High-temperature resistant and impact-resistant rigid polyvinyl chloride corrugated pipe special granules and their preparation method

By introducing chlorinated polyvinyl chloride and acrylonitrile-butadiene-styrene resin into the polyvinyl chloride corrugated pipe, and combining calcium-zinc-tin stabilizer and toughening agent, the heat resistance and impact strength of the corrugated pipe were solved, and the stability and toughness of the material at high temperature were improved.

CN117586589BActive Publication Date: 2026-11-17WUXI JIAHONG PLASTICS TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311691747.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-11
Publication Date
2026-11-17
Estimated Expiration
2043-12-11

AI Technical Summary

Technical Problem

The existing PVC corrugated pipes have insufficient heat resistance and impact strength, which limits their application range.

Method used

A composite heat-resistant modification system of chlorinated polyvinyl chloride resin and acrylonitrile-butadiene-styrene resin, combined with calcium-zinc-tin composite heat stabilizer, toughening agent and processing modifier, is used to form special granules for rigid polyvinyl chloride corrugated pipes that are resistant to high temperature and impact.

Benefits of technology

It improves the heat resistance and impact strength of the corrugated pipe, enhances the high temperature resistance and toughness of the material, and improves the processing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004599414300000081
    Figure BDA0004599414300000081
  • Figure BDA0004599414300000091
    Figure BDA0004599414300000091
  • Figure BDA0004599414300000092
    Figure BDA0004599414300000092
Patent Text Reader

Abstract

This invention belongs to the field of pipe material technology, specifically relating to a special granular material for high-temperature resistant and impact-resistant rigid PVC corrugated pipes and its preparation method. The mass formula of this special granular material for high-temperature resistant and impact-resistant rigid PVC corrugated pipes is as follows: 100 parts PVC resin, 40-60 parts heat-resistant modified resin, 5-8 parts calcium-zinc-tin composite heat stabilizer, 10-20 parts toughening agent, 2-4 parts lubricant, 5-8 parts processing modifier, and 1-2 parts natural paraffin release agent. This invention solves the problems of low heat resistance and low impact strength of existing PVC corrugated pipes. It uses a calcium-zinc-tin composite heat stabilizer to form a composite stabilizer system that combines heat resistance and thermal stability. The high heat distortion temperature of chlorinated PVC resin and acrylonitrile-butadiene-styrene resin improves high-temperature resistance, and the composite toughening system of toughening agent and processing modifier improves impact resistance while reducing the impact on high-temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of pipe material technology, specifically relating to high-temperature resistant and impact-resistant rigid polyvinyl chloride corrugated pipe special granules and their preparation method. Background Technology

[0002] Polyvinyl chloride (PVC) is the world's third-largest produced synthetic polymer plastic (after polyethylene and polypropylene). Pure PVC resin is a rigid thermoplastic with a decomposition temperature very close to its plasticizing temperature, and it has poor mechanical strength. Therefore, PVC resin cannot be used to mold products directly; plasticizers, stabilizers, fillers, etc., must be added to improve its properties to produce PVC plastic, which is then processed into various products.

[0003] Although polyvinyl chloride (PVC) has developed into a general-purpose resin with large production volume, excellent comprehensive performance, and wide application, and people are constantly trying to modify it in various aspects (such as processing performance, impact resistance, heat resistance, and plasticizer migration), its inherent defects still restrict its further development. The most important problem is its poor heat resistance, such as poor high-temperature fluidity. During the modification process, PVC is always accompanied by decomposition, which impairs its processing performance. After decomposition, unsaturated double bonds are formed on the main chain, resulting in polymer discoloration and performance degradation. Although PVC has good chemical resistance and flame retardancy, its Vicat softening point temperature is only about 70°C, and its maximum continuous use temperature is only 65°C, which is relatively poor in heat resistance and limits its application range.

