A biodegradable environmentally friendly plastic film, its preparation method and application
Patent Information
- Application Number
- CN202311655368.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-12-05
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of plastic films, and more specifically, relates to a degradable and environmentally friendly plastic film and a preparation method and application thereof. Background Art
[0002] With the rapid economic development and the continuous upgrading of consumption, plastic film materials are widely used in food packaging, foaming materials, medical delivery, water treatment membranes, and even space exploration due to their advantages such as low toxicity, high strength, high transparency, good elongation and folding resistance. However, a large amount of plastic waste decomposes into microplastics and even nanoplastics, which then enter the marine and terrestrial ecosystems, causing serious pollution of marine and freshwater systems. Considering the potential adverse effects on nature and human health, an effective way to solve this problem is to find sustainable alternative materials for petroleum products. Therefore, as a favorable substitute for petroleum products, biodegradable nanocomposites have received widespread attention.
[0003] Nanocellulose has a wide range of sources (including bamboo, wood, cotton, hemp, seaweed and other plant fibers, animals and microorganisms), abundant reserves and easy access. Cellulose nanofibrils (CNFs) are cellulose materials with nanometer size made by mechanical, chemical or biological methods. Because of its large aspect ratio, excellent mechanical properties, optical properties and thermal stability and degradable properties, it has great application potential in food packaging, flexible electronic materials, conductive materials, energy conversion, gas filtration, liquid separation and tissue engineering materials. Preparing it into a thin film material for use in production and life can provide a rational choice for better solving the problem of white pollution.
[0004] CN113493572A discloses a degradable environmentally friendly plastic film, its preparation method and application. The degradable environmentally friendly plastic film comprises the following components in parts by weight: 60-80 parts of thermoplastic starch; 10-20 parts of polyvinyl alcohol; 5-10 parts of inorganic powder filler; 4-6 parts of cross-linking agent; 4-6 parts of coupling agent; 1-3 parts of lubricant; the preparation steps of thermoplastic starch are: stirring and mixing ordinary starch and plasticizer, adding waxy starch and cellulose nanocrystals, refining after ultrasonic treatment, refining, tableting, cooling, and crushing; wherein the weight ratio of ordinary starch, plasticizer, waxy starch and cellulose nanocrystals is 1: (0.05-0.25): (0.1-0.3): (0.12-0.18). The degradable environmentally friendly plastic film of the present application has good mechanical properties and high degradation rate. Although the document adds cellulose to improve the degradability, its mechanical properties are insufficient and a large number of components are added. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art and provide a degradable environmentally friendly plastic film and its preparation method and application. In the raw materials for preparing the degradable environmentally friendly plastic film of the present invention, nanocellulose and zirconium oxide nanofibers are added to significantly improve the mechanical properties of the plastic film, so that it has a good application prospect in vegetable greenhouse film, food or medical treatment.
[0006] The purpose of the invention is to provide a degradable and environmentally friendly plastic film.
[0007] Another object of the present invention is to provide a method for preparing a degradable and environmentally friendly plastic film.
[0008] Another object of the present invention is to provide a use of a degradable and environmentally friendly plastic film.
[0009] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0010] A degradable environmentally friendly plastic film, the raw materials of which include the following components by weight:
[0011] Polybutylene terephthalate-adipate (PBAT) 70-90 parts;
[0012] Polylactic acid (PLA) 10-30 parts;
[0013] Nanocellulose 20-30 parts;
[0014] 3~9 parts of zirconium oxide nanofibers.
[0015] In the present invention, in a preferred embodiment, the weight average molecular weight of the PBAT is 40,000 to 80,000; the weight average molecular weight of the PLA is 100,000 to 200,000.
[0016] In the present invention, in a preferred embodiment, the length of the zirconium oxide nanofibers is at least one of 10 to 30 nm, 60 to 100 nm or 140 to 180 nm.
[0017] In the present invention, a further preferred embodiment is that the aspect ratio of the nano zirconium oxide fiber with a length of 10 to 30 nm is 4 to 6:1; the aspect ratio of the nano zirconium oxide fiber with a length of 60 to 100 nm is 20 to 50:1; the aspect ratio of the nano zirconium oxide fiber with a length of 140 to 180 nm is 40 to 60:1; preferably, the length of the zirconia nanofiber is 10 to 30 nm, and the length of the nano zirconium oxide fiber is 60 to 100 nm or 140 to 180 nm. The mass ratio of the nano zirconia fibers with a length of 10-30 nm to the nano zirconia fibers with a length of 60-100 nm or 140-180 nm is 2:1; further preferably, the length of the nano zirconia fibers consists of 10-30 nm, 60-100 nm and 140-180 nm; the mass ratio of the nano zirconia fibers with a length of 10-30 nm, the nano zirconia fibers with a length of 60-100 nm and the nano zirconia fibers with a length of 140-180 nm is 2:0.7:0.3.
