters of the adhesive layer a formed from the adhesive composition (P-1) are as follows: storage modulus G at 23°C 23 : 3.E+05, loss tangent (tanδ) at 23°C: 0.33, storage modulus G at 100°C 100 : 8.E+04, loss tangent (tanδ) at 100°C: 0.48, the temperature at which the loss tangent (tanδ) of the adhesive layer a1 reaches 0.45 or higher: 94°C or higher.

[0150] The viscoelastic parameters of the adhesive layer a formed from the adhesive composition (P-2) are as follows: storage modulus G at 23°C 23 : 9.E+04, loss tangent (tanδ) at 23°C: 0.69, storage modulus G at 100°C 100 : 2.E+04, loss tangent (tanδ) at 100°C: 0.33, the temperature at which the loss tangent (tanδ) of the adhesive layer a2 reaches 0.45 or higher: exceeding 150°C.

[0151] <Production of Article> For the adhesive tape of Example 1 ( Figure 8A denoted by reference numeral 10 in FIGS. to C), the release liner on the adhesive layer a1 side is peeled off, and it is attached such that the length of the adhesive surface (effective portion) of the tape is 50 mm, crossing the center of the adherend 50a along the width direction of the adherend 50a (refer to Figure 8A~C) On the substrate 50a (glass, 40mm wide × 50mm long × 10mm thick). Next, peel off the release liner on the adhesive layer a2 side to hold the adhesive tape 10 in the shape of the substrate 50b (glass, 30mm wide × 100mm long × 2.8mm thick) (refer to...). Figure 8A ~C) Paste, at 20N / cm 2 Press for 10 seconds, and place the resulting attachment at 23°C and 50% RH for more than 24 hours to obtain the article of Example 1.

[0152] (Example 2) Using a 10μm thick stainless steel foil (manufactured by Takeuchi Metal Foil Powder Industry Co., Ltd., trade name: "Stainless Steel SUS304-H") with a volume resistivity of 72.0μΩ·cm (rated value 79.9μΩ·cm) instead of nickel-chromium alloy foil, the adhesive tape (T-2) and article of Example 2 with a total thickness of 110μm were obtained by the same operation as in Example 1.

[0153] (Example 3) Using a 10μm thick stainless steel foil (manufactured by Takeuchi Metal Foil Powder Industry Co., Ltd., trade name: "Stainless Steel SUS430-H") with a volume resistivity of 60.0μΩ·cm (rated value 62.0μΩ·cm) instead of nickel-chromium alloy foil, the adhesive tape (T-3) and article of Example 2 with a total thickness of 110μm were obtained by the same operation as in Example 1.

[0154] (Example 4) Using a 10 μm thick titanium foil (manufactured by Takeuchi Metal Foil Powder Industry Co., Ltd., trade name: "Titanium Type TR270C-H") with a volume resistivity of 55.0 μΩ·cm (rated value 51.8 μΩ·cm) instead of nickel-chromium alloy foil, the adhesive tape (T-4) and article of Example 2 with a total thickness of 110 μm were obtained by the same operation as in Example 1.

[0155] (Example 5) Using a 10μm thick nickel-silver foil (manufactured by Takeuchi Metal Foil Powder Industry Co., Ltd., trade name: "Yangbai C7701") with a volume resistivity of 34.0μΩ·cm (rated value 33.1μΩ·cm) instead of nickel-chromium alloy foil, the adhesive tape (T-5) and article of Example 2 with a total thickness of 110μm were obtained by the same operation as in Example 1.