[0004] CPVC (chlorinated polyvinyl chloride) resin is a resin obtained by chlorinating and modifying PVC. Due to its high chlorine content, it has better heat resistance than PVC, with a Vicat softening point temperature exceeding 110℃ and a long-term service temperature reaching 100℃. Its flame retardancy is also superior to PVC; CPVC with a chlorine content of 67% by mass can achieve an oxygen index exceeding 70%, while the limiting oxygen index of PVC is only 45%–49%. Furthermore, CPVC's low price, high mechanical strength, high hardness, and excellent corrosion resistance make it widely applicable in chemical, building materials, electrical appliances, and adhesives industries. However, the high melt viscosity and poor thermal stability of CPVC, along with its similar processing and decomposition temperatures, limit its widespread application. When the chlorine content of CPVC is around 65% by mass, its tensile strength and flexural strength are superior to PVC. When the chlorine content exceeds 70% by mass, the increased molecular polarity and steric hindrance restrict intramolecular rotation, significantly deteriorating its processing performance. Furthermore, it exhibits low impact strength and poor toughness, severely limiting its application range. Therefore, to overcome the shortcomings of CPVC resin, such as difficult processing and low impact strength, further modification of CPVC is still necessary.

[0005] Besides the aforementioned method of modifying PVC's heat resistance through chlorination, other approaches include blending with heat-resistant polymers and copolymerization. However, while these methods can effectively improve the heat resistance of PVC, they all inevitably lead to a loss of its physical and mechanical properties, especially notched impact strength, which drops sharply from 80 J / m to 30 J / m, severely affecting the normal use of downstream products.

[0006] The PVC corrugated pipe granules currently available on the market suffer from the aforementioned defects of PVC materials: they are not heat-resistant and are easily deformed when heated, resulting in a relatively low Vicat softening point temperature; they are also not impact-resistant and are prone to cracking during installation and use, resulting in a relatively low notched impact strength. Summary of the Invention

[0007] To address the problems in existing technologies, this invention provides a special granule for high-temperature resistant and impact-resistant rigid polyvinyl chloride (PVC) corrugated pipes. This solves the problems of low heat resistance and low impact strength in existing PVC corrugated pipes. The high heat distortion temperature of chlorinated PVC resin and acrylonitrile-butadiene-styrene resin can improve high-temperature resistance. The composite toughening system of toughening agent and processing modifier improves impact resistance while reducing the impact on high-temperature resistance.

[0008] To achieve the above technical objectives, one technical solution of the present invention is:

[0009] The quality formula of the high-temperature resistant and impact-resistant rigid PVC corrugated pipe granules is as follows:

[0010] The mixture comprises 100 parts of PVC resin, 40-60 parts of heat-resistant modified resin, 5-8 parts of calcium-zinc-tin composite heat stabilizer, 10-20 parts of toughening agent, 2-4 parts of lubricant, 5-8 parts of processing modifier, and 1-2 parts of natural paraffin release agent; wherein the heat-resistant modified resin is a composite heat-resistant modified system of chlorinated polyvinyl chloride resin and acrylonitrile-butadiene-styrene resin.

[0011] The above technical solution has the following beneficial effects:

[0012] (1) In the formulation of the special granules for high temperature resistant and impact resistant rigid polyvinyl chloride corrugated pipe, the heat stabilizer is a calcium zinc-tin composite heat stabilizer, which forms a composite stabilizer system with both heat resistance and thermal stability.

[0013] (2) The heat-resistant modified resin adopts a composite heat-resistant modified system of chlorinated polyvinyl chloride resin and acrylonitrile-butadiene-styrene resin. Due to the high chlorine content of chlorinated polyvinyl chloride resin, the excellent chemical properties of polyvinyl chloride are retained and the heat resistance is improved. The Vicat softening point temperature can reach above 110℃. Blending with polyvinyl chloride can effectively improve the heat resistance temperature of the mixture. However, it has a large melt viscosity and is difficult to process. Adding acrylonitrile-butadiene-styrene resin can reduce the melt viscosity of chlorinated polyvinyl chloride resin. Moreover, the Vicat softening point temperature of acrylonitrile-butadiene-styrene resin is also above 105℃. Thus, the defect of high melt viscosity of chlorinated polyvinyl chloride is improved without affecting the overall heat resistance of the mixture. That is, the high heat distortion temperature of chlorinated polyvinyl chloride resin and acrylonitrile-butadiene-styrene resin can improve the high temperature resistance.

[0014] (3) The composite toughening system using toughening agents and processing modifiers improves impact resistance while reducing the impact on high temperature resistance.