[0018] In the present invention, a further preferred solution is to modify the nanocellulose using a zirconate coupling agent; the modification of the nanocellulose using a zirconate coupling agent comprises the following steps:
[0019] The nanocellulose is ultrasonically dispersed in ethanol water to obtain a mixed solution, and then a certain amount of zirconate coupling agent is added to the mixed solution. The mixture is reacted at 50-70° C. for 4-8 hours under stirring conditions. The nanocellulose modified with the zirconate coupling agent is obtained by centrifugal separation and washing.
[0020] Preferably, the volume ratio of the ethanol to water is 7:3; the mass ratio of the nanocellulose to the zirconate coupling agent is 10:0.6-1.2; and the zirconate coupling agent is neoalkoxy tris(p-aminophenoxy) zirconate.
[0021] In the present invention, a further preferred solution is to use polyethylene glycol to modify the zirconium oxide nanofibers: the modification of the zirconium oxide nanofibers using polyethylene glycol comprises the following steps:
[0022] Zirconia nanofibers and polyethylene glycol (PEG-500) were added to deionized water, ultrasonically dispersed, and then reacted at 50-70°C for 3-6 hours. Then, they were filtered, washed, and dried at 80-120°C for 10-20 hours to obtain polyethylene glycol-modified zirconia nanofibers.
[0023] Preferably, the mass ratio of the zirconium oxide nanofibers to polyethylene glycol is 1:0.06-0.10.
[0024] Based on the above-mentioned method for preparing a degradable environmentally friendly plastic film, the preparation method comprises the following steps:
[0025] The raw materials are mixed uniformly according to the proportion and added into a twin-screw extruder, and the parameters are set as follows: screw speed 150-300rpm, heating temperatures of zones 1-5 are as follows: 150-160°C, 160-165°C, 165-175°C, 165-175°C, 175-180°C; granulation, and then drying the granulated material at 60-80°C for 6-12h to obtain a film blowing material, which is then put into a film blowing machine for film blowing, and the parameters are set as follows: screw speed 150-250rpm, heating temperatures of zones 1-5 are as follows: 140-150°C, 145-155°C, 155-160°C, 160-170°C, 170-175°C, and traction speed 8.5-9.5m / min.
[0026] Based on the above-mentioned application of a degradable and environmentally friendly plastic film in vegetable greenhouse film, food or medical treatment.
[0027] The present invention has the following beneficial effects:
[0028] (1) By adding nanocellulose and zirconium oxide nanofibers to the raw materials for preparing the degradable and environmentally friendly plastic film of the present invention, the mechanical properties of the plastic film are significantly improved;
[0029] (2) The mechanical properties of the plastic film were further improved by selecting zirconia nanofibers with different fiber lengths;
[0030] (3) Furthermore, by modifying the nanocellulose and zirconia nanofibers, the dispersibility and bonding strength of the above components were promoted, and the mechanical properties of the plastic film were further improved.
[0031] (4) The degradable and environmentally friendly plastic film prepared by the present invention has good application prospects in vegetable greenhouse film, food or medical treatment. DETAILED DESCRIPTION
[0032] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0033] Nanocellulose (TEMPO method), analytical grade, from Northern Century Cellulose Materials Co., Ltd.
[0034] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0035] Example 1
[0036] A degradable environmentally friendly plastic film, the raw materials of which include the following components by weight:
[0037] 80 parts of polybutylene terephthalate-adipate (PBAT); the weight average molecular weight of the PBAT is 60,000;
[0038] Polylactic acid (PLA) 20 parts; the weight average molecular weight of PLA is 150,000;
[0039] Nanocellulose 25 parts;
[0040] 6 parts of zirconium oxide nanofibers.
[0041] The length of the nano-zirconia fibers is 20 nm;
[0042] The aspect ratio of the 20 nm nano zirconium oxide fiber is 5:1;
[0043] A method for preparing a degradable environmentally friendly plastic film, the method comprising the following steps:
[0044] The raw materials are mixed evenly according to the ratio and added into a twin-screw extruder, and the parameters are set as follows: screw speed 250rpm, heating temperatures of zones 1-5 are as follows: 155°C, 163°C, 170°C, 175°C, 180°C; granulation, and then the granulated material is dried at 70°C for 8h to obtain a film blowing material, which is then put into a film blowing machine for blow molding into a film, and the parameters are set as follows: screw speed 200rpm, heating temperatures of zones 1-5 are as follows: 145°C, 150°C, 160°C, 170°C, 175°C, and traction speed 9m / min.