[0156] (Example 6) 7.5g of amphoteric surfactant (manufactured by Toho Chemical Industry Co., Ltd., trade name: "Obazoline CAB-30") and 7.6g of carbon nanotubes (manufactured by Nanocyl Co., Ltd., trade name: "NC 7000") were mixed in 500ml of water to make an aqueous solution. The solution was then placed in a ball mill body (capacity = 900ml, ball mill diameter = 130mm, ball filling amount = 1600g) and stirred to make a paste. The ball mill body was placed on a rotating platform and stirred for two hours. The entire volume of the obtained dispersion was removed from the ball mill body, and 250 ml of a 15% aqueous solution of the above-mentioned amphoteric surfactant was added. The mixture was then filled into a bead mill (manufactured by WAB, trade name: filled with "DYNO-MILL ECM-AP2", internal volume = 1900 ml, 1800 g of 0.6 mm diameter zirconia beads). The mixture was stirred for 60 minutes at a speed of 300 times / minute to prepare an aqueous dispersion of carbon nanotubes containing the amphoteric surfactant (carbon nanotube concentration = 0.99 w%).

[0157] An aqueous dispersion of carbon nanotubes was coated onto one side of a 25 μm thick polyimide film (manufactured by Toray DuPont, trade name: "Kapton 100H") using a rod coater to achieve a dried film thickness of 3 μm. The coating was dried at 100°C for 10 minutes, forming a carbon nanotube layer on the single side of the polyimide film, resulting in a carbon nanotube-coated film. The measured volume resistivity of the carbon nanotube layer was 19270 μΩ·cm.

[0158] Using the carbon nanotube coating film described above instead of the nickel-chromium alloy foil of Example 1, except that the same operation as in Example 1 was performed to obtain the adhesive tape (T-6) and article of Example 6 with a total thickness of 128 μm. It should be noted that the carbon nanotube coating film is used to bond the carbon nanotube layer to the adhesive layer a1 in adjacent contact.

[0159] (Example 7) Metallic nonwoven fabric (material: SUS 316L, thickness: 25μm, density: 1.6g / cm³) was used. 3 The adhesive tape (T-7) and article of Example 7 with a total thickness of 125 μm were obtained by replacing the nickel-chromium alloy foil with a fiber diameter of 7 μm and a measured volume resistivity of 783 μΩ·cm. Otherwise, the same operation as in Example 1 was performed.

[0160] (Example 8) A crystalline polyester resin coating (manufactured by Mitsubishi Chemical Corporation, trade name: "NichigoPolyester MSP-640", melting point 100℃, molecular weight 10000, non-sticky) (P-3) was applied to the release-treated side of a release liner (a 75μm thick polyethylene terephthalate film with a single-sided release treatment) to a thickness of 50μm after drying. The coating was dried at 90℃ for 3 minutes to create a melt-softened layer c. Using a hand roller, melt-softened layer c, cut to arbitrary widths at 50mm lengths, was bonded to one side of a 100mm long nickel-chromium alloy foil, positioned with the foil extending 25mm from each end in the length direction. The lamination was performed at 120℃ using a roller with a linear pressure of 5kg / cm to create a multilayer structure. Next, following the same procedure as in Example 1, two adhesive layers with a thickness of 50 μm were prepared by coating and drying the adhesive composition (P-2) onto the release liner. These adhesive layers were then cut into arbitrary widths with a length of 50 mm. The adhesive layers were then bonded to both sides of the multilayer body where the release liner had been removed, and lamination was performed using a roller with a linear pressure of 5 kg / cm to produce adhesive layer a1 and adhesive layer a2. This yielded the adhesive tape (T-8) and article of Example 8 with a total thickness of 160 μm.

[0161] (Refer to Example 1) Using a 10 μm thick nickel foil (manufactured by Takeuchi Metal Foil Powder Industry Co., Ltd., trade name: "Ni-H") with a volume resistivity of 8.5 μΩ·cm (rated value 8.2 μΩ·cm) instead of nickel-chromium alloy foil, the adhesive tape (T-9) and article of Reference Example 1 with a total thickness of 110 μm were obtained by the same operation as in Example 1.

[0162] (See Example 2 for reference) Using a 10μm thick copper foil (manufactured by Takeuchi Metal Foil Powder Industry Co., Ltd., trade name: "Copper C1020R-H") with a volume resistivity of 1.7μΩ·cm (rated value 1.7μΩ·cm, measured value 1.9μΩ·cm) instead of a nickel-chromium alloy foil, the adhesive tape (T-10) and article of Reference Example 2 with a total thickness of 110μm were obtained by the same operation as in Example 1.