[0015] Preferably, the mass ratio of the chlorinated polyvinyl chloride resin to the acrylonitrile-butadiene-styrene resin is 1:1 to 3:1. Due to the high chlorine content of the chlorinated polyvinyl chloride resin, its heat resistance is improved, and its Vicat softening point temperature can reach above 110°C. Blending it with polyvinyl chloride can effectively improve the heat resistance temperature of the mixture, but it has a high melt viscosity and is difficult to process. Adding acrylonitrile-butadiene-styrene resin can reduce the melt viscosity of the chlorinated polyvinyl chloride resin, and the Vicat softening point temperature of acrylonitrile-butadiene-styrene resin is also above 105°C. Thus, the defect of high melt viscosity of chlorinated polyvinyl chloride is improved without affecting the overall heat resistance of the mixture.

[0016] Preferably, the calcium-zinc-tin composite heat stabilizer uses calcium stearate-zinc stearate stabilizer and methyl tin mercaptan-dibutyltin maleate composite stabilizer, and the mass ratio of calcium stearate-zinc stearate stabilizer to methyl tin mercaptan-dibutyltin maleate composite stabilizer is 3:1 to 5:1. Calcium stearate-zinc stearate stabilizer is a non-toxic stabilizer based on metal salts, which has good lubricity and metal surface peeling properties, and a high melting point, so it can not affect the heat resistance temperature of the material. However, its thermal stability is generally poor. Adding a small amount of thiol-based organotin stabilizer can make up for this defect and form a composite stabilizer system that has both heat resistance and thermal stability.

[0017] Preferably, the toughening agent is at least one of methyl methacrylate-butadiene-styrene resin and chlorinated polyethylene resin. The methyl methacrylate-butadiene-styrene resin is polymerized from methyl methacrylate, butadiene, and styrene using an emulsion polymerization method. It has a core-shell structure in its submicroscopic morphology. When the blend is impacted, the core, composed of a rubber phase, causes stress concentration and triggers numerous crazing patterns, absorbing impact energy. Furthermore, the butadiene in the acrylate toughening agent has elasticity, improving the blend's toughness and providing excellent toughening effect. Moreover, the methyl methacrylate in the shell of the acrylate toughening agent has a similar solubility parameter to the processing modifier, and the acrylate toughening agent acts as a binder with the processing modifier. Increasing the compatibility between chlorinated polyvinyl chloride (PVC) and polyvinyl chloride (PVC) molecules promotes the formation of a homogeneous phase during processing and melting, increasing the melt shear force and thus improving the impact energy absorption effect of the blend, thereby increasing the notched impact strength of the blend. Chlorinated polyethylene (CPE) is made by chlorinating high-density polyethylene, generally containing 20-50% chlorine. It has good weather resistance, cold resistance, chemical resistance, and oil resistance, as well as good electrical properties and flame retardancy. When used as a toughening agent for PVC resin, the CPE resin forms a continuous network structure similar to cross-linked rubber, exhibiting a certain degree of high elasticity. It can withstand large strain in the direction of external force and also consumes a certain amount of external work, thus contributing to the toughening of PVC resin.

[0018] Preferably, the lubricant is at least one of glycerol fatty acid esters, fatty acid complex esters, polyethylene wax, and oxidized polyethylene wax; glycerol fatty acid esters and fatty acid complex esters are prepared by reacting fatty acids with different alcohols. Besides excellent lubrication, they can also improve the dispersibility and wettability of polyvinyl chloride (PVC) resin. Fatty acid esters have good compatibility with PVC resin, providing a balanced internal and external lubrication effect with minimal impact on adhesion. Furthermore, fatty acid esters also act as plasticizers, reducing the viscosity and improving the flowability of PVC resin. Polyethylene wax and oxidized polyethylene wax are fully saturated ethylene homopolymers. During extrusion or calendering processes, PVC resin is subjected to shear stress and enters the micropores of the processing equipment cavity wall, hindering melt flow and causing wall adhesion. This reduces the processing performance and extrusion surface smoothness of the product. Polyethylene wax and oxidized polyethylene wax can largely overflow onto the melt surface and form a lubricating film between the processing machinery interface, thereby reducing friction between the PVC resin and the metal surface of the processing equipment.