[0045] Example 2
[0046] A degradable environmentally friendly plastic film, the raw materials of which include the following components by weight:
[0047] 90 parts of polybutylene terephthalate-adipate (PBAT); the weight average molecular weight of the PBAT is 40,000;
[0048] Polylactic acid (PLA) 10 parts; the weight average molecular weight of PLA is 200,000;
[0049] Nanocellulose 30 parts;
[0050] 3 parts of zirconium oxide nanofibers.
[0051] The length of the nano-zirconia fibers is 160 nm;
[0052] The aspect ratio of the 160 nm nano zirconium oxide fiber is 50:1;
[0053] The preparation process and conditions of a degradable and environmentally friendly plastic film are the same as those in Example 1.
[0054] Example 3
[0055] A degradable environmentally friendly plastic film, the raw materials of which include the following components by weight:
[0056] 70 parts of polybutylene terephthalate-adipate (PBAT); the weight average molecular weight of the PBAT is 80,000;
[0057] Polylactic acid (PLA) 30 parts; the weight average molecular weight of PLA is 100,000;
[0058] Nanocellulose 20 parts;
[0059] Zirconia nanofiber 9 parts.
[0060] The length of the nano-zirconia fibers is 80 nm;
[0061] The aspect ratio of the 80nm nano zirconium oxide fiber is 40:1;
[0062] The preparation process and conditions of a degradable and environmentally friendly plastic film are the same as those in Example 1.
[0063] Example 4
[0064] Except for the differences, Example 4 is exactly the same as Example 1. The differences are:
[0065] The length of nano-zirconia fibers consists of 20nm and 80nm;
[0066] The aspect ratio of the 80nm nano zirconium oxide fiber is 40:1;
[0067] The mass ratio of the nano-zirconia fibers with a length of 20 nm to the nano-zirconia fibers with a length of 80 nm is 2:1.
[0068] Example 5
[0069] Except for the differences, Example 5 is exactly the same as Example 1. The differences are:
[0070] The length of nano-zirconia fibers consists of 20nm and 160nm;
[0071] The aspect ratio of the 160 nm nano zirconium oxide fiber is 50:1;
[0072] The mass ratio of the nano zirconium oxide fibers with a length of 20 nm to the nano zirconium oxide fibers with a length of 160 nm is 2:1.
[0073] Example 6
[0074] Except for the differences, Example 6 is exactly the same as Example 1. The differences are:
[0075] The length of the nano zirconium oxide fiber consists of 20nm, 80nm and 160nm; the aspect ratio of the nano zirconium oxide fiber with a length of 80nm is 40:1; the aspect ratio of the nano zirconium oxide fiber with a length of 160nm is 50:1;
[0076] The mass ratio of the nano-zirconia fibers with a length of 20 nm, the nano-zirconia fibers with a length of 80 nm and the nano-zirconia fibers with a length of 160 nm is 2:0.7:0.3.
[0077] Example 7
[0078] Except for the differences, Example 7 is exactly the same as Example 6. The differences are:
[0079] The nanocellulose is modified by using a zirconate coupling agent; the modification of the nanocellulose by using a zirconate coupling agent comprises the following steps:
[0080] 100 g of nanocellulose is ultrasonically dispersed in 100 mL of ethanol water to obtain a mixed solution (the volume ratio of ethanol to water is 7:3), and then 10 g of zirconate coupling agent is added to the mixed solution. The mixture is reacted at 60° C. for 6 hours under stirring conditions. The mixture is centrifuged and washed to obtain nanocellulose modified with a zirconate coupling agent. The zirconate coupling agent is neoalkoxy tris(p-aminophenoxy) zirconate.
[0081] Example 8
[0082] Except for the differences, Example 8 is exactly the same as Example 7. The differences are:
[0083] Modification of zirconium oxide nanofibers by polyethylene glycol: The modification of zirconium oxide nanofibers by polyethylene glycol comprises the following steps:
[0084] 100 g of zirconia nanofibers and 8 g of polyethylene glycol (PEG-500) were added to 150 mL of deionized water, ultrasonically dispersed, and then reacted at 60° C. for 5 h, and then filtered, washed, and dried at 100° C. for 16 h to obtain polyethylene glycol-modified zirconia nanofibers.