[0163] (Refer to Example 3) Using a 12μm thick PET film (manufactured by Uniqlo Co., Ltd., trade name: "PETB") instead of nickel-chromium alloy foil, and otherwise following the same procedure as in Example 1, an adhesive tape (T-11) and article of Reference Example 3 with a total thickness of 112μm were obtained. It should be noted that the PET film was not electrified, and its volume resistivity was >10. 23 μΩ·cm (literature value).

[0164] <Evaluation> <<Peel Strength>> [Pre-heating compressive strength] Using the articles from Examples 1-7 and Reference Examples 1-3 as test pieces, the samples were tested at 23°C. Figure 8A The pressing position, using Figure 8B The probe 70 shown in ~C presses the glass plate at a speed of 10 mm / min in the direction of the arrow to measure the strength of the adhesive tape peel (G1). [Pressure strength after heating for 10 seconds] Next, the protruding portion e of the metal foil (heating element) in the adhesive tape 10 of the test piece was clamped with an alligator clip 60. A current of 3.7A was flowed through a dry cell battery and a resistor (manufactured by uxcell, trade name: "Metal Clatt Resistance"). Ten seconds after the power-on started, the glass plate was pressed at a speed of 10 mm / min, and the adhesive strength (G2) at this time was measured. It should be noted that in the evaluation of the article (adhesive tape (T-6)) obtained in Example 6, a DC stabilized power supply (manufactured by Kikusui Electronics Industry Co., Ltd., trade name: "PAS160-1") was used instead of a dry cell battery to flow a current of 0.06A, and the adhesive strength (G2) was measured in the same manner.

[0165] [Reduction rate of compressive strength] Using the compressive strength (G1) measured before heating and the compressive strength (G2) measured after heating for 10 seconds, the compressive strength reduction rate is calculated using the following formula. The rate of decrease in compressive strength (%) = 1 - (G2 / G1) × 100 The results are shown in Table 1. It should be noted that in Examples 1-6 and Reference Examples 1-3, delamination occurred within the adhesive layer a1. In Example 7, delamination occurred at the interface between the metal nonwoven fabric and the adhesive layer a1. In Example 8, damage occurred within the melt-softened layer c.

[0166] <<Temperature of the Adhesive>> In the above-mentioned peeling time determination, the temperature of the adhered material was measured over time, and the highest temperature reached by the adhered material during disassembly was measured. For the temperature measurement of the adhered material, a thin-type temperature sensor (device name: ST-50 (K thermocouple), manufactured by RIKEN K.K.) and a recorder (device name: midi LOGGER GL200A, manufactured by GraphTec Co., Ltd.) were used. Thermocouples were placed on the surface of the adhered material 50b (glass, 30mm wide × 100mm long × 2.8mm thick) (opposite to the adhesive tape) for measurement. The results are shown in Table 1.

[0167] <<Ease of Heating Operation>> The ease of heating operation was evaluated based on the following criteria. The results are shown in Table 1. [Evaluation Criteria] ◎: The power supply or external device is simple and very easy to connect to the power source. ○: The power supply or external device is simple and easy to connect to the power source. △: The power supply or external device is simple, but it is not easy to connect to the power source. ×: The power supply or external device is not simple and is not easy to connect to the power source. -: Cannot be peeled off.