[0019] Preferably, the processing modifier is a blend of methyl methacrylate-acrylate copolymer and α-methylstyrene. The main components of the blend are methyl methacrylate and methylstyrene. After the processing modifier is mixed with polyvinyl chloride resin, it melts under heat and shear force and then adheres to the polyvinyl chloride resin to form a network structure. At the same time, it transfers the external shear force to the resin to promote the plasticization of polyvinyl chloride. This can significantly improve the fluidity of the melt, increase the melt strength, improve the plasticization degree of the product, and improve the physical and mechanical properties of the product.

[0020] Preferably, the natural paraffin release agent is solid paraffin refined from solid hydrocarbons in petroleum or shale oil; it appears as white solid crystals, has low oil content, good plasticity, and certain strength and toughness. Solid paraffin is incompatible with polyvinyl chloride resin, but has high lubrication efficiency, which can improve the lubrication between polymer and metal, improve extrusion efficiency, improve the dispersibility of colorants, and give the product a good gloss.

[0021] To achieve the above technical objectives, the present invention also provides a method for preparing the above-mentioned high-temperature resistant and impact-resistant rigid polyvinyl chloride corrugated pipe granules, the steps of which include:

[0022] Prepare PVC resin, chlorinated polyvinyl chloride resin, acrylonitrile-butadiene-styrene resin, calcium zinc-tin composite heat stabilizer, toughening agent, lubricant, processing modifier, and natural paraffin release agent according to the formula ratio.

[0023] Acrylonitrile-butadiene-styrene resin is added to a ball mill and ball-milled to form acrylonitrile-butadiene-styrene resin powder.

[0024] PVC resin and chlorinated polyvinyl chloride resin are added to a high-speed mixer and stirred for 5-10 minutes to obtain a premixed powder;

[0025] Add calcium-zinc-tin composite heat stabilizer, lubricant, processing modifier, and natural paraffin release agent to the premixed powder and stir evenly. Then add acrylonitrile-butadiene-styrene resin powder and toughening agent and stir until completely mixed to obtain a mixed powder.

[0026] Add the mixed powder to a low-speed mixer and stir for 10-20 minutes. Then cool it and place it in a twin-screw extruder for melt extrusion, cooling, and pelletizing to obtain high-temperature resistant and impact-resistant rigid polyvinyl chloride corrugated pipe granules.

[0027] The above preparation method has the following advantages:

[0028] Through a simple and efficient mixing and granulation process, physical modification of PVC / heat-resistant modified resin and toughening agent was achieved, thereby improving the heat resistance and toughness of PVC resin.

[0029] Preferably, the mixing temperature of the PVC resin and the chlorinated polyvinyl chloride resin is 80-130°C and the pressure is 0.3-0.7 MPa. The temperature of 80-130°C helps other additives to penetrate into the voids of the polyvinyl chloride resin / heat-resistant modified resin, so that the additives are evenly dispersed in the resin. Temperatures above 100°C are also conducive to the evaporation of moisture and various small molecule volatiles in the material.

[0030] Preferably, the mixing temperature of the low-speed mixer is 40-60℃, the conical twin-screw compression ratio of the twin-screw extruder is 3.5-5.0, the screw speed is 30-50 r / min, the extrusion granulation temperature is 150-180℃, and the residence time is 1-2 min; after low-speed mixing, the mixed powder is completely cooled to prevent material decomposition and additive volatilization caused by untimely heat dissipation. Detailed Implementation

[0031] The embodiments of the present invention are described in detail below, but the claims of the present invention are not intended to limit the scope of the invention.

[0032] To address the problems of low heat resistance and low impact strength in existing PVC corrugated pipes, this invention provides a formulation for a special granular material for high-temperature resistant and impact-resistant rigid PVC corrugated pipes, with the following component proportions (by mass):

[0033] 100 parts of PVC resin;

[0034] 40-60 parts of heat-resistant modified resin can be a composite heat-resistant modified system of chlorinated polyvinyl chloride resin and acrylonitrile-butadiene-styrene resin, wherein the mass ratio of chlorinated polyvinyl chloride resin to acrylonitrile-butadiene-styrene resin is 1:1 to 3:1, preferably 2:1.