[0085] Comparative Example 1
[0086] Except for the differences, Comparative Example 1 is identical to Example 1.
[0087] A degradable environmentally friendly plastic film, the raw materials of which include the following components by weight:
[0088] 80 parts of polybutylene terephthalate-adipate (PBAT); the weight average molecular weight of the PBAT is 60,000; 20 parts of polylactic acid (PLA); the weight average molecular weight of PLA is 150,000;
[0089] Nanocellulose 31 parts.
[0090] The performance of Examples 1-8 and Comparative Example 1 was tested, and the specific test results are shown in Table 1:
[0091] Refer to the method in GB / T1040.1-2018 "Determination of Tensile Properties of Plastics" to test the tensile strength of plastic film, the unit is MPa.
[0092] Table 1
[0093]
[0094] It can be seen from Table 1 that by adding nanocellulose and zirconium oxide nanofibers to the raw materials for preparing the degradable environmentally friendly plastic film of the present invention, the mechanical properties of the plastic film are significantly improved, and by modifying the raw materials, the mechanical properties of the plastic film are further improved.
[0095] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A degradable and environmentally friendly plastic film, characterized in that: By weight, the raw materials include the following components: Polybutylene terephthalate-adipate (PBAT) 70-90 parts; Polylactic acid (PLA) 10-30 parts; 20-30 parts of nanocellulose; 3-9 parts of zirconium oxide nanofibers; The length of the zirconia nanofibers is composed of 10-30nm, 60-100nm and 140-180nm; the mass ratio of the zirconia nanofibers with a length of 10-30nm, the zirconia nanofibers with a length of 60-100nm and the zirconia nanofibers with a length of 140-180nm is 2:0.7:0.3; the aspect ratio of the zirconia nanofibers with a length of 10-30nm is 4-6:1; the aspect ratio of the zirconia nanofibers with a length of 60-100nm is 20-50:1; the aspect ratio of the zirconia nanofibers with a length of 140-180nm is 40-60:1; Wherein, the nanocellulose is modified by using a zirconate coupling agent; the modification of the nanocellulose by using a zirconate coupling agent comprises the following steps: Ultrasonic dispersion of nanocellulose in ethanol water to obtain a mixed solution, then adding a certain amount of zirconate coupling agent to the mixed solution, reacting at 50-70° C. for 4-8 hours under stirring conditions, centrifugation and washing to obtain nanocellulose modified with zirconate coupling agent; the mass ratio of the nanocellulose to the zirconate coupling agent is 10:0.6-1.2; the zirconate coupling agent is neoalkoxy tris(p-aminophenoxy) zirconate; Modification of zirconium oxide nanofibers by polyethylene glycol: The modification of zirconium oxide nanofibers by polyethylene glycol comprises the following steps: Zirconia nanofibers and polyethylene glycol are added to deionized water, ultrasonically dispersed, and then reacted at 50-70°C for 3-6 hours. Then, the reaction is filtered, washed, and dried at 80-120°C for 10-20 hours to obtain polyethylene glycol-modified zirconium oxide nanofibers; the mass ratio of the zirconium oxide nanofibers to the polyethylene glycol is 1:0.06-0.
10.
2. The degradable and environmentally friendly plastic film according to claim 1, characterized in that: The weight average molecular weight of the PBAT is 40,000 to 80,000; the weight average molecular weight of the PLA is 100,000 to 200,000.
3. The degradable and environmentally friendly plastic film according to claim 1, characterized in that: The volume ratio of the ethanol to water is 7:
3.
4. A method for preparing a degradable and environmentally friendly plastic film according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: The raw materials are mixed uniformly according to the ratio and then added into a twin-screw extruder, and the parameters are set as follows: screw speed 150-300rpm, heating temperatures of zones 1-5 are as follows: 150-160°C, 160-165°C, 165-175°C, 165-175°C, 175-180°C; granulation, and then drying the granulated material at 60-80°C for 6-12h to obtain a film blowing material, and then putting it into a film blowing machine for film blowing, and the parameters are set as follows: screw speed 150-250rpm, heating temperatures of zones 1-5 are as follows: 140-150°C, 145-155°C, 155-160°C, 160-170°C, 170-175°C, and traction speed 8.5-9.5m / min.
5. Use of a degradable and environmentally friendly plastic film according to any one of claims 1 to 3 in vegetable greenhouse film.