[0168] [Table 1]

[0169] According to the results of Example 1, the adhesive strength after 10 seconds of resistance heating was significantly lower than before heating, with a strength reduction rate of 71%. On the other hand, in Reference Examples 1 and 2, which used a heating element with a volume resistivity of less than 30 μΩ·cm, the strength reduction rates were only 3% and 1%, respectively. Therefore, it can be seen that in Example 1, peeling can be performed in a shorter time compared to Reference Examples 1-2. According to the results of Examples 1-8, it was observed that the strength reduction rate varies depending on the volume resistivity of the heating element, and it can be seen that if the volume resistivity is 30 μΩ·cm or higher, peeling can be performed in a short time within a practical range. In addition, without using large-scale devices such as electromagnetic induction heating or other heating methods, such as heat-generating sources, heat peeling can be easily performed by connecting to a power source (dry cell battery). In Reference Example 3, which is shown as a reference, the PET film was not energized, so no resistance heating was generated, and peeling was not possible. Industrial availability

[0170] This invention can be used as an adhesive tape for fixing components in various electronic devices such as mobile phones, smartphones, tablet PCs, portable music players and PDAs, wearable devices such as smartwatches and VR goggles, digital cameras, video recorders, car navigation systems, personal computers, monitors, televisions, game consoles, air conditioners, and photocopiers.

[0171] This application claims priority based on Japanese application filed on July 9, 2021, namely Japanese Patent Application No. 2021-114334, and invokes all the contents contained in that Japanese application. Explanation of reference numerals in the attached figures

[0172] a1, a2, a3: Adhesive layer b: Heating element c: Melted softened layer e: (The protrusion of the heating element) 10, 20, 30: Adhesive tape 50: Adhesive 100, 300: Items 60: Alligator Clip 70: Probe P: Press position

Claims

1. An adhesive tape, characterized by, The adhesive tape has an adhesive layer A comprising a heating element and an adhesive. The adhesive layer A is a laminate consisting of the planar heating element and adhesive layers a1 and a2 respectively located on each surface of the heating element. In the top view, the planar heating element has a pair of protrusions extending from the outer periphery of the adhesive layer a1 and the adhesive layer a2. The volume resistivity of the heating element is above 30 μΩ·cm. By resistive heating, the adhesive layer A melts or softens, thereby enabling it to be peeled off.

2. The adhesive tape according to claim 1, wherein The adhesive is at least one of pressure-sensitive adhesive and hot melt adhesive.

3. The adhesive tape according to claim 1, wherein The heating element is selected from the group consisting of nickel-chromium alloy, stainless steel, titanium, nickel-silver and carbon.

4. The adhesive tape according to claim 1, wherein, At least one of the adhesive layer a1 and the adhesive layer a2 is melted or softened by resistance heating, thereby enabling peeling.

5. The adhesive tape according to any one of claims 1 to 4, wherein The temperature at which the loss tangent tanδ of the adhesive layer formed by the adhesive reaches 0.45 or higher is located in the temperature range of 80°C or higher and 200°C or lower.

6. An article characterized in that, The item comprises: At least two objects to be glued; and The adhesive tape according to any one of claims 1 to 5 between the two adhered objects. The two objects to be adhered are bonded together via the adhesive tape. In a top view, the adhesive tape has a pair of protrusions extending from the outer periphery of the adhered object.

7. The method for disassembling an article according to claim 6, wherein, The pair of protrusions are connected to a power source as terminals. Power is supplied to the heating element from the power source, and the adhesive layer A is softened or melted by resistance heating, thereby separating the two adhered objects.

8. The method for disassembling an article according to claim 7, wherein, The power source is an external power source.

9. The method for disassembling an article according to claim 7, wherein, The item is an electronic device or a component built into an electronic device. The power source is the driving power source for the electronic device. The pair of protrusions are connected as terminals to the drive power supply and circuit of the electronic device. Power is supplied from the drive power supply to the heating element, and the adhesive layer A is melted or softened by resistance heating, thereby separating the two adhered objects.

Citation Information

Patent Citations

  • Hot-melt type adhesive composition

    JP2002188068A

  • Demolition method for building

    JP2006200279A

  • Double-sided adhesive tape and method for producing the same, adhering and separating double-sided adhesive tape

    JP2016108394A

  • Work support method

    JP2021114334A

  • Separation structure, electric apparatus non-electric apparatus having separation structure, and separation method

    JP2010118776A