[0035] 5-8 parts of calcium-zinc-tin composite heat stabilizer, which can be calcium stearate-zinc stearate stabilizer and methyl tin mercaptan-dibutyltin maleate composite stabilizer, wherein the mass ratio of calcium stearate-zinc stearate stabilizer to methyl tin mercaptan-dibutyltin maleate composite stabilizer is 3:1 to 5:1, preferably 5:1;

[0036] The toughening agent, 10-20 parts, can be at least one of methyl methacrylate-butadiene-styrene resin and chlorinated polyethylene resin;

[0037] 2-4 parts of lubricant, which may be at least one of glycerol fatty acid ester, fatty acid complex ester, polyethylene wax and oxidized polyethylene wax;

[0038] The processing modifier, 5-8 parts, can be a blend of methyl methacrylate-acrylate copolymer and α-methylstyrene;

[0039] 1-2 parts of natural paraffin release agent, which can be solid paraffin refined from solid hydrocarbons in petroleum or shale oil;

[0040] In the above formula:

[0041] (1) The heat stabilizer adopts calcium stearate-zinc stearate stabilizer and methyl tin mercaptan-dibutyltin maleate composite stabilizer, and the mass ratio of calcium stearate-zinc stearate stabilizer to methyl tin mercaptan-dibutyltin maleate composite stabilizer is 3:1 to 5:1; calcium stearate-zinc stearate stabilizer is a non-toxic stabilizer based on metal salt, with good lubricity and metal surface peeling properties, and a high melting point, which can not affect the heat resistance temperature of the material, but the effect on thermal stability is generally average; in order to solve this problem, a small amount of thiol organotin stabilizer is added, which can make up for this defect and form a composite stabilizer system with both heat resistance and thermal stability;

[0042] (2) The heat-resistant modified resin adopts a composite heat-resistant modified system of chlorinated polyvinyl chloride resin and acrylonitrile-butadiene-styrene resin, and the mass ratio of chlorinated polyvinyl chloride resin to acrylonitrile-butadiene-styrene resin is 2:1. Due to the high chlorine content of chlorinated polyvinyl chloride resin, the excellent chemical properties of polyvinyl chloride are retained and the heat resistance is improved. The Vicat softening point temperature can reach above 110℃. Blending with polyvinyl chloride can effectively improve the heat resistance temperature of the mixture, but the melt viscosity is high and it is difficult to process. In order to solve this problem, acrylonitrile-butadiene-styrene resin is added, which can reduce the melt viscosity of chlorinated polyvinyl chloride resin. Moreover, the Vicat softening point temperature of acrylonitrile-butadiene-styrene resin is also above 105℃. The defect of high melt viscosity of chlorinated polyvinyl chloride is improved without affecting the overall heat resistance of the mixture.

[0043] (3) The toughening agent is methyl methacrylate-butadiene-styrene resin, which is polymerized by emulsion polymerization of methyl methacrylate, butadiene, and styrene. It has a core-shell structure in its submicroscopic morphology. When the blend is impacted, the core, composed of the rubber phase, causes stress concentration and triggers numerous crazing, absorbing impact energy. Furthermore, the butadiene in the acrylate toughening agent has elasticity, improving the toughness of the blend and providing excellent toughening effect. The processing modifier is a copolymer of methyl methacrylate and acrylate, with methyl methacrylate as the main component. After mixing the processing modifier with the polyvinyl chloride resin, the processing modifier melts under heat and shear force, then adheres to the polyvinyl chloride resin to form a network structure, simultaneously transferring external shear force to the resin to promote the plasticization of the polyvinyl chloride. The methyl methacrylate in the shell of acrylate toughening agents has a similar solubility parameter to that of processing modifiers. Acrylate toughening agents and processing modifiers act as binders, increasing the compatibility between chlorinated polyvinyl chloride (PVC) and polyvinyl chloride (PVC) molecules. This promotes the formation of a homogeneous phase between PVC and PVC during processing and melting, increasing melt shear force and thus improving the impact energy absorption of the blend, thereby increasing the notched impact strength of the blend. When chlorinated polyethylene resin is used as a toughening agent for PVC resin, chlorinated polyethylene resin with a chlorine content of 36-38% exhibits good elasticity and compatibility with PVC resin. Its low crystallinity and glass transition temperature provide good rubber elasticity. After blending with PVC resin, it forms a continuous network structure, and the blend resembles cross-linked rubber, exhibiting a certain degree of high elasticity. It can withstand large strain in the direction of external force and also consumes a certain amount of external work, thus contributing to the toughening of PVC resin.

[0044] Based on the above formulation, a preparation method is provided, comprising the following steps:

[0045] Prepare PVC resin, chlorinated polyvinyl chloride resin, acrylonitrile-butadiene-styrene resin, calcium zinc-tin composite heat stabilizer, toughening agent, lubricant, processing modifier, and natural paraffin release agent according to the formula ratio.

[0046] Acrylonitrile-butadiene-styrene resin is added to a ball mill and ball-milled to form acrylonitrile-butadiene-styrene resin powder.

[0047] PVC resin and chlorinated polyvinyl chloride resin are added to a high-speed mixer and stirred for 5 to 10 minutes to obtain a premixed powder. The stirring temperature of PVC resin and chlorinated polyvinyl chloride resin is 80 to 130°C and the pressure is 0.3 to 0.7 MPa.

[0048] Add calcium-zinc-tin composite heat stabilizer, lubricant, processing modifier, and natural paraffin release agent to the premixed powder and stir evenly. Then add acrylonitrile-butadiene-styrene resin powder and toughening agent and stir until completely mixed to obtain a mixed powder.

[0049] Add the mixed powder to a low-speed mixer and stir for 10-20 minutes. The stirring temperature of the low-speed mixer is 40-60℃. Then cool it. Then place it in a twin-screw extruder for melt extrusion, cooling, and pelletizing to obtain high-temperature resistant and impact-resistant rigid PVC corrugated pipe granules. The conical twin-screw compression ratio of the twin-screw extruder is 3.5-5.0, the screw speed is 30-50 r / min, the extrusion granulation temperature is 150-180℃, and the residence time is 1-2 minutes.

[0050] Based on the above-mentioned formulation and preparation method of high-temperature resistant and impact-resistant rigid PVC corrugated pipe granules, six kinds of high-temperature resistant and impact-resistant rigid PVC corrugated pipe granules were specifically prepared. The formulation component ratios (by mass) in the six implementation schemes (Examples 1 to 6) are shown in Table 1:

[0051] Table 1. Distribution ratio of formulation groups (unit: portions)

[0052]

[0053]

[0054] The properties of the high-temperature resistant and impact-resistant rigid PVC corrugated pipe granules prepared according to the six implementation schemes in Table 1 and the commercially available rigid PVC corrugated pipes in the comparative example were tested. The test results are compared in Table 2.

[0055] Table 2 Comparison of Performance Test Results

[0056]

[0057] In Table 2:

[0058] (1) Vicat softening point test: heating rate 120℃ / h, load 50N.

[0059] (2) The drop hammer impact performance test was conducted at -5℃ with a hammer head mass of 0.8kg and a drop height of 1m.

[0060] (3) The hydrostatic test temperature is 20℃, the test pressure is 1.00MPa, and the time is 48 hours.

[0061] As can be seen from Table 2, the high-temperature resistant and impact-resistant rigid PVC corrugated pipe granules prepared using the formulation and preparation method proposed in this invention have a Vicat softening point temperature that is better than that of commercially available polyethylene corrugated pipes, and their drop hammer impact performance is better than that of commercially available similar products. Therefore, they have good heat resistance and impact strength properties.

[0062] In summary, the present invention has the following advantages:

[0063] 1. This invention solves the problems of low heat resistance and low impact strength of existing polyvinyl chloride corrugated pipes. The high heat distortion temperature of chlorinated polyvinyl chloride resin and acrylonitrile-butadiene-styrene resin can improve the high temperature resistance.

[0064] 2. This invention employs a composite toughening system of toughening agents and processing modifiers to improve impact resistance while reducing the impact on high-temperature resistance;

[0065] 3. This invention uses a calcium-zinc-tin composite heat stabilizer to form a composite stabilizer system that combines heat resistance and thermal stability.

[0066] It is understood that the above detailed description of the present invention is for illustrative purposes only and is not intended to limit the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that modifications or equivalent substitutions can still be made to the present invention to achieve the same technical effects; as long as the usage requirements are met, they are all within the protection scope of the present invention.

Claims

1. High-temperature resistant and impact-resistant rigid polyvinyl chloride corrugated pipe granules, characterized in that: Its quality formula is as follows: 100 parts PVC resin, 40-60 parts heat-resistant modified resin, 5-8 parts calcium-zinc-tin composite heat stabilizer, 10-20 parts toughening agent, 2-4 parts lubricant, 5-8 parts processing modifier, and 1-2 parts natural paraffin release agent. The heat-resistant modified resin is a composite heat-resistant modified system of chlorinated polyvinyl chloride resin and acrylonitrile-butadiene-styrene resin, and the mass ratio of chlorinated polyvinyl chloride resin to acrylonitrile-butadiene-styrene resin is 1:1 to 3:

1. The calcium-zinc-tin composite heat stabilizer uses calcium stearate-zinc stearate stabilizer and methyl tin mercaptan-dibutyltin maleate composite stabilizer, and the mass ratio of calcium stearate-zinc stearate stabilizer to methyl tin mercaptan-dibutyltin maleate composite stabilizer is 3:1 to 5:

1. The toughening agent is at least one of methyl methacrylate-butadiene-styrene resin and chlorinated polyethylene resin; The processing modifier is a blend of methyl methacrylate-acrylate copolymer and α-methylstyrene.

2. The high-temperature resistant and impact-resistant rigid polyvinyl chloride corrugated pipe granules according to claim 1, characterized in that: The lubricant is at least one of glycerol fatty acid ester, fatty acid complex ester, polyethylene wax, and oxidized polyethylene wax.

3. The high-temperature resistant and impact-resistant rigid polyvinyl chloride corrugated pipe granules according to claim 1, characterized in that: The natural paraffin release agent is made from solid paraffin refined from solid hydrocarbons in petroleum or shale oil.

4. A method for preparing high-temperature resistant and impact-resistant rigid polyvinyl chloride corrugated pipe granules as described in any one of claims 1 to 3, comprising the following steps: Prepare PVC resin, chlorinated polyvinyl chloride resin, acrylonitrile-butadiene-styrene resin, calcium zinc-tin composite heat stabilizer, toughening agent, lubricant, processing modifier, and natural paraffin release agent according to the formula ratio. Acrylonitrile-butadiene-styrene resin is added to a ball mill and ball-milled to form acrylonitrile-butadiene-styrene resin powder. PVC resin and chlorinated polyvinyl chloride resin are added to a high-speed mixer and stirred for 5-10 minutes to obtain a premixed powder; Add calcium-zinc-tin composite heat stabilizer, lubricant, processing modifier, and natural paraffin release agent to the premixed powder and stir evenly. Then add acrylonitrile-butadiene-styrene resin powder and toughening agent and stir until completely mixed to obtain a mixed powder. Add the mixed powder to a low-speed mixer and stir for 20 minutes. Then cool it and place it in a twin-screw extruder for melt extrusion, cooling, and pelletizing to obtain high-temperature resistant and impact-resistant rigid polyvinyl chloride corrugated pipe granules.

5. The high-temperature resistant and impact-resistant rigid polyvinyl chloride corrugated pipe granules according to claim 4, characterized in that: The mixing temperature of the PVC resin and chlorinated polyvinyl chloride resin is 80-130℃, and the pressure is 0.3-0.7MPa.

6. The high-temperature resistant and impact-resistant rigid polyvinyl chloride corrugated pipe granules according to claim 4, characterized in that: The mixing temperature of the low-speed mixer is 40-60℃, the conical twin-screw compression ratio of the twin-screw extruder is 3.5-5.0, the screw speed is 30-50 r / min, the extrusion granulation temperature is 150-180℃, and the residence time is 1-2 min.

Citation Information

Patent Citations

  • Injection molding grade flame retardant PVC / ABS alloy material and preparation method thereof

    CN103509289A

  • Blended modified chlorinated polyvinyl chloride material and preparation method thereof

    CN110283412A

  • PVC / CPVC / ABS alloy composite material and preparation method and application thereof

    CN116769